Preparation method of self-repairing dispersion function positive electrode binding material, positive electrode slurry and preparation method thereof, and preparation method of positive electrode sheet
By using a twin-screw extrusion method in lithium-ion batteries to prepare a self-healing dispersion functional cathode binding material, combined with a cross-linking system of β-cyclodextrin and gallic acid, the problem of insufficient bonding force of the cathode material is solved and the electrode performance is improved. The flexibility and cycle performance of the sheet enable efficient and low-cost battery electrode sheet preparation.
Patent Information
- Application Number
- CN202410803395.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-20
AI Technical Summary
Insufficient adhesion of cathode materials in existing lithium-ion batteries leads to deagglomeration of electrode particles and easy cracking of pole pieces. This is a serious problem especially in high-energy-density batteries. Moreover, the existing modification methods have low process efficiency, high pollution, and grafting. The rate is not high.
The PVDF powder is mixed with the initiator, graft monomer and self-healing functional monomer through a pulverizer, processed by a twin-screw extruder with an aspect ratio of L/D=40 under high temperature and high pressure, and spray-dried to prepare a self-healing dispersion. Functional cathode binding material, combined with a reversible cross-linking system of β-cyclodextrin and gallic acid, improves the flexibility and bonding strength of the binding material.
The preparation of high-efficiency, low-cost, and pollution-free positive electrode bonding materials has been achieved, which improves the flexibility and peeling force of the electrode piece, reduces the risk of cracking, and introduces self-healing effect through dynamic cross-linking to enhance cycle performance.
Smart Images

Figure CN118360015B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries, and specifically relates to a method for preparing a positive electrode adhesive material with a self-repairing dispersion function, a positive electrode slurry and a method for preparing the same, and a method for preparing a positive electrode sheet. Background Art
[0002] In the past few decades, polyvinylidene fluoride (PVDF)-based fluorinated polymers have been widely used in the preparation of electrode materials due to their remarkable thermal stability, chemical inertness, low surface energy, and unique electrical properties. However, because they rely on weak van der Waals forces to provide a bonding network, it can lead to deagglomeration of electrode particles, easy cracking of pole pieces, and easy capacity decay, especially in high energy density batteries. This defect is more prominent. Therefore, we will graft PVDF to improve its surface hydrophilicity and develop new fluorinated polymers with adjustable structures and properties to meet the diverse material requirements of different applications.
[0003] Patent CN102153704A discloses a method of modifying PVDF by co-radiation grafting of N-vinyl pyrrolidone (NVP) monomer and PVDF powder; Patent US 5576106 discloses a method of grafting unsaturated functional monomers onto the surface of powdered fluorinated polymers by radiation grafting.
[0004] Although the grafting method mentioned above can achieve a higher grafting rate, a large amount of solvent is used in the grafting process, which makes subsequent treatment troublesome.
[0005] Patent CN102603986A discloses a surface solid phase graft modified PVDF and a preparation method thereof, but the process requires strong alkali pretreatment and nitrogen protection, and the preparation efficiency is low.
[0006] Therefore, it is necessary to develop a new PVDF modification method with high efficiency, long-term use, low pollution and high grafting rate to solve the problems of electrode particle deagglomeration and electrode cracking caused by insufficient adhesion of positive electrode materials in existing lithium batteries. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a positive electrode adhesive material with self-repairing dispersion function, a positive electrode slurry and a method for preparing the positive electrode sheet.
[0008] The technical solution of the present invention is:
[0009] A method for preparing a self-repairing dispersion functional positive electrode bonding material, the method comprising:
[0010] (1) Mixing PVDF powder, appropriate amount of initiator, grafting monomer, and self-repairing functional monomer evenly by a pulverizer;
[0011] (2) Extruding the uniformly mixed sample into a PVDF modified product through a twin-screw extruder with a length-to-diameter ratio of L / D=40 under high temperature and high pressure reaction conditions;
[0012] (3) The obtained PVDF modified product is spray-dried to obtain the final product.
[0013] Furthermore, in step (1), the weight percentages of the reaction components are: 100 parts of PVDF; 10-20 parts of grafting monomer; 0.5 parts of initiator; and 5 parts of self-repairing functional monomer.
[0014] Furthermore, the PVDF is preferably PVDF binder Fonolin (2032).
[0015] Furthermore, in step (1), the grafting monomer is any one of methyl methacrylate phosphate (PM-2), glycidyl methacrylate (GMA), isopropyl bornyl methacrylate (IBOA), tetrahydrofuran methyl methacrylate (THFFA), vinyl acetate (VA), N-vinyl pyrrolidone (NVP), 1,6-hexanediol diacrylate (HDDA), neopentyl glycol diacrylate (NPGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA) and trimethylolpropane triacrylate (TMPTA), or a combination of at least two thereof.
[0016] Furthermore, the grafting monomer is preferably methyl methacrylate phosphate (PM-2).
[0017] Furthermore, in step (1), the self-repairing functional monomer is any one of β-cyclodextrin, calixarene, columnarene, and gallic acid, or a combination of at least two of them.
[0018] Furthermore, the self-repairing functional monomers are preferably β-cyclodextrin and gallic acid.
[0019] Furthermore, in step (1), the initiator is any one of di-tert-butyl peroxide (DTBP), di-tert-butyl isopropyl peroxide (BIBP), benzoyl peroxide (BPO), tert-butyl perbenzoate (TBPB), lauryl peroxide (LPO), diisopropyl peroxide (DCP), and tert-butyl isononanoate (TBPIN).
[0020] Furthermore, the initiator is preferably di-tert-butylcumene peroxide (BIBP).
[0021] Furthermore, in step (2), the twin-screw extruder is provided with six sections, wherein the temperatures of the first section to the sixth section are 30°C, 80°C, 160°C, 160°C, 160°C, and 150°C, respectively.
[0022] Furthermore, in step (2), the feed port of the twin-screw extruder is in the first section, the feed rate is 30 rpm, the screw speed is 40 rpm, and the average residence time of the material in the twin-screw extruder is 1.5-3 min.
[0023] Another technical solution of the present invention is:
[0024] A positive electrode slurry includes a solid material and an organic solvent; wherein the solid material, calculated by weight, includes: 2 parts of a self-repairing dispersible positive electrode adhesive material prepared by the method described above; 1 part of a conductive agent; and 97 parts of lithium iron phosphate.
[0025] Furthermore, the weight of the organic solvent accounts for 40% of the total weight of the positive electrode slurry.
[0026] Furthermore, the organic solvent is one or a combination of at least two of N-methylpyrrolidone, ethyl acetate, methyl propionate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.
[0027] Furthermore, the organic solvent is preferably N-methylpyrrolidone.
[0028] Furthermore, the conductive agent is one of KS-6, KS-15, SFG-6, SFG-15, acetylene black, Super P, Super S, 350G, carbon fiber, carbon nanotube, activated carbon, or a combination of at least two thereof.
[0029] Furthermore, the conductive agent is preferably Super P.
[0030] The third technical solution of the present invention is:
[0031] A method for preparing the positive electrode slurry as described above, the method comprising:
[0032] (1) adding and mixing the self-repairing dispersion function positive electrode binding material, a conductive agent and an organic solvent;
[0033] (2) The lithium iron phosphate is then added, stirred and dispersed to obtain a positive electrode slurry.
[0034] Furthermore, it is preferred that a high-speed deaerator is used for uniform stirring.
[0035] The fourth technical solution of the present invention is:
[0036] A method for preparing a positive electrode sheet, the method comprising:
[0037] (1) The positive electrode slurry as described above is uniformly dispersed and coated on the substrate using aluminum foil as the positive electrode substrate;
[0038] (2) The substrate coated with the positive electrode slurry is placed in an oven and dried at 105° C. to obtain a positive electrode sheet.
[0039] Furthermore, the positive electrode slurry has a wet thickness of 200 or 300 μm after coating.
[0040] The present invention provides a method for preparing a positive electrode bonding material with a self-repairing dispersion function, a positive electrode slurry and a method for preparing the same, and a method for preparing a positive electrode sheet, and the beneficial effects are:
[0041] (1) The preparation process of the positive electrode binder material of the present invention is simple, low-cost, short-time, high-efficiency, pollution-free, and can be produced continuously, thus meeting the conditions for industrial production;
[0042] (2) The method for preparing the self-repairing dispersion function positive electrode bonding material of the present invention reduces the crystallinity of the original bonding material through mechanical deformation, greatly improves the solubility of the bonding material, and improves the flexibility of the obtained electrode piece. At the same time, by setting the grafted monomer, the peeling force of the electrode piece is increased and the influence of the electrode piece cracking is reduced;
[0043] (3) The positive electrode slurry prepared by the present invention has good charge repulsion due to the grafting of phosphate groups, and the PVDF long chain itself has a certain steric hindrance effect, which greatly improves the slurry viscosity and stability;
[0044] (4) The positive electrode slurry prepared by the present invention realizes dynamic crosslinking due to the reversible crosslinking system of host-guest interaction between β-cyclodextrin and gallic acid, which can restore the broken bonds between polymer chains during continuous cycles, thereby introducing a self-healing effect; at the same time, the unique spatial network structure of β-cyclodextrin itself further maintains the stability of the slurry.
[0045] (5) The positive electrode sheet prepared by the present invention has a stronger contact between the two components due to the multi-dimensional hydrogen bond interaction between the hyperbranched network structure of β-cyclodextrin and the positive electrode material. At the same time, the chelation effect between the carboxyl group of gallic acid and the aluminum material increases the bonding force between the positive electrode material and the substrate. This bonding force will be tighter during the entire dynamic cross-linking process, thereby stabilizing the structure of the electrode film and enhancing the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is an enlarged view of the cracking degree of the 300um wet thickness dried electrode of Examples 1-3 and Comparative Example 1 when it is taken out and after being placed in the glove box for 48 hours. DETAILED DESCRIPTION
[0047] The present invention provides a method for preparing a self-repairing dispersion functional positive electrode bonding material, the method comprising:
[0048] (1) Mixing PVDF powder, appropriate amount of initiator, grafting monomer, and self-repairing functional monomer uniformly by a pulverizer;
[0049] (2) Extruding the uniformly mixed sample into a PVDF modified product through a twin-screw extruder with a length-to-diameter ratio of L / D=40 under high temperature and high pressure reaction conditions;
[0050] (3) The obtained PVDF modified product is spray-dried to obtain the final product.
[0051] In step (1), the mass fractions of the reaction components are: 100 parts of PVDF; 10-20 parts of grafted monomer; 0.5 parts of initiator; 5 parts of self-healing functional monomer, wherein the PVDF is PVDF binder Fonolin (2032), the grafted monomer is methyl methacrylate phosphate (PM-2), the initiator is di-tert-butyl isopropyl peroxide (BIBP), and the self-healing functional monomers are β-cyclodextrin and gallic acid.
[0052] The present invention also provides a positive electrode slurry, comprising a solid material and an organic solvent; wherein the solid material is calculated by weight and comprises: 2 parts of the self-healing dispersible functional positive electrode adhesive material prepared by the aforementioned method; 1 part of a conductive agent; 97 parts of lithium iron phosphate, wherein the organic solvent is N-methylpyrrolidone and the conductive agent is Super P.
[0053] The preparation method of the positive electrode slurry comprises:
[0054] (1) adding and mixing the self-repairing dispersion function positive electrode binder material, conductive agent and organic solvent;
[0055] (2) The lithium iron phosphate is then added, stirred and dispersed to obtain a positive electrode slurry.
[0056] The present invention also provides a method for preparing a positive electrode sheet, the method comprising:
[0057] (1) The above-mentioned positive electrode slurry dispersed evenly is coated on the substrate with aluminum foil as the positive electrode substrate;
[0058] (2) The substrate coated with the positive electrode slurry is placed in an oven and dried at 105° C. to obtain a positive electrode sheet.
[0059] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical solutions of the present invention are further described below in conjunction with embodiments. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.
[0060] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0061] Example 1: The preparation method of the self-repairing dispersion functional positive electrode bonding material and the positive electrode slurry is as follows:
[0062] (1) Weigh 100 parts of PVDF powder, 10 parts of methyl methacrylate phosphate (PM-2), 0.5 parts of di-tert-butyl isopropyl peroxide (BIBP), 2 parts of β-cyclodextrin and 3 parts of gallic acid and mix them evenly.
[0063] (2) Preheat the twin-screw extruder, then add the evenly mixed powder into the feed port for extrusion reaction, and spray dry the obtained modified PVDF to obtain the self-healing dispersed functional positive electrode binder material P1.
[0064] (3) Weigh 7 g of positive electrode binder P1 and dissolve it in 93 g of N-methylpyrrolidone. Stir the mixture in a water bath at 60°C with magnetic stirring at 300 rpm to see how long it takes to completely dissolve the solvent.
[0065] Specifically, a 7% self-healing dispersed functional positive electrode adhesive material P1 solution was dried in an 80°C forced air drying oven for 2 hours and then heated to 90°C for two hours to form a film. The film was cut into strips with a width of 15 mm and a length of 80 mm and placed in a horizontal peel strength machine for a tensile test.
[0066] (4) The solid material ratio of the lithium iron phosphate positive electrode slurry is as follows: 2wt% of the self-healing dispersion functional positive electrode binder material P1, 1wt% of the conductive agent Super P and 97wt% of lithium iron phosphate. The positive electrode slurry is composed of solid materials and N-methylpyrrolidone, wherein the weight of N-methylpyrrolidone accounts for 40% of the total weight of the positive electrode slurry.
[0067] In this embodiment, specifically, the self-healing dispersing functional positive electrode binder P1, Super P and N-methylpyrrolidone are mixed together, stirred in a degassing machine at a speed of 800 rpm / min for 20 seconds, and then lithium iron phosphate is added and stirred in a degassing machine at a speed of 2000 rpm / min for 20 minutes to obtain a positive electrode slurry.
[0068] In this embodiment, specifically, the positive electrode slurry is uniformly coated on the surface of the aluminum foil with a thickness of 200 um and 300 um respectively.
[0069] In this embodiment, specifically, the evenly dispersed slurry is used as the positive electrode sheet substrate using aluminum foil, and is evenly coated on the substrate with a thickness of 200um & 300um respectively.
[0070] In this embodiment, specifically, the manufactured positive electrode sheet is placed in an oven and dried at 105° C. for 30 min. & 1 h.
[0071] In this embodiment, specifically, the electrode sheet with a wet thickness of 200 um and dried is rolled and then tested for peel strength and folding endurance.
[0072] Furthermore, the electrode with a wet thickness of 300um and dried was placed under an electronic magnifying glass to observe its cracking degree, and was placed in a glove box for 48 hours to observe the cracking condition.
[0073] Example 2: The preparation method of the self-repairing dispersion functional positive electrode bonding material and the positive electrode slurry is as follows:
[0074] (1) Weigh 100 parts of PVDF powder, 15 parts of methyl methacrylate phosphate (PM-2), 0.5 parts of di-tert-butyl isopropyl peroxide (BIBP), 2 parts of β-cyclodextrin and 3 parts of gallic acid and mix them evenly.
[0075] (2) Preheat the twin-screw extruder, then add the evenly mixed powder into the feed port for extrusion reaction, and spray dry the obtained modified PVDF to obtain the self-healing dispersed functional positive electrode binder material P2.
[0076] (3) Weigh 7 g of self-healing dispersible functional positive electrode binder P2 and dissolve it in 93 g of N-methylpyrrolidone. Stir magnetically in a water bath at 60°C and at a speed of 300 rpm to observe the time required for complete solvent absorption.
[0077] Specifically, a 7% self-healing dispersed functional positive electrode adhesive material P2 solution was dried in an 80°C forced air drying oven for 2 hours and then heated to 90°C for two hours to form a film. The film was cut into strips with a width of 15 mm and a length of 80 mm and placed in a horizontal peel strength machine for a tensile test.
[0078] (4) The solid material ratio of the lithium iron phosphate positive electrode slurry is as follows: 2wt% of the self-healing dispersion functional positive electrode binder material P2, 1wt% of the conductive agent Super P and 97wt% of lithium iron phosphate. The positive electrode slurry is composed of solid materials and N-methylpyrrolidone, wherein the weight of N-methylpyrrolidone accounts for 40% of the total weight of the positive electrode slurry.
[0079] In this embodiment, specifically, the self-healing dispersing functional positive electrode binder P2, Super P and N-methylpyrrolidone are mixed together, stirred in a degassing machine at a speed of 800 rpm / min for 20 seconds, and then lithium iron phosphate is added and stirred in a degassing machine at a speed of 2000 rpm / min for 20 minutes to obtain a positive electrode slurry.
[0080] In this embodiment, specifically, the positive electrode slurry is uniformly coated on the surface of the aluminum foil with a thickness of 200 um and 300 um respectively.
[0081] In this embodiment, specifically, the evenly dispersed slurry is used as the positive electrode sheet substrate using aluminum foil, and is evenly coated on the substrate with a thickness of 200um & 300um respectively.
[0082] In this embodiment, specifically, the manufactured positive electrode sheet is placed in an oven and dried at 105° C. for 30 min. & 1 h.
[0083] In this embodiment, specifically, the electrode sheet with a wet thickness of 200 um and dried is rolled and then tested for peel strength and folding endurance.
[0084] In this embodiment, specifically, the electrode with a wet thickness of 300 um and dried was placed under an electronic magnifying glass to observe its cracking degree, and was placed in a glove box for 48 hours to observe the cracking condition.
[0085] Example 3, the preparation method of the self-repairing dispersion functional positive electrode bonding material and the positive electrode slurry is as follows:
[0086] (1) Weigh 100 parts of PVDF powder, 20 parts of methyl methacrylate phosphate (PM-2), 0.5 parts of di-tert-butyl isopropyl peroxide (BIBP), 2 parts of β-cyclodextrin and 3 parts of gallic acid and mix them evenly.
[0087] (2) Preheat the twin-screw extruder, then add the evenly mixed powder into the feed port for extrusion reaction, and spray dry the obtained modified PVDF to obtain the self-healing dispersed functional positive electrode binder material P3.
[0088] (3) Weigh 7 g of self-healing dispersible functional positive electrode binder P3 and dissolve it in 93 g of N-methylpyrrolidone. Stir magnetically in a water bath at 60°C and at a speed of 300 rpm to observe the time required for complete solvent absorption.
[0089] Specifically, a 7% self-healing dispersed functional positive electrode adhesive material P3 solution was dried in an 80°C forced air drying oven for 2 hours and then heated to 90°C for two hours to form a film. The film was cut into strips with a width of 15 mm and a length of 80 mm and placed in a horizontal peel strength machine for a tensile test.
[0090] (4) The solid material ratio of the lithium iron phosphate positive electrode slurry is as follows: 2wt% of the self-healing dispersion functional positive electrode binder material P3, 1wt% of the conductive agent Super P and 97wt% of lithium iron phosphate. The positive electrode slurry is composed of solid materials and N-methylpyrrolidone, wherein the weight of N-methylpyrrolidone accounts for 40% of the total weight of the positive electrode slurry.
[0091] In this embodiment, specifically, the self-healing dispersing functional positive electrode binder P3, Super P and N-methylpyrrolidone are mixed together, stirred in a degassing machine at a speed of 800 rpm / min for 20 seconds, and then lithium iron phosphate is added and stirred in a degassing machine at a speed of 2000 rpm / min for 20 minutes to obtain a positive electrode slurry.
[0092] In this embodiment, specifically, the positive electrode slurry is uniformly coated on the surface of the aluminum foil with a thickness of 200 um and 300 um respectively.
[0093] In this embodiment, specifically, the evenly dispersed slurry is used as the positive electrode sheet substrate using aluminum foil, and is evenly coated on the substrate with a thickness of 200um & 300um respectively.
[0094] In this embodiment, specifically, the manufactured positive electrode sheet is placed in an oven and dried at 105° C. for 30 min. & 1 h.
[0095] In this embodiment, specifically, the electrode sheet with a wet thickness of 200 um and dried is rolled and then tested for peel strength and folding endurance.
[0096] In this embodiment, specifically, the electrode with a wet thickness of 300 um and dried was placed under an electronic magnifying glass to observe its cracking degree, and was placed in a glove box for 48 hours to observe the cracking condition.
[0097] Comparative Example 1: The preparation method of the positive electrode binding material and the positive electrode slurry is as follows:
[0098] (1) Weigh 7 g of positive electrode binder material Fonolin (2032) and dissolve it in 93 g of N-methylpyrrolidone. Stir magnetically in a water bath at 60°C and at a speed of 300 rpm to observe the time required for complete solvent absorption.
[0099] Furthermore, the 7% positive electrode adhesive material solution was dried in a blast drying oven at 80°C for 2 hours and then heated to 90°C for two hours to form a film. The film was cut into strips with a width of 15 mm and a length of 80 mm and placed in a horizontal peel strength machine for a tensile test.
[0100] (2) The solid material ratio of the lithium iron phosphate positive electrode slurry is as follows: 2wt% of the positive electrode binder material Fonolin (2032), 1wt% of the conductive agent Super P and 97wt% of lithium iron phosphate. The positive electrode slurry is composed of solid materials and N-methylpyrrolidone, wherein the weight of N-methylpyrrolidone accounts for 40% of the total weight of the positive electrode slurry.
[0101] In this embodiment, specifically, the positive electrode binder material Fonolin (2032), Super P and N-methylpyrrolidone are mixed together, stirred in a degassing machine at a speed of 800 rpm / min for 20 seconds, and then lithium iron phosphate is added and stirred in a degassing machine at a speed of 2000 rpm / min for 20 minutes to obtain a positive electrode slurry.
[0102] In this embodiment, specifically, the positive electrode slurry is uniformly coated on the surface of the aluminum foil with a thickness of 200 um and 300 um respectively.
[0103] In this embodiment, specifically, the evenly dispersed slurry is used as the positive electrode sheet substrate using aluminum foil, and is evenly coated on the substrate with a thickness of 200um & 300um respectively.
[0104] In this embodiment, specifically, the manufactured positive electrode sheet is placed in an oven and dried at 105° C. for 30 min. & 1 h.
[0105] In this embodiment, specifically, the electrode sheet with a wet thickness of 200 um and dried is rolled and then tested for peel strength and folding endurance.
[0106] In this embodiment, specifically, the electrode with a wet thickness of 300 um and dried was placed under an electronic magnifying glass to observe its cracking degree, and was placed in a glove box for 48 hours to observe the cracking condition.
[0107] In this embodiment, specifically, the dissolution performance test results of the above-mentioned embodiments 1-3 and comparative example 1 are shown in the following Table 1.
[0108] Table 1 Dissolution performance test results of Examples 1-3 and Comparative Example 1
[0109]
[0110] In the present embodiment, specifically, by comparing Examples 1-3 with Comparative Example 1, it can be seen that: 1. The dissolution time of the self-healing dispersion functional positive electrode adhesive material of the present invention is reduced compared with the positive electrode adhesive material Funolin (2032). When the grafted monomer reaches more than 15 parts, the dissolution time no longer decreases, and is reduced by up to 37.5%; 2. The 7% solution viscosity of the self-healing dispersion functional positive electrode adhesive material of the present invention is reduced by 30% to 40% compared with the positive electrode adhesive material Funolin (2032).
[0111] In this embodiment, specifically, the test results of the film properties of the above embodiments 1-3 and comparative example 1 are shown in Table 2 below.
[0112] Table 2 Test results of film properties of Examples 1-3 and Comparative Example 1
[0113]
[0114] In this embodiment, specifically, by comparing Examples 1-3 with Comparative Example 1, it can be seen that: 1. The flexibility of the self-healing dispersion functional positive electrode adhesive material of the present invention is improved, and the elongation of the film is close to twice that of the positive electrode adhesive material Fonolin (2032). The reduction in the elastic modulus further illustrates that the toughness of the self-healing dispersion functional positive electrode adhesive material of the present invention is improved; 2. When the grafted monomer is 15 parts, the flexibility of the self-healing dispersion functional positive electrode adhesive material of the present invention is improved to a near saturation state.
[0115] In this embodiment, specifically, the slurry performance test results of the above embodiments 1-3 and comparative example 1 are shown in Table 3 below.
[0116] Table 3 Slurry performance test results of Examples 1-3 and Comparative Example 1
[0117]
[0118] In this embodiment, specifically, the viscosity detection method is as follows: the sample is placed in a constant temperature water bath at 25°C for 1 hour, and is detected using a NDJ-5S digital rotational viscometer, using a No. 4 rotor, a rotation speed of 12 rpm, and a detection temperature of 25°C.
[0119] In this embodiment, specifically, by comparing Examples 1-3 with Comparative Example 1, it can be seen that: 1. As the amount of grafted monomer increases, the slurry viscosity gradually decreases. When the grafted monomer is 20 parts, the slurry viscosity is 62% lower than the viscosity of the control sample; 2. The slurry made of the self-healing dispersion functional positive electrode adhesive material of the present invention has better stability, which only increased by about 30% in 24 hours, while the slurry made of the positive electrode adhesive material Fonolin (2032) increased by nearly 130% in 24 hours.
[0120] In this embodiment, specifically, the peel strength and folding endurance test results of the 200 um wet thickness dried electrode sheets of the above-mentioned embodiments 1-3 and comparative example 1 are shown in Table 4 below.
[0121] Table 4 Peel strength and folding endurance test results of 200um wet thickness dried electrodes of Examples 1-3 and Comparative Example 1
[0122]
[0123] In this embodiment, specifically, the above-mentioned peeling force detection method is: the pole piece rolled to a compaction density of 2.4g / m3 is cut into a sample strip of 15mm×200mm, and tested using a 180° horizontal peel strength tester with a speed of 150mm / min and a test temperature of 23°C.
[0124] In this embodiment, specifically, the above-mentioned folding resistance test method is: the electrode piece is rolled to a compaction density of 2.4g / m3, the electrode piece is cut into a sample strip of 15mm×200mm, and the coated surface and the aluminum foil surface are folded once respectively, until the sample strip cracks.
[0125] In the present embodiment, specifically, by comparing Examples 1-3 with Comparative Example 1, it can be seen that: 1. The peeling strength of the positive electrode sheet prepared by the self-healing dispersion functional positive electrode adhesive material of the present invention is significantly increased. When the grafted monomer is 10 parts, the peeling force is about 5 times that of the positive electrode sheet made of the positive electrode adhesive material Fonolin (2032); 2. With the increase of the grafted monomer, the peeling force and folding resistance will decrease. When the grafted monomer is 15 parts, it is the optimal grafting amount.
[0126] See also Figure 1 ,like Figure 1 Shown are enlarged views of the cracking degree of the 300um wet-thick dried electrodes of Examples 1-3 and Comparative Example 1 when taken out and after being placed in the glove box for 48 hours.
[0127] In the present embodiment, specifically, by comparing embodiments 1-3 with comparative example 1, it can be seen that: 1. The anti-cracking effect of the positive electrode sheet prepared by the self-healing dispersion functional positive electrode adhesive material of the present invention is far better than the positive electrode sheet made of the positive electrode adhesive material Funolin (2032); 2. The anti-cracking effect decreases slightly with the increase of grafted monomers; 3. When placed in a glove box for 48 hours, the positive electrode sheet prepared by the self-healing dispersion functional positive electrode adhesive material of the present invention has fewer cracks or even disappears, while the cracks of the positive electrode sheet made of the positive electrode adhesive material Funolin (2032) have no improvement.
[0128] In summary, the preparation method of the self-repairing dispersion function positive electrode binding material, the positive electrode slurry and the preparation method thereof, and the preparation method of the positive electrode sheet of the present invention have the following beneficial effects:
[0129] (1) The preparation method of the self-repairing dispersion function positive electrode bonding material of the present invention reduces the crystallinity of the original bonding material through mechanical deformation and grafting monomers, greatly improves the solubility of the bonding material, and improves the flexibility of the obtained electrode piece, thereby reducing the impact of electrode piece cracking;
[0130] (2) The positive electrode slurry prepared by the present invention has good charge repulsion due to the grafting of phosphate groups, and the PVDF long chain itself has a certain steric hindrance effect, which greatly improves the slurry viscosity and stability;
[0131] (3) The positive electrode slurry prepared by the present invention realizes dynamic crosslinking due to the reversible crosslinking system of host-guest interaction between β-cyclodextrin and gallic acid, which can restore the broken bonds between polymer chains during continuous cycles, thereby introducing a self-healing effect; at the same time, the unique spatial network structure of β-cyclodextrin itself further maintains the stability of the slurry.
[0132] (4) The positive electrode sheet prepared by the present invention has a stronger contact between the two components due to the multi-dimensional hydrogen bond interaction between the hyperbranched network structure of β-cyclodextrin and the positive electrode material. At the same time, the chelation effect between the carboxyl group of gallic acid and the aluminum material increases the bonding force between the positive electrode material and the substrate. This bonding force will be tighter during the entire dynamic cross-linking process, thereby stabilizing the structure of the electrode film and enhancing the cycle performance.
[0133] In this embodiment, specifically, the self-repairing and dispersing functional positive electrode adhesive material prepared by this extrusion method has a simple production process, low cost, short time, high efficiency, no pollution, can be produced continuously, and has the conditions for industrial production.
[0134] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a self-repairing dispersion functional positive electrode bonding material, characterized in that: The method includes: (1) Mixing PVDF powder, appropriate amount of initiator, grafting monomer, and self-repairing functional monomer uniformly by a pulverizer; (2) Extruding the uniformly mixed sample through a twin-screw extruder with a length-to-diameter ratio of L / D=40 under high temperature and high pressure reaction conditions to produce a PVDF modified product; (3) spray drying the obtained PVDF modified product to obtain the final product; In step (1), the weight percentages of the reaction components are: 100 parts of PVDF; 10-20 parts of grafting monomer; 0.5 parts of initiator; 5 parts of self-repairing functional monomer; The self-repairing functional monomer is 2 parts of β-cyclodextrin and 3 parts of gallic acid.
2. The method for preparing a self-repairing dispersion functional positive electrode bonding material according to claim 1, characterized in that: In step (1), the grafting monomer is any one of methyl methacrylate phosphate, glycidyl methacrylate, isopropyl bornyl methacrylate, tetrahydrofuran methyl methacrylate, vinyl acetate, N-vinyl pyrrolidone, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate and trimethylolpropane triacrylate, or a combination of at least two thereof.
3. The method for preparing a self-repairing dispersion functional positive electrode bonding material according to claim 1, characterized in that: In step (1), the initiator is any one of di-tert-butyl peroxide, di-tert-butyl isopropyl peroxide, benzoyl peroxide, tert-butyl perbenzoate, dodecyl peroxide, diisopropyl peroxide, and tert-butyl isononanoate peroxide.
4. The method for preparing a self-repairing dispersion functional positive electrode bonding material according to claim 1, characterized in that: In step (2), the twin-screw extruder is provided with six sections, wherein the temperatures of the first section to the sixth section are 30°C, 80°C, 160°C, 160°C, 160°C, and 150°C, respectively.
5. The method for preparing a self-repairing dispersion functional positive electrode bonding material according to claim 1, characterized in that: In step (2), the feed port of the twin-screw extruder is in the first section, the feed rate is 30 rpm, the screw speed is 40 rpm, and the average residence time of the material in the twin-screw extruder is 1.5-3 min.
6. A positive electrode slurry, characterized in that: Includes solid materials and organic solvents; The solid material is calculated by weight and includes: 2 parts of the self-healing dispersible functional positive electrode adhesive material prepared by the method according to any one of claims 1 to 5; 1 part of the conductive agent; and 97 parts of lithium iron phosphate.
7. A method for preparing a positive electrode slurry as claimed in claim 6, characterized in that: The method includes: (1) adding and mixing the self-repairing dispersion function positive electrode binding material, a conductive agent and an organic solvent; (2) The lithium iron phosphate is then added, stirred and dispersed to obtain a positive electrode slurry.
8. A method for preparing a positive electrode sheet, characterized in that: The method includes: (1) The cathode slurry as claimed in claim 6 is uniformly coated on an aluminum foil as a cathode substrate; (2) The substrate coated with the positive electrode slurry is placed in an oven and dried at 105° C. to obtain a positive electrode sheet.