A modified waterborne polyurethane emulsion, a modified waterborne polyurethane film and a preparation method thereof
Through the block copolymerization reaction of silicone-polyfluorodiol aqueous polyurethane emulsion, combined with polyamine chain extender, the shortcomings of aqueous polyurethane materials in wear resistance and aging resistance are solved, and excellent water resistance and resistance are prepared. Chemically modified water-based polyurethane film suitable for high-performance leather coatings.
Patent Information
- Application Number
- CN202410797472.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-06-20
AI Technical Summary
Existing water-based polyurethane materials cannot have both wear resistance and aging resistance in actual applications, especially after natural light aging outdoors, the leather is prone to blackening and has poor dirt resistance or stain resistance.
Using the preparation method of silicone-polyfluorodiol aqueous polyurethane emulsion, the chemical bonds of silicone and organic fluorine are introduced through block copolymerization reaction, and combined with polyamine as a post-chain extender, the molecular weight and solid content of polyurethane are increased, and the molecular weight and solid content of polyurethane are improved, and the modification is prepared. Water-based polyurethane film.
It significantly improves the thermal stability, water resistance, chemical resistance and mechanical properties of the modified water-based polyurethane film, and has excellent mechanical properties, water resistance and chemical resistance, and is suitable for high-performance leather coatings.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a modified waterborne polyurethane emulsion, a modified waterborne polyurethane film and a preparation method thereof. Background Art
[0002] Polyurethane materials are prepared by polymerization reaction of diisocyanate and polyol as raw materials. Due to the rich variety of raw materials and wide reaction ratio, the content of soft and hard segments in polyurethane can be adjusted according to the required performance, so they are widely used in various fields. Leather coating is one of the application fields of polyurethane materials. The coating prepared by more rational polyurethane should have good aging resistance, water resistance, wear resistance and weather resistance. For example, Chinese patent application CN116284588 A discloses a highly aging-resistant modified waterborne polyurethane and its preparation method and application, wherein carbon dioxide copolymer polyol has both ether bonds and carbonate bonds and thus has a larger polarity, and polybutadiene polyol has a lower polarity. Through block copolymerization, they are combined together, making the internal phase separation of the polyurethane structure more obvious, showing more excellent wear resistance and aging resistance. Chinese patent application CN 116815517 A discloses a method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather. The water-based suede microfiber leather is used, a composite modified nano powder is added, and the nano-modified material is used as the core to prepare the microfiber leather, which can effectively improve the aging resistance and wear resistance of the water-based suede microfiber leather. However, in actual use, the effect of having multiple excellent properties is often not achieved. In view of the poor stain resistance of existing water-based polyurethanes, the leather is blackened and dirty, and the existing technical means have not yet had a better technical solution to perfectly solve this problem, especially the leather soaked in water-based polyurethane is obviously blackened after aging in outdoor natural light, and the dirt resistance or stain resistance is extremely poor. Therefore, there is still a need to develop a more aging-resistant and wear-resistant water-based polyurethane coating. Summary of the invention
[0003] In view of this, the present invention provides a modified waterborne polyurethane emulsion, a modified waterborne polyurethane film and a preparation method thereof, which aims to solve the problem that the existing polyurethane materials cannot have both wear resistance and aging resistance in practical applications.
[0004] In order to achieve the above object, the present invention adopts the following technical solution:
[0005] The present invention provides a method for preparing a modified aqueous polyurethane emulsion, comprising the following steps:
[0006] S1, mixing diol A, diol B and diol C and performing dehydration treatment to obtain a diol mixture;
[0007] S2, mixing the diol mixture, diisocyanate, crosslinking agent and catalyst and reacting them to obtain an intermediate;
[0008] S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer;
[0009] S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a modified waterborne polyurethane emulsion;
[0010] The diol A includes siloxane diol; the diol B includes polyfluoro diol; and the diol C includes one or more of polyester diol, polycarbonate diol and polyether diol.
[0011] Furthermore, in step S1, the mass ratio of diol A, diol B and diol C is 1-5:1-5:20-80.
[0012] Furthermore, in step S2, the reaction temperature is 65-80° C., and the reaction time is 1.5-2.5 h;
[0013] The mass ratio of diisocyanate to crosslinker is 30-70:1-10; the amount of catalyst is 2-4% of the total mass of diol mixture, diisocyanate and crosslinker;
[0014] The mass ratio of diol C to diisocyanate is 20~80:30~70.
[0015] Furthermore, in step S3, the reaction temperature is 65-80° C., and the reaction time is 1-3 h;
[0016] The mass ratio of diol C to chain extender is 20~80:4~20.
[0017] Furthermore, in step S4, the reaction temperature is 40-50° C., and the reaction time is 1-2 h;
[0018] The mass ratio of polyamine, water and ethylenediamine is 2~4:25~45:1~3;
[0019] The mass ratio of glycol C to water is 20~80:25~45.
[0020] The invention provides a modified waterborne polyurethane emulsion prepared by the preparation method.
[0021] The present invention provides a modified waterborne polyurethane film prepared from the modified waterborne polyurethane emulsion, comprising the following components in parts by weight:
[0022] 80-120 parts of modified waterborne polyurethane emulsion, 10-50 parts of pigments and fillers, and 0.1-5 parts of waterborne additives.
[0023] Furthermore, the pigment filler includes one or more of talcum powder, calcite powder, titanium dioxide, kaolin, lithopone, and silica powder.
[0024] Furthermore, the aqueous auxiliary agent includes 2-amino-2-methyl-propanol.
[0025] The present invention also provides a method for preparing the modified waterborne polyurethane film, comprising the following steps:
[0026] The modified waterborne polyurethane emulsion, pigments and fillers and water-based additives are mixed and coated on a substrate, and then naturally dried at 20-30°C for 7 days or more to obtain a modified waterborne polyurethane film.
[0027] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0028] The present invention uses the mass of non-aqueous components in the siloxane-polyfluorodiol waterborne polyurethane emulsion as a benchmark, and uses macromolecular polyols to introduce organic silicon and organic fluorine chemical bonds into the waterborne polyurethane chain segments. The introduction of organic silicon and organic fluorine brings good thermal stability, water resistance, chemical resistance, aging resistance and mechanical properties to the waterborne polyurethane material, and has good market prospects. Polyamine is used as a post-chain extender to simultaneously increase the solid content of the modified waterborne polyurethane emulsion and the molecular weight of the polyurethane.
[0029] The modified waterborne polyurethane film prepared by using the modified waterborne polyurethane emulsion provided by the present invention has excellent mechanical properties, water resistance and chemical resistance. The contact angle of the film to water is between 80° and 102°, the tensile strength is between 4.2 and 27.5 MPa, and the elongation at break is between 310 and 766%. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing a modified aqueous polyurethane emulsion, comprising the following steps:
[0031] S1, mixing diol A, diol B and diol C and performing dehydration treatment to obtain a diol mixture;
[0032] S2, mixing the diol mixture, diisocyanate, crosslinking agent and catalyst and reacting them to obtain an intermediate;
[0033] S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer;
[0034] S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a modified waterborne polyurethane emulsion;
[0035] The diol A includes siloxane diol; the diol B includes polyfluoro diol; and the diol C includes one or more of polyester diol, polycarbonate diol and polyether diol.
[0036] In the present invention, the siloxane diol includes one or more of bishydroxy polyether modified siloxane, hydroxyl-terminated polydimethylsiloxane, vinyl-terminated dimethylpolysiloxane, bistrimethylsiloxymethylsilane, divinyl-terminated phenylpolysiloxane and bis(3-aminopropyl)-terminated polydimethylsiloxane;
[0037] The number average molecular weight of the siloxane diol is 1000-9000 g / mol, preferably 2000-8000 g / mol, and more preferably 4000-6000 g / mol;
[0038] The structural formula of siloxane is as follows:
[0039] ; wherein n=20~30, preferably 22~28, and more preferably 24~26.
[0040] In the present invention, the polyfluoro diol includes one or more of hexafluoro-1,10-decanediol, 2,2,3,3,4,4,5,5-octafluoro-1,6-hexanediol, hexafluoro-2,3-bis(trifluoromethyl)-2,3-butanediol and 2,2,3,3-tetrafluoro-1,4-butanediol.
[0041] In the present invention, the polyester diol includes a macromolecular polymer diol containing an ester bond, preferably one or more of polycaprolactone diol, polybutylene succinate diol, polyhexamethylene glycol butylene glycol ester diol, polyethylene succinate diol, polyhexamethylene glycol ethylene glycol ester diol, polyethylene terephthalate diol and polybutylene terephthalate diol;
[0042] The number average molecular weight of the polyester diol is 1500-2500 g / mol, preferably 1700-2300 g / mol, and more preferably 1800-2200 g / mol.
[0043] In the present invention, the polycarbonate diol is preferably one or more of polycarbonate butanediol diol, polycarbonate hexanediol diol, polycarbonate decanediol diol and polycarbonate cyclohexanedimethanol diol;
[0044] The number average molecular weight of the polycarbonate diol is 1500-2500 g / mol, preferably 1700-2300 g / mol, and more preferably 1800-2200 g / mol.
[0045] In the present invention, the polyether diol is preferably one or more of polytetrahydrofuran diol, polyethylene glycol diol and polypropylene glycol diol;
[0046] The number average molecular weight of the polyether diol is 1500-2500 g / mol, preferably 1700-2300 g / mol, and more preferably 1800-2200 g / mol.
[0047] In the present invention, the polyester diol, polycarbonate diol and polyether diol are preferably used in the same amount.
[0048] In the present invention, in the step S1, the dehydration treatment is performed under a protective gas, and the protective gas includes nitrogen.
[0049] In the present invention, in step S1, the mass ratio of diol A, diol B and diol C is 1-5:1-5:20-80, preferably 2-4:2-4:30-60, and more preferably 3:3:40-50.
[0050] In the present invention, in step S2, the reaction temperature is 65-80°C, preferably 68-76°C, and more preferably 70-75°C; the reaction time is 1.5-2.5h, preferably 1.6-2.4h, and more preferably 1.8-2.0h; the mass ratio of diisocyanate to cross-linking agent is 30-70:1-10, preferably 40-60:2-8, and more preferably 45-50:4-6; the amount of catalyst is 2-4% of the total mass of the diol mixture, diisocyanate and cross-linking agent, preferably 2.5-3.5%, and more preferably 3.0%; the mass ratio of diol C to diisocyanate is 20-80:30-70, preferably 30-60:40-60, and more preferably 40-50:45-50.
[0051] In the present invention, the diisocyanate includes one or more of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), 1,6-hexamethylene diisocyanate (HDI), xylylene diisocyanate (XDI), naphthalene-1,5-diisocyanate (NDI), polymethylene polyphenyl isocyanate (PAPI), tetramethylxylylene diisocyanate (TMXDI), methylcyclohexyl diisocyanate (HTDI) and dicyclohexylmethane diisocyanate (HMDI);
[0052] The crosslinking agent includes dimethylol propionic acid; the catalyst includes one or more of zinc chloride, tin tetrachloride, stannous chloride, germanium chloride, dibutyltin laurate, dibutyltin diacetate and stannous octoate.
[0053] In the present invention, in step S3, the reaction temperature is 65-80°C, preferably 66-76°C, and more preferably 68-72°C; the reaction time is 1-3h, preferably 1.5-2.5h, and more preferably 2.0h; the mass ratio of diol C to chain extender is 20-80:4-20, preferably 30-70:8-16, and more preferably 40-60:10-12.
[0054] In the present invention, the chain extender includes one or more of 2,2,3,3,4,4-hexafluoro-1,5-pentanediol, ethylene glycol, diethylene glycol, 1,4-butanediol, 2,3-butanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, glycerol, sorbitol, trimethylolpropane, dimethylolcyclohexane, pentaerythritol diacrylate (PEDA), dipentaerythritol tetraacrylate (DPETA), trimethylolpropane monoacrylate (TMPMA) and dimethylolpropionic acid.
[0055] In the present invention, in step S4, the reaction temperature is 40-50°C, preferably 42-48°C, preferably 44-46°C; the reaction time is 1-2h, preferably 1.5h; the mass ratio of polyamine, water and ethylenediamine is 2-4:25-45:1-3, preferably 2.5-3.5:30-40:1.4-2.6, more preferably 2.8-3.2:33-37:1.7-2.2; the mass ratio of diol C and water is 20-80:25-45, preferably 30-70:30-40, more preferably 40-60:33-37.
[0056] In the present invention, the polyamine includes one or more of triethylamine, diethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and isophoronediamine.
[0057] The present invention provides a modified aqueous polyurethane emulsion prepared by the above preparation method, wherein the solid content of the modified aqueous polyurethane emulsion is 25-31%, preferably 26-30%, and more preferably 27-29%.
[0058] The present invention provides a modified waterborne polyurethane film prepared from the modified waterborne polyurethane emulsion, comprising the following components in parts by weight:
[0059] 80-120 parts of modified waterborne polyurethane emulsion, 10-50 parts of pigments and fillers, and 0.1-5 parts of waterborne additives.
[0060] In the present invention, the thickness of the modified waterborne polyurethane film is 0.8-1.2 mm, preferably 0.9-1.1 mm, and more preferably 1.0 mm.
[0061] In the present invention, the amount of the modified aqueous polyurethane emulsion is preferably 85 to 115 parts, more preferably 90 to 110 parts.
[0062] In the present invention, the amount of the pigment and filler is preferably 20 to 40 parts, and more preferably 25 to 30 parts.
[0063] In the present invention, the amount of the aqueous auxiliary agent is preferably 1 to 4 parts, more preferably 2 to 3 parts.
[0064] In the present invention, the pigment filler includes one or more of talc powder, calcite powder, titanium dioxide, kaolin, lithopone, and silica powder.
[0065] In the present invention, the aqueous auxiliary agent includes 2-amino-2-methyl-propanol.
[0066] The present invention also provides a method for preparing the modified waterborne polyurethane film, comprising the following steps:
[0067] The modified waterborne polyurethane emulsion, pigments and fillers and water-based additives are mixed and coated on a substrate, and then naturally dried at 20-30°C for 7 days or more to obtain a modified waterborne polyurethane film.
[0068] In the present invention, the substrate includes a polytetrafluoroethylene plate.
[0069] In the present invention, the natural drying temperature is preferably 22-28° C., more preferably 24-26° C.; the natural drying time is preferably ≥7.5 days, more preferably ≥8 days.
[0070] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0071] Example 1
[0072] 20 parts of polycaprolactone diol (number average molecular weight of 2000 g / mol), 5 parts of dihydroxysiloxane and 1 part of hexafluoro-1,10-decanediol were mixed, and water was removed by reduced pressure distillation under N2 protection to obtain a diol mixture, which was cooled to 65°C, 30 parts of isophorone diisocyanate and 1 part of dimethylolpropionic acid as a cross-linking agent were added, and 2% of the total mass of dibutyltin dilaurate was added dropwise, and the mixture was reacted at 65°C for 2.5 h to obtain an intermediate, and 4 parts of chain extender 1,4-butanediol were added to continue the reaction for 3 h to obtain a prepolymer; the mixture was cooled to 45°C, 2 parts of triethylamine were added, and 25 parts of water and 1 part of ethylenediamine were added under stirring for 2 h to obtain a modified waterborne polyurethane emulsion.
[0073] Example 2
[0074] The same as Example 1, except that the amount of polycaprolactone diol (number average molecular weight of 2000 g / mol) used is 30 parts.
[0075] Example 3
[0076] The same as Example 1, except that the amount of polycaprolactone diol (number average molecular weight of 2000 g / mol) used is 40 parts.
[0077] Example 4
[0078] 20 parts of polyethylene glycol diol (number average molecular weight of 2000 g / mol), 5 parts of dihydroxysiloxane and 2 parts of hexafluoro-1,10-decanediol were mixed, and water was removed by reduced pressure distillation under N2 protection to obtain a diol mixture, which was cooled to 70°C, 30 parts of isophorone diisocyanate and 1 part of dihydroxymethylpropionic acid as a cross-linking agent were added, and 2% of the total mass of dibutyltin dilaurate was added dropwise, and the mixture was reacted at 70°C for 2h to obtain an intermediate, and 5 parts of chain extender 1,4-butanediol were added to continue the reaction for 2.5h to obtain a prepolymer; the mixture was cooled to 50°C, 2 parts of diethylenetriamine were added, and 25 parts of water and 1 part of ethylenediamine were added under stirring to react for 2h to obtain a modified waterborne polyurethane emulsion.
[0079] Example 5
[0080] The same as Example 4, except that the amount of polyethylene glycol (number average molecular weight 2000 g / mol) used is 30 parts.
[0081] Example 6
[0082] The same as Example 4, except that the amount of polyethylene glycol (number average molecular weight 2000 g / mol) used is 40 parts.
[0083] Example 7
[0084] 20 parts of polycaprolactone diol (number average molecular weight of 2500g / mol), 5 parts of dihydroxysiloxane and 1 part of hexafluoro-1,10-decanediol were mixed, and water was removed by reduced pressure distillation under N2 protection to obtain a diol mixture, which was cooled to 65°C, 30 parts of toluene diisocyanate and 1 part of dihydroxymethylpropionic acid as a cross-linking agent were added, and 2% of the total mass of dibutyltin dilaurate was added dropwise, and the mixture was reacted at 65°C for 2.5 hours to obtain an intermediate, and 4 parts of chain extender 1,4-butanediol were added to continue the reaction for 3 hours to obtain a prepolymer; the mixture was cooled to 45°C, 2 parts of triethylamine were added, and 25 parts of water and 1 part of ethylenediamine were added under stirring for 2 hours to obtain a modified waterborne polyurethane emulsion.
[0085] Example 8
[0086] The same as Example 7, except that the amount of toluene diisocyanate used is 40 parts.
[0087] Example 9
[0088] The same as Example 7, except that the amount of toluene diisocyanate used is 50 parts.
[0089] Example 10
[0090] 20 parts of polycaprolactone diol (number average molecular weight of 1500g / mol), 5 parts of dihydroxysiloxane and 1 part of hexafluoro-1,10-decanediol were mixed, and water was removed by reduced pressure distillation under N2 protection to obtain a diol mixture, which was cooled to 65°C, 30 parts of isophorone diisocyanate and 1 part of dimethylolpropionic acid as a cross-linking agent were added, and 2% of the total mass of dibutyltin dilaurate was added dropwise, and the mixture was reacted at 65°C for 2.5 hours to obtain an intermediate, and 4 parts of chain extender 2,3-butanediol were added to continue the reaction for 3 hours to obtain a prepolymer; the mixture was cooled to 45°C, 2 parts of triethylamine were added, and 25 parts of water and 1 part of ethylenediamine were added under stirring for 2 hours to obtain a modified waterborne polyurethane emulsion.
[0091] Embodiment 11
[0092] The same as Example 10, except that the amount of 2,3-butanediol used is 10 parts.
[0093] Example 12
[0094] The same as Example 10, except that the amount of 2,3-butanediol used is 15 parts.
[0095] Embodiment 13
[0096] 20 parts of polycaprolactone diol (number average molecular weight of 2200 g / mol), 5 parts of dihydroxysiloxane and 1 part of 2,2,3,3,4,4,5,5-octafluoro-1,6-hexanediol were mixed, and water was removed by reduced pressure distillation under N2 protection to obtain a diol mixture, which was cooled to 65°C, 30 parts of 1,6-hexamethylene diisocyanate and 1 part of dimethylol propionic acid as a cross-linking agent were added, and zinc chloride of 2% of the total mass of the reactants was added dropwise, and the mixture was reacted at 65°C for 2.5 h to obtain an intermediate, and 4 parts of chain extender neopentyl glycol were added to continue the reaction for 3 h to obtain a prepolymer; the mixture was cooled to 45°C, 2 parts of triethylenetetramine were added, and 25 parts of water and 1 part of ethylenediamine were added under stirring for 2 h to obtain a modified waterborne polyurethane emulsion.
[0097] Application Examples
[0098] Take 100 parts of the modified waterborne polyurethane emulsion prepared in Example 1, 50 parts of pigments and fillers (10 parts each of talcum powder, calcite powder, titanium dioxide, kaolin and lithopone) and 2 parts of 2-amino-2-methyl-propanol, mix them and evenly coat them on a polytetrafluoroethylene plate with a thickness of 1 mm, and dry them at 25°C for one week to obtain a modified waterborne polyurethane film.
[0099] The modified waterborne polyurethane emulsions prepared in Examples 2 to 13 were respectively used to prepare modified waterborne polyurethane films according to the above steps, and the abrasion resistance and aging resistance of all the films were tested. The test results are shown in Table 1. The abrasion resistance test standard refers to GB / T1768-1979 "Determination of abrasion resistance of paint films", and the aging resistance test standard refers to GB / T 16422.3-2014 "Plastics laboratory light source exposure test method Part 3: Fluorescent ultraviolet lamp".
[0100] Table 1 Performance test results of modified waterborne polyurethane membrane
[0101]
[0102] It can be seen from Table 1 that the modified waterborne polyurethane film prepared by using the modified waterborne polyurethane emulsion provided by the present invention has excellent wear resistance and aging resistance in practical applications.
[0103] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a modified aqueous polyurethane emulsion, characterized in that: The following steps are involved: S1, mixing diol A, diol B and diol C and performing dehydration treatment to obtain a diol mixture; S2, mixing the diol mixture, diisocyanate, crosslinking agent and catalyst and reacting them to obtain an intermediate; S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer; S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a modified waterborne polyurethane emulsion; The diol A is dihydroxysiloxane; the diol B is hexafluoro-1,10-decanediol; the diol C is polyethylene glycol diol; the number average molecular weight of the polyethylene glycol diol is 2000 g / mol; In the step S1, the mass ratio of diol A, diol B and diol C is 1-5:1-5:20-80; In step S2, the mass ratio of diisocyanate to crosslinking agent is 30-70:1-10; the amount of catalyst is 2-4% of the total mass of diol mixture, diisocyanate and crosslinking agent; the mass ratio of diol C to diisocyanate is 20-80:30-70; In the step S3, the mass ratio of diol C to chain extender is 20-80:4-20; In step S4, the reaction temperature is 40-50° C., the reaction time is 1-2 hours; the mass ratio of polyamine, water and ethylenediamine is 2-4:25-45:1-3; the mass ratio of diol C and water is 20-80:25-45.
2. The method for preparing the modified aqueous polyurethane emulsion according to claim 1, characterized in that: In step S2, the reaction temperature is 65-80° C., and the reaction time is 1.5-2.5 h.
3. The method for preparing the modified aqueous polyurethane emulsion according to claim 1, characterized in that: In step S3, the reaction temperature is 65-80° C., and the reaction time is 1-3 hours.
4. The modified aqueous polyurethane emulsion prepared by the method for preparing the modified aqueous polyurethane emulsion according to any one of claims 1 to 3.
5. A modified waterborne polyurethane film prepared by using the modified waterborne polyurethane emulsion according to claim 4, characterized in that: The composition comprises the following components in parts by weight: 80-120 parts of modified waterborne polyurethane emulsion, 10-50 parts of pigments and fillers, and 0.1-5 parts of waterborne additives.
6. The modified waterborne polyurethane film according to claim 5, characterized in that: The pigment and filler include one or more of talcum powder, calcite powder, titanium dioxide, kaolin, lithopone, and silica powder.
7. The modified waterborne polyurethane film according to claim 6, characterized in that: The aqueous auxiliary agent includes 2-amino-2-methyl-propanol.
8. The method for preparing a modified waterborne polyurethane film according to any one of claims 5 to 7, characterized in that: The following steps are involved: The modified waterborne polyurethane emulsion, pigments and fillers and water-based additives are mixed and coated on a substrate, and dried naturally at 20-30° C. for 7 days or more to obtain a modified waterborne polyurethane film.