A perfluoropolyether grafted modified compound and its preparation method and application

The introduction of perfluoropolyether compounds with branched structures through grafting reactions solves the problem of insufficient solubility of perfluoropolyethers, achieving good solubility in common solvents and efficient antifouling properties, and is suitable for a variety of coatings and surface treatments.

CN118359801BActive Publication Date: 2024-10-11DONGHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410791582.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-11
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

Perfluoropolyethers are nearly insoluble in common solvents, making them insufficiently soluble in coatings and other applications, making them difficult to use widely.

Method used

Compounds containing olefin double bonds and functional groups are combined with perfluoropolyether polythiol compounds through grafting reactions to introduce branched structures to form perfluoropolyether graft-modified compounds, which improve their performance in common organic solvents. Solubility and used in the preparation of antifouling coatings and surface treatments.

Benefits of technology

It achieves good solubility of perfluoropolyether in common organic solvents, enhances the bonding strength between the coating and the substrate, improves the antifouling performance and durability of the coating, simplifies the preparation process and reduces side reactions. The product High purity and adjustable structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118359801B_ABST
    Figure CN118359801B_ABST
Patent Text Reader

Abstract

The present invention relates to a perfluoropolyether grafted modified compound and a preparation method and application thereof. The present invention can adjust the branching degree and structure of the target compound by using different structures and polythiol compounds with different numbers, and can further graft corresponding functional groups through the thiol group according to the downstream target application scenario to obtain a perfluoropolyether compound with good solubility in common organic solvents such as tetrahydrofuran, esters, ketones, etc., which can be applied to different substrates and coating systems. Compared with the prior art, the reaction is simple, the product purity is high, and the compound structure can be adjusted in a wide range according to downstream needs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional materials, and particularly relates to a perfluoropolyether grafted modified compound and a preparation method and application thereof. Background Art

[0002] Perfluoropolyether is a type of polymer whose main chain consists of CO and CC bonds, and all hydrogen atoms are replaced by fluorine atoms. Due to the strong shielding effect of the fluorine element, perfluoropolyether has excellent heat resistance, chemical stability, oxidation stability and complete non-flammability, and is therefore used as lubricating oil in the nuclear industry and aerospace. In recent years, with the widespread use of interactive touch screens, perfluoropolyether materials have also been widely used as the main component of anti-fingerprint agents for screens. However, this substance is almost insoluble in organic solvents and has a certain solubility only in perfluoro solvents or fluorinated solvents such as F113 (trichlorotrifluoroethane). For this reason, it is crucial to solve the solubility problem of perfluoropolyether in ordinary solvents. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a perfluoropolyether graft-modified compound and a preparation method and application thereof.

[0004] The present invention provides a perfluoropolyether grafted modified compound, the general structural formula of the perfluoropolyether grafted modified compound is: , wherein X is one or more of an amide group, an ester group, an ether group, and an amine group; the Y has a branched structure, and the branched structure contains at least two -SR terminal groups;

[0005] The R contains a functional group; wherein the functional group includes one or more of a hydroxyl group, an amino group, a hydrazide group, a benzophenone group, a (meth)acryloxy group, an epoxy group, and a trialkoxysilane group;

[0006] Where m is an integer from 0 to 28, and n is a positive integer from 1 to 2;

[0007] The PFPE is a perfluoropolyether chain; wherein the perfluoropolyether chain is one of Z type, K type, Y type and D type, and has a molecular weight of 300-20000.

[0008] Preferably, the Y branched structure contains 2 to 12 -SRs.

[0009] Preferably, said Y comprises: , , , At least one of .

[0010] Preferably, the graft-modified compound is: , , , Wherein m is an integer from 0 to 28, and n is a positive integer from 1 to 2.

[0011] Preferably, said R comprises: , , , , , At least one of .

[0012] The invention provides a method for preparing a graft modified compound, comprising: subjecting raw materials containing a perfluoropolyether polythiol compound and a compound containing an olefin double bond and a functional group to a graft reaction to obtain a perfluoropolyether graft modified compound.

[0013] The grafting reaction is a grafting reaction between the thiol group in the perfluoropolyether polythiol compound and the compound containing olefin double bonds and functional groups.

[0014] The compounds containing olefin double bonds and functional groups include but are not limited to: , , , , , One or more of the .

[0015] The preparation method of the perfluoropolyether multimercapto compound comprises: mixing a perfluoropolyether with an olefin double bond at the end, a multimercapto compound with a branched structure, an initiator, and a solvent, and obtaining the perfluoropolyether multimercapto compound through a thiol-olefin click reaction; wherein the perfluoropolyether with an olefin double bond at the end is , wherein X is one or more of amide, ester, ether, and amine; the perfluoropolyether with a terminal olefin double bond is prepared by reacting a perfluoropolyether derivative (such as perfluoropolyether alcohol, perfluoropolyether methyl ester, perfluoropolyether acyl fluoride, perfluoropolyether acyl chloride or perfluoropolyether carboxylic acid, etc.) with a compound with an olefin double bond through etherification, esterification, amidation, amination, etc. The initiator is a free radical initiator or a basic initiator. When the double bond in is an electron-rich double bond, the initiator selected includes a free radical initiator, wherein the free radical initiator includes a peroxide initiator, an azo initiator, a photoinitiator, etc.; when When the double bond in the reaction is an electron-deficient double bond, the initiator is a basic initiator, such as an organic amine or organic phosphine alkaline initiator, specifically triethylamine, triphenylphosphine, etc.

[0016] Preferably, the solvent is a fluorine-containing polar solvent, such as hexafluoroisopropanol, trifluoroacetic acid, etc.

[0017] Preferably, the branched structured polythiol compound comprises: , , , At least one of .

[0018] Preferably, the molar ratio of the perfluoropolyether with an olefin double bond at the terminal, the polythio compound with a branched structure, and the initiator is 1:1~2:0.01~0.2; the amount of the fluorinated polar solvent is 5~100 times the total mass of the above three substances (perfluoropolyether with an olefin double bond at the terminal, the polythio compound with a branched structure, and the initiator).

[0019] Preferably, the temperature of the thiol-olefin click reaction is: when the initiator is a photoinitiator or an alkaline initiator, the reaction temperature is -30°C to 60°C; when the initiator is a thermally initiated free radical initiator, the reaction temperature is the initiation temperature corresponding to the initiator used.

[0020] The invention provides an antifouling composition, which comprises any one of the perfluoropolyether graft-modified compounds and an organic solvent.

[0021] Preferably, the organic solvent includes at least one of a fluorinated solvent such as a hydrofluoroether, an alcohol (such as ethanol, methoxyethanol, etc.), an ester (such as ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, etc.), a ketone (such as methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), and an ether (such as tetrahydrofuran, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, etc.).

[0022] The composition contains a coating, wherein the perfluoropolyether grafted modified compound accounts for 0.1-10% of the coating mass.

[0023] Preferably, the coating is at least one of acrylic coating, epoxy coating, phenolic coating, alkyd coating, polyurethane coating, amino coating, polysiloxane coating, vinyl resin coating, and light-curing coating.

[0024] Furthermore, the composition comprises a perfluoropolyether grafted modified compound and an organic solvent, or a perfluoropolyether grafted modified compound, an organic solvent and a coating.

[0025] The present invention provides an application of any of the antifouling compositions in an anti-fingerprint agent, an anti-graffiti coating, and a surface treatment agent.

[0026] In the present invention, another compound containing olefin double bonds is directly added to the perfluoropolyether polythiol compound to directly graft and modify other functional groups on the unreacted thiol group. For example, by reacting with 6-benzophenoneoxyhexene, a perfluoropolyether compound with a photoinitiator group can be grafted, which can be used in, for example, a photocurable coating system, such as Example 1.

[0027] For example, by reacting with ethylene glycol monoallyl ether, hydroxyl-containing functional groups can be modified and grafted, and can be used in amino paint coating systems. On the basis of this polyhydroxy perfluoropolyether compound, further reaction with methyl acyloxyethyl isocyanate can graft methacrylate groups. This compound can be used as an anti-fingerprint agent in a photocuring system, such as Example 2.

[0028] In addition, by reacting with vinyltrialkoxysilane, a new type of perfluoropolyether siloxane compound can be prepared, which can be used as a treatment agent for the surface of glass and inorganic materials, as shown in Example 3.

[0029] Finally, at low temperature, by reacting with allyl glycidyl ether, a perfluoropolyether compound containing an epoxy functional group can be prepared, which can be used in epoxy system coatings, such as Example 4.

[0030] Beneficial Effects

[0031] (1) The present invention can adjust the branching degree and structure of the target compound by adopting different structures and polythiol compounds with different numbers. According to the downstream target application scenario, the corresponding functional groups can be further grafted through the thiol group to obtain a perfluoropolyether compound with good solubility in common organic solvents such as tetrahydrofuran, esters, ketones, etc., which can be applied to different substrates and coating systems.

[0032] (2) The present invention can further increase the bonding strength between the perfluoropolyether chain and the coating or substrate by introducing a branched structure at the end of the perfluoropolyether chain, thereby increasing the durability of the antifouling performance of the coating.

[0033] (4) Compared with the existing technology, the reaction is simple, the product purity is high, the compound structure can be adjusted to a wide range according to downstream needs, and the coating prepared by it has long-lasting antifouling performance.

[0034] (5) In the present invention, the polythiol perfluoropolyether compound is prepared by a click reaction, the reaction is quantitative, and there is almost no side reaction. The obtained product can be directly used without purification or directly subjected to the next step of reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the 1H NMR spectrum of the compound whose functional group is methacrylate obtained in Example 1.

[0036] Figure 2 This is the 1H NMR spectrum of the compound whose functional group is methacrylate obtained in Example 2. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0038] Allyl-terminated perfluoropolyethers were of K type with a molecular weight of 4600 g / mol and were purchased from Shanghai Institute of Organic Chemistry.

[0039] The Chinese names corresponding to the abbreviations involved in the embodiments and chemical equations are: PFPE: perfluoropolyether; HFE7200: nonafluorobutyl ether; HFIP: hexafluoroisopropanol; ABVN: azobisisoheptylcyanide; DBTDL: dibutyltin dilaurate; MEHQ: p-hydroxyanisole; POSS-SH8: octamercaptopropylsilsesquioxane; THF tetrahydrofuran; TPO: 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0040] Example 1

[0041] Under nitrogen protection, 4.6 g of allyl-terminated perfluoropolyether (Mn=4600 g / mol, 1 mmol), 0.783 g (1 mmol) of dipentaerythritol hexa(3-mercaptopropionic acid), 0.02 g of azobisisoheptylcyanide, and 50 ml of hexafluoroisopropanol were added to a 100 ml reaction bottle and reacted at 55°C for 2 hours. 1 The reaction was tracked by H NMR until the double bond signal disappeared. Under nitrogen protection, 1.402 g (5 mmol) of 6-benzophenoneoxyhexene and 0.02 g of diisoheptanonitrile were added, and the reaction was continued at 55°C for 6 hours. The reaction was tracked by 1H NMR until the double bond signal basically disappeared. The reaction solution was concentrated to obtain a viscous liquid product. The product was dissolved in butyl propionate and added to UV curing varnish at a mass percentage of 0.5% to obtain UV anti-graffiti coating 1.

[0042] Attached Figure 1 The obtained compound 1 H NMR spectrum, the number and chemical shift of all hydrogen atoms in the figure completely correspond to the number and chemical shift of hydrogen atoms in the compound of the target structure, proving that the obtained compound has a high purity.

[0043] The reaction equation is as follows: .

[0044] Example 2

[0045] Under nitrogen protection, 4.6 g of allyl-terminated perfluoropolyether (Mn=4600 g / mol, 1 mmol), 0.783 g (1 mmol) of dipentaerythritol hexa(3-mercaptopropionic acid), 0.02 g of azobisisoheptylcyanide, and 50 ml of hexafluoroisopropanol were added to a 100 ml reaction bottle and reacted at 55°C for 2 hours. 1 The reaction was followed by HNMR until the double bond signal disappeared. Under nitrogen protection, 0.511 g (5 mmol) of ethylene glycol monoallyl and 0.02 g of azobisisoheptyl cyanide were added and the reaction was continued at 55°C for 6 hours. 1 HNMR tracks the reaction until the double bond signal disappears. After the reaction solution is concentrated, a viscous liquid product is obtained. After the product is subjected to high vacuum to remove low-boiling substances, it is dissolved in 50 ml of dry tetrahydrofuran, and 0.78 g (5 mmol) of methacryloyloxyethyl isocyanate, 0.02 g of DBTDL (dibutyltin dilaurate), and 0.05 g of MEHQ (p-hydroxyanisole) are added. The reaction is carried out at 60°C for 8 hours. After the reaction solution is concentrated, it is dissolved and diluted with methyl isobutyl ketone. It is added to UV curing varnish in an amount of 0.5% by mass to obtain UV anti-graffiti coating 2.

[0046] Attached Figure 2 The obtained compound 1 H NMR spectrum, the number and chemical shift of all hydrogen atoms in the figure completely correspond to the number and chemical shift of hydrogen atoms in the compound of the target structure, proving that the obtained compound has a high purity.

[0047] The reaction equation is as follows: .

[0048] Example 3

[0049] Under nitrogen protection, 4.6 g of allyl-terminated perfluoropolyether (Mn=4600 g / mol, 1 mmol), 0.2 g (1 mmol) of 2,2-bis(mercaptomethyl)-1,3-propanedithiol, 0.01 g of azobisisoheptylcyanide, and 50 ml of dry hexafluoroisopropanol were added to a 100 ml reaction bottle and reacted at 55°C for 2 hours. 1 The reaction was tracked by H NMR until the double bond signal disappeared. Under nitrogen protection, 0.445 g (3 mmol) of vinyltrimethoxysilane and 0.01 g of azobisisoheptylcyanide were added, and the reaction was continued at 55 °C for 6 hours. The reaction was tracked by 1H NMR until the double bond signal disappeared. No further treatment was required, and the reaction solution was directly diluted with HFE7200 (nonafluorobutyl ether) to obtain anti-fingerprint agent 3, which can be used for anti-fingerprint coating of glass substrates.

[0050] .

[0051] Example 4

[0052] Under nitrogen protection, 4.6 g of allyl-terminated perfluoropolyether (Mn=4600 g / mol, 1 mmol), 1.02 g (1 mmol) of POSS-SH8, 0.03 g of azobisisoheptylcyanide, and 100 ml of hexafluoroisopropanol were added to a 250 ml reaction bottle and reacted at 55 °C for 2 hours. 1 HNMR followed the reaction until the double bond signal disappeared. The reaction solution was cooled to below -20°C, and under nitrogen protection, 0.8 g (7 mmol) of allyl glycidyl ether and 0.08 g of TPO photoinitiator were added. The reaction was irradiated with 365 nm ultraviolet light for 3 hours at a temperature not exceeding -10°C. 1 The reaction was tracked by H NMR until the double bond signal disappeared. The reaction solution was concentrated to obtain a viscous liquid product. The product was dissolved in tetrahydrofuran and added to the epoxy system coating in an amount of 0.5% by mass to obtain an anti-graffiti coating 4.

[0053] The reaction equation is as follows: .

[0054] Application and performance:

[0055] The perfluoropolyether compound obtained in the above examples is applied to different coating systems to obtain a coating with antifouling properties.

[0056] The antifouling coating formed above was directly subjected to the following performance tests, and the test results are shown in the table below.

[0057] (1) Contact angle test

[0058] The static contact angles of water and hexadecane were measured using a contact angle tester. The measurement was carried out at room temperature, and the coating sample to be tested was laid flat on the horizontal platform of the contact angle tester and fixed, with a droplet size of 3 μl.

[0059] (2) Sliding angle test

[0060] The sliding angle of water and hexadecane was measured using a contact angle tester. The measurement was carried out at room temperature. The coating sample to be tested was fixed flat on the horizontal platform of the contact angle tester. The coating plane was slowly tilted at a speed of 0.5° / s. The platform angle when the droplet just started to slide was the sliding angle. The droplet size was 30 microliters.

[0061] Table 1 Test results of coating antifouling performance

[0062]

[0063] a. The perfluoropolyether compound obtained in Example 1 and Example 2 was added to a UV coating curing liquid for PET at a mass percentage of 5‰, and coated on the surface of the PET material after low-temperature plasma treatment, and then heat treated at 100°C for 2 minutes, and then cured by ultraviolet light to obtain an antifouling coating on the surface of the PET substrate.

[0064] b. The perfluoropolyether compound obtained in Example 3 was dissolved in HFE7200 (nonafluorobutyl ether) solvent at a concentration of 5‰ by mass. The glass substrate treated with low-temperature plasma was immersed in the above solution, taken out and dried, and treated at 130°C for 1 hour to obtain an antifouling coating on the surface of the glass substrate.

[0065] c. The perfluoropolyether compound obtained in Example 4 was added to the epoxy resin coating at a mass percentage of 5‰, and diluted with ethyl acetate to a solid content of 30%, which was applied to the surface of the tinplate material after low-temperature plasma treatment, and then cured at 100°C for 6 hours to obtain an antifouling coating on the surface of the tinplate substrate.

[0066] It can be seen from the test results that the perfluoropolyether compound prepared by the present invention can be dissolved in common solvents such as esters and ketones, and can be applied to different coating systems and different substrates. The obtained coating has good hydrophobic and oleophobic properties, especially for different test liquids, it has a very low sliding angle, which makes it easy for different pollutants to slide off its surface. Therefore, from the application test results, this is in line with the original intention of the present invention.

[0067] (3) Coating durability test and analysis of the results of the static initial angle with water

[0068] First, when the surface treatment layer is formed and there is no contact (i.e. the number of frictions is zero), the angle measured is the initial angle. Then, the steel wool friction durability evaluation is carried out. Specifically, 0000# steel wool (size 5mmx5mmx2mm) is used to contact the surface treatment layer, and a load of 1kg is applied thereon. Then, in this load-applied contact state, the steel wool is reciprocated a certain number of times at a speed of 60 times / minute, and the static contact angle of water on the contact surface is measured as the evaluation.

[0069] Table 2 Test results of wear resistance of antifouling coating on PET surface

[0070]

[0071] Note: 1) The comparative compound is Shin-Etsu KY1203, which is also a compound with perfluoropolyether end-grafted with acrylate.

[0072] 2) The perfluoropolyether compound obtained in Example 2 and the comparative compound 1 (Shin-Etsu KY1203) were added to a UV coating curing liquid dedicated to PET at a mass ratio of 5‰, coated on the surface of the PET material after low-temperature plasma treatment, and then heat treated at 100°C for 2 minutes, and then cured by ultraviolet light to obtain an antifouling coating on the surface of the PET substrate.

[0073] Table 3 Test results of wear resistance of antifouling coating on glass surface

[0074]

[0075] Note: 1) The comparison compound is Daikin OPTOOL UD509, which is also a compound with trimethoxysilane grafted onto the end of perfluoropolyether.

[0076] 2) The perfluoropolyether compound obtained in Example 3 and the comparative compound 2 (Daikin OPTOOL UD509) were dissolved in HFE7200 (nonafluorobutyl ether) solvent at a concentration of 5‰ by mass, and the glass substrate treated with low-temperature plasma was immersed in the above solution, taken out and dried, and treated at 130°C for 1 hour to obtain an antifouling coating on the surface of the glass substrate.

[0077] It can be seen from the test results of Examples 2 and 3 and the comparative example that the static contact angle of water of the perfluoropolyether compound with a branched structure at the end prepared by the present invention applied to the antifouling coating is greater than the contact angle of the control compound. At the same time, the contact angle test results measured after wiping the horizontal coating sample with steel wool show that the wear resistance of the antifouling coating prepared by the perfluoropolyether compound with a branched structure at the end prepared by the present invention is better than that of the comparative example. This shows that the perfluoropolyether compound with a branched structure at the end prepared by the present invention has excellent comprehensive performance, which is in line with the original intention of the present invention.

Claims

1. A perfluoropolyether graft-modified compound, characterized in that: The general structural formula of the perfluoropolyether grafted modified compound is Wherein X is one or more of an amide group, an ester group, an ether group, and an amine group; and Y has a branched structure, and the branched structure contains at least two -SR terminal groups; The R contains a functional group; wherein the functional group includes one or more of a hydroxyl group, an amino group, a hydrazide group, a benzophenone group, a (meth)acryloxy group, an epoxy group, and a trialkoxysilane group; Wherein m is an integer from 0 to 28, and n is a positive integer from 1 to 2; The PFPE is a perfluoropolyether chain; wherein the perfluoropolyether chain is one of Z type, K type, Y type, and D type, and has a molecular weight of 300 to 20,000; Wherein Y include: At least one of .

2. The perfluoropolyether graft-modified compound according to claim 1, characterized in that: The R includes: At least one of .

3. The perfluoropolyether graft-modified compound according to claim 1, characterized in that: The grafted modified compound is: Wherein, m is an integer from 0 to 28, and n is a positive integer from 1 to 2.

4. A method for preparing the perfluoropolyether graft-modified compound according to claim 1, comprising: The raw materials of the perfluoropolyether polythiol compound and the compound containing olefin double bonds and functional groups are subjected to a grafting reaction to obtain a perfluoropolyether graft-modified compound; The preparation method of the perfluoropolyether multimercapto compound comprises: mixing a perfluoropolyether with an olefin double bond at the end, a multimercapto compound with a branched structure, an initiator, and a solvent, and obtaining the perfluoropolyether multimercapto compound through a thiol-olefin click reaction; wherein the perfluoropolyether with an olefin double bond at the end is Wherein X is one or more of amide group, ester group, ether group, and amine group; The compounds containing olefin double bonds and functional groups include: One or more of the .

5. An antifouling composition, characterized in that The composition comprises the perfluoropolyether graft-modified compound according to any one of claims 1 to 3 and an organic solvent.

6. The antifouling composition according to claim 5, characterized in that: The organic solvent includes at least one of a fluorine-containing solvent, an alcohol, an ester, a ketone, and an ether non-fluorine organic solvent.

7. The antifouling composition according to claim 5, characterized in that: The composition contains coating; the coating is at least one of acrylic coating, epoxy coating, phenolic coating, alkyd coating, polyurethane coating, amino coating, polysiloxane coating, vinyl resin coating and light-curing coating.

8. Use of the antifouling composition according to any one of claims 5 to 7 in anti-fingerprint agents, anti-graffiti coatings, and surface treatment agents.