Preparation method of heat transfer heat printing explosion-proof tempered glass photo frame and heat transfer heat printing explosion-proof tempered glass photo frame
Through the electric heating tempering of soda-lime-silica glass, the preparation of nano-titanium dioxide-graphene oxide composite particles and the use of silane-modified isophorone, combined with electrostatic-assisted thermal transfer technology, the problem of poor impact resistance and automatic self-adjustment of traditional glass photo frames has been solved. The problems of poor cleanability and low pattern transfer quality have been solved, and a high-performance explosion-proof tempered glass photo frame has been realized.
Patent Information
- Application Number
- CN202410443579.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-04-13
AI Technical Summary
Traditional glass photo frames have poor impact resistance, poor self-cleaning performance, low pattern transfer quality, and immature tempering processes, which are prone to self-explosion and other problems.
Soda-lime-silica glass is used for electric heating and tempering to prepare nano-titanium dioxide-graphene oxide composite particles and silane-modified isophorone. Combined with electrostatic-assisted thermal transfer technology, a composite coating is prepared and hot-pressed to improve the coating's durability. Self-cleaning, abrasion resistance and pattern fineness.
The explosion-proof, self-cleaning, high-definition pattern glass photo frame has been realized, which improves the safety, beauty and durability of the glass photo frame, and significantly improves the impact resistance and pattern transfer quality.
Smart Images

Figure CN118370462B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal transfer photo frames, in particular to a preparation method of a thermal transfer heat transfer explosion-proof tempered glass photo frame and a thermal transfer heat transfer explosion-proof tempered glass photo frame. Background Art
[0002] Glass photo frames are widely used in home decoration and commercial display due to their advantages such as lightness, transparency and easy cleaning. However, traditional glass photo frames have many shortcomings and are in urgent need of further technological innovation and improvement.
[0003] Most existing glass photo frames use ordinary float glass as the base material, which has poor impact resistance and is very easy to break during use, threatening the personal safety of users. Although tempered glass photo frames are available on the market, their tempering process is not mature yet, and the tempering stress distribution is uneven, which is prone to self-explosion and other problems.
[0004] In addition, glass photo frames are exposed to the environment for a long time, and their surfaces are easily adsorbed by dust, fingerprints and other stains, making them inconvenient to clean and maintain. The existing technology usually uses hydrophobic coatings to improve the self-cleaning performance of the glass surface, but the wear resistance and weather resistance of the coatings still need to be improved.
[0005] Glass surface pattern decoration is also a highlight of glass photo frames. However, traditional methods such as screen printing and inkjet printing often make it difficult to obtain high-precision and high-saturation pattern effects. Although thermal transfer technology has good color reproduction, the pattern is prone to deformation and blur during the transfer process, and the quality is not ideal.
[0006] In view of the above technical difficulties, it is urgent to provide a method for preparing a thermal transfer and heat transfer explosion-proof tempered glass photo frame. Summary of the invention
[0007] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a heat transfer and hot stamping explosion-proof tempered glass photo frame, and to develop a new type of glass photo frame that is explosion-proof, self-cleaning, wear-resistant and weather-resistant, and has high-precision patterns. This invention is expected to fundamentally solve many pain points of traditional glass photo frames, achieve an all-round improvement in the performance of glass photo frames, and bring consumers a safer, more beautiful, and more durable product experience.
[0008] The object of the present invention is to provide a method for preparing a heat transfer heat transfer explosion-proof tempered glass photo frame, comprising the following steps:
[0009] (1) Preparation of explosion-proof tempered glass: Select a soda-lime-silica glass sheet, place the glass sheet in an electric heating tempering furnace, keep it at 650-700°C for 4-6 hours, then quickly quench it for 2-5 minutes, and then slowly cool it to room temperature at 80-120°C;
[0010] (2) Preparation of nano titanium dioxide-graphene oxide composite particles: adding 1-3 parts by weight of graphene oxide powder to 100-300 parts by weight of deionized water, and ultrasonically dispersing for 30-60 minutes; adding 10-30 parts by weight of nano titanium dioxide powder, and ultrasonically dispersing for 30-60 minutes; filtering, washing 3-5 times, and drying at 80-120° C. for 4-8 hours;
[0011] (3) Preparation of silane-modified isophorone: 5-10 parts by weight of 3-aminopropyltriethoxysilane is added to 80-120 parts by weight of anhydrous ethanol; 15-25 parts by weight of isophorone is added, and the mixture is refluxed at 60-80° C. for 2-4 hours; and ethanol is removed by distillation under reduced pressure. The structural formula is as follows:
[0012]
[0013] (4) preparing a composite coating liquid: dissolving 25-35 parts by weight of a modified polyester resin in 150-250 parts by weight of xylene or 1,2,4,5-tetramethylbenzene; adding 3-8 parts by weight of nano titanium dioxide-graphene oxide composite particles, and ultrasonically dispersing for 30-60 minutes; adding 3-6 parts by weight of hexamethyldisiloxane and 15-25 parts by weight of silane-modified isophorone, and stirring for 30-60 minutes; and ball milling at 200-400 rpm for 2-4 hours;
[0014] (5) applying a composite coating: applying the composite coating liquid obtained in step (4) onto the explosion-proof film, with a coating thickness of 50-100 μm; drying at 80-120° C. for 10-30 minutes; and hot pressing with the tempered glass obtained in step (1) at 120-180° C. for 10-30 minutes;
[0015] (6) Thermal transfer: preparing a thermal sublimation ink comprising 3-6 parts by weight of (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one, 10-20 parts by weight of poly(styrene-butyl acrylate), and 70-85 parts by weight of ethyl acetate; inkjet printing a pattern on a transfer paper; aligning the transfer paper with the composite coated glass obtained in step (5), placing the paper in a flat-bed thermal transfer machine, and applying a 5-15 kV / cm electrostatic field on both sides of the transfer area; thermal transfer at 180-200° C. for 60-180 seconds. The chemical structure of (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one is as follows:
[0016]
[0017] Specifically, the size tolerance and thickness tolerance of the soda-lime-silica glass original sheet conform to the provisions of GB11614-2009 standard.
[0018] Specifically, the cooling air pressure for rapid quenching in step (1) is 0.2-0.4 MPa.
[0019] Specifically, the cooling rate of the slow cooling in step (1) is 2-5°C / min.
[0020] Specifically, the surface stress of the explosion-proof tempered glass obtained in step (1) is 90-120 MPa, and the impact resistance is such that a 50-gram steel ball falls freely from a height of 1 meter without breaking or cracking.
[0021] Specifically, the particle size of the nano titanium dioxide powder in step (2) is 20-50 nanometers.
[0022] Specifically, the number average molecular weight of the modified polyester resin in step (4) is 1000-5000.
[0023] Specifically, the poly(styrene-butyl acrylate) in step (6) has a styrene content of 60-80 mol % and a number average molecular weight of 50,000-100,000.
[0024] Specifically, the transfer paper used for thermal transfer in step (6) is acrylic transfer paper, and the resolution of inkjet printing is 600-1200dpi.
[0025] The invention discloses a method for preparing a heat transfer heat printing explosion-proof tempered glass photo frame and a heat transfer heat printing explosion-proof tempered glass photo frame.
[0026] The thermal transfer and heat transfer explosion-proof tempered glass photo frame is prepared by the method for preparing the thermal transfer and heat transfer explosion-proof tempered glass photo frame.
[0027] Compared with the prior art, the method for preparing the heat transfer and heat transfer explosion-proof tempered glass photo frame of the present invention can achieve the following beneficial effects:
[0028] 1. Nano-titanium dioxide has excellent photocatalytic performance. The band gap between its valence band and conduction band is about 3.2eV. It can be excited by visible light to generate electron-hole pairs; holes can react with water to generate hydroxyl radicals, which have strong oxidative degradation ability and can effectively decompose organic pollutants on the surface of the coating. At the same time, graphene oxide has extremely high specific surface area and mechanical strength. According to molecular orbital theory, there are a large number of epoxy, hydroxyl and carboxyl functional groups in graphene oxide, which makes its surface present rich chemical active sites. When titanium dioxide nanoparticles are loaded on graphene oxide sheets, a strong chemical bond can be formed between the two, which improves the dispersion stability of nanoparticles. In addition, graphene oxide can act as an electron acceptor, effectively promoting the separation of photogenerated electron-hole pairs in titanium dioxide, prolonging the carrier lifetime, and thus enhancing the photocatalytic activity. The close coupling of titanium dioxide and graphene oxide at the nanoscale achieves the synergistic improvement of photocatalytic performance and mechanical properties, giving the coating excellent self-cleaning and wear resistance.
[0029] The graphene sheets also play a nano-reinforcement role, embedded in the coating polymer matrix like steel bars, significantly improving the hardness, impact resistance and wear resistance of the coating by increasing the interface contact area and force transmission. The coupling of this mechanical reinforcement and the photocatalytic synergistic effect ultimately enables the nano-composite coating to obtain a series of unexpected excellent properties, providing a reliable guarantee for the practicality and durability of explosion-proof tempered glass photo frames.
[0030] 2. The present invention uses γ-aminopropyltriethoxysilane to modify isophorone. The silicon atom in the silane coupling agent has low electronegativity and empty 3d orbitals, which are easy to form coordination bonds and enhance the compatibility of the isophorone molecule with the coating matrix. At the same time, the silane group can undergo hydrolysis and condensation reactions to form a dense siloxane network structure, thereby improving the impact resistance and flexibility of the coating. In the silane coupling agent molecule, the ethoxy group can undergo hydrolysis and condensation reactions to form an inorganic siloxane skeleton structure, and cross-link with the polymer matrix through covalent bonds, thereby improving the hardness, wear resistance and impact resistance of the coating.
[0031] In addition, the γ-aminopropyl group can form hydrogen bonds with the ketocarbonyl group in the isophorone molecule, enhancing the physical compatibility of isophorone with the coating matrix, while also preventing the photodegradation reaction caused by ultraviolet light, and improving the photostability and weather resistance of isophorone. In summary, silane modification gives isophorone multiple performance improvements, allowing it to play an extraordinary role in the coating for explosion-proof tempered glass photo frames. Silane modification achieves uniform dispersion of isophorone in the coating matrix while taking into account mechanical properties.
[0032] 3. The traditional thermal transfer process is limited by the degree of ink spreading and penetration on the coating surface, and it is difficult to obtain high-resolution and high-saturation patterns. The present invention cleverly applies an electrostatic field during the transfer process, and uses the electric field force to directionally drive the migration of charged ink particles, which significantly improves the transfer quality. According to the theory of polymer physical chemistry, under high temperature conditions, the thermal motion of the molecular chain segments of the polymer intensifies and the free volume of the system increases. When an electrostatic field is applied, the charged particles in the ink accelerate their migration under the action of the electric field force, making it easier to break through the steric hindrance of the polymer molecular chain and penetrate deeply into the coating matrix. The external electric field can also induce polarization of the polymer matrix, so that it generates a stronger interaction force with the charged ink particles. The electrostatic effect promotes the uniform spreading of the ink particles on the coating surface, improving the fineness and color saturation of the pattern.
[0033] 4. (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one is a thermosensitive colorant with a unique molecular structure and photochromic mechanism. In the molecule, the diphenylamine group and the benzothiazol group act as electron donors and acceptors, respectively, and are conjugated to form a push-pull electron system. Under heating conditions, the charge transfer effect within the molecule is enhanced, and the absorption spectrum undergoes a red shift, causing a color change. This reversible thermochromic mechanism gives the transferred pattern a unique color-changing effect and anti-counterfeiting identification function. The benzene ring and carbon-carbon double bond conjugated system in the molecule can not only improve the thermal stability of the molecule, but also increase the polarizability of the molecule, which is beneficial to improving the coloring power and photostability of the colorant. In addition, the keto carbonyl group and nitrogen heterocycle in the molecule can also form hydrogen bonds with the coating matrix to improve the compatibility and retention rate of the colorant. The combination of these unique molecular structures and mechanisms enables the thermosensitive colorant to exhibit excellent transfer quality and color-changing effect during the thermal transfer process, providing a strong guarantee for the decorativeness and anti-counterfeiting properties of the product.
[0034] Based on the above analysis, the method of the present invention sublimates the pattern onto the explosion-proof tempered glass through high temperature. This technology has high color reproduction, simple operation, convenience and speed, and low cost of supporting equipment; and it is highly safe. The tempered and explosion-proof glass is not easy to break, and will not cause harm to people if it is broken;
[0035] The present invention has achieved a number of innovations in chemical mechanisms in the field of explosion-proof tempered glass photo frames: nanocomposite particles play a synergistic role to improve coating performance; silane-modified isophorone balances multiple performance requirements through molecular design; and electrostatic assisted thermal transfer improves pattern quality from a microscopic mechanism. These innovations in chemical mechanisms enable the explosion-proof tempered glass photo frame of the present invention to achieve technical effects far exceeding those of traditional products in terms of self-cleaning, mechanical properties, weather resistance, and pattern fineness. The high-performance explosion-proof tempered glass photo frame of the present invention can be mass-produced and has great economic value. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a physical picture of the heat transfer and heat transfer explosion-proof tempered glass photo frame of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0038] Example 1
[0039] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0040] (1) Preparation of explosion-proof tempered glass: Select a soda-lime-silica glass sheet whose size tolerance and thickness tolerance meet the GB11614-2009 standard, keep it at 650°C for 4 hours, then quickly quench it at 0.2MPa wind pressure for 2 minutes, and then slowly cool it to room temperature at 80°C at a rate of 2°C / min. The surface stress of the obtained explosion-proof tempered glass is 90MPa, and it will not break or crack when impacted by a 50g steel ball falling from a height of 1m;
[0041] (2) Preparation of nano-titanium dioxide-graphene oxide composite particles: adding 1 part by weight of graphene oxide powder to 100 parts by weight of deionized water, and ultrasonically dispersing for 30 minutes; adding 10 parts by weight of nano-titanium dioxide powder with a particle size of 20 nanometers, and ultrasonically dispersing for 30 minutes; filtering, washing 3 times, and drying at 80°C for 4 hours;
[0042] (3) Preparation of silane-modified isophorone: 5 parts by weight of 3-aminopropyltriethoxysilane was added to 80 parts by weight of anhydrous ethanol; 15 parts by weight of isophorone was added, and the mixture was refluxed at 60° C. for 2 hours; and ethanol was removed by distillation under reduced pressure;
[0043] (4) preparing a composite coating liquid: dissolving 25 parts by weight of a modified polyester resin having a number average molecular weight of 1000 in 150 parts by weight of xylene; adding 3 parts by weight of the composite particles obtained in step 2, and ultrasonically dispersing for 30 minutes; adding 3 parts by weight of hexamethyldisiloxane and 15 parts by weight of the silane-modified isophorone obtained in step 3, and stirring for 30 minutes; and ball milling at 200 rpm for 2 hours;
[0044] (5) Applying a composite coating: applying the composite coating liquid obtained in step 4 onto the explosion-proof film, with a coating thickness of 50 μm; drying at 80° C. for 10 minutes; and hot pressing with the tempered glass obtained in step 1 at 120° C. for 10 minutes;
[0045] (6) Thermal transfer: prepare a thermal sublimation ink comprising 3 parts by weight of (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one, 10 parts by weight of poly(styrene-butyl acrylate) (styrene content 60 mol%, number average molecular weight 50,000), and 70 parts by weight of ethyl acetate; inkjet print a pattern on acrylic transfer paper at a resolution of 600 dpi; align the transfer paper with the composite coated glass obtained in step 5, place them in a flatbed thermal transfer machine, and apply an electrostatic field of 5 kV / cm on both sides of the transfer area; and perform thermal transfer at 180°C for 60 seconds.
[0046] Example 2
[0047] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0048] (1) Preparation of explosion-proof tempered glass: Selecting a soda-lime-silica glass sheet whose size tolerance and thickness tolerance meet the GB11614-2009 standard, keeping it at 700°C for 6 hours, then rapidly quenching it at a wind pressure of 0.4 MPa for 5 minutes, and then slowly cooling it to room temperature at a rate of 5°C / min at 120°C; the surface stress of the obtained explosion-proof tempered glass is 120 MPa, and it does not break or crack when impacted by a 50-g steel ball falling freely from a height of 1 meter;
[0049] (2) Preparation of nano-titanium dioxide-graphene oxide composite particles: 3 parts by weight of graphene oxide powder was added to 300 parts by weight of deionized water, and ultrasonic dispersion was performed for 60 minutes; 30 parts by weight of nano-titanium dioxide powder with a particle size of 50 nanometers was added, and ultrasonic dispersion was performed for 60 minutes; filtration was performed, washing was performed 5 times, and drying was performed at 120° C. for 8 hours;
[0050] (3) Preparation of silane-modified isophorone: adding 10 parts by weight of 3-aminopropyltriethoxysilane to 120 parts by weight of anhydrous ethanol; adding 25 parts by weight of isophorone, and refluxing at 80° C. for 4 hours; and removing ethanol by distillation under reduced pressure;
[0051] (4) preparing a composite coating liquid: dissolving 35 parts by weight of a modified polyester resin having a number average molecular weight of 5000 in 250 parts by weight of 1,2,4,5-tetramethylbenzene; adding 8 parts by weight of the composite particles obtained in step 2, and ultrasonically dispersing for 60 minutes; adding 6 parts by weight of hexamethyldisiloxane and 25 parts by weight of the silane-modified isophorone obtained in step 3, and stirring for 60 minutes; and ball milling at 400 rpm for 4 hours;
[0052] (5) Applying a composite coating: applying the composite coating liquid obtained in step 4 onto the explosion-proof film, with a coating thickness of 100 μm; drying at 120° C. for 30 minutes; and hot pressing with the tempered glass obtained in step 1 at 180° C. for 30 minutes;
[0053] (6) Thermal transfer: prepare a thermal sublimation ink comprising 6 parts by weight of (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one, 20 parts by weight of poly(styrene-butyl acrylate) (styrene content 80 mol%, number average molecular weight 100,000), and 85 parts by weight of ethyl acetate; inkjet print a pattern on acrylic transfer paper at a resolution of 1200 dpi; align the transfer paper with the composite coated glass obtained in step 5, place them in a flatbed thermal transfer machine, and apply an electrostatic field of 15 kV / cm on both sides of the transfer area; and perform thermal transfer at 200°C for 180 seconds.
[0054] Example 3
[0055] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0056] (1) Preparation of explosion-proof tempered glass: Select a soda-lime-silica glass sheet with a size tolerance and thickness tolerance that meets the GB11614-2009 standard, keep it at 675°C for 5 hours, then quickly quench it at a wind pressure of 0.3MPa for 3.5 minutes, and then slowly cool it to room temperature at 100°C at a rate of 3.5°C / min. The surface stress of the obtained explosion-proof tempered glass is 105MPa, and it will not break or crack when impacted by a 50g steel ball falling from a height of 1m;
[0057] (2) The preparation of nano-titanium dioxide-graphene oxide composite particles, the preparation of silane-modified isophorone, the preparation of the composite coating liquid, the coating of the composite coating and thermal transfer were carried out according to the method of Example 1.
[0058] Example 4
[0059] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0060] (1) The preparation of explosion-proof tempered glass is carried out according to the method of Example 1;
[0061] (2) Preparation of nano-titanium dioxide-graphene oxide composite particles: adding 2 parts by weight of graphene oxide powder to 200 parts by weight of deionized water, and ultrasonically dispersing for 45 minutes; adding 20 parts by weight of nano-titanium dioxide powder with a particle size of 35 nanometers, and ultrasonically dispersing for 45 minutes; filtering, washing 4 times, and drying at 100° C. for 6 hours;
[0062] (3) The preparation of silane-modified isophorone, the preparation of the composite coating liquid, the coating of the composite coating and thermal transfer were carried out according to the method of Example 1.
[0063] Example 5
[0064] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0065] (1) The preparation of explosion-proof tempered glass and the preparation of nano-titanium dioxide-graphene oxide composite particles were carried out according to the method of Example 1;
[0066] (2) Preparation of silane-modified isophorone: adding 7.5 parts by weight of 3-aminopropyltriethoxysilane to 100 parts by weight of anhydrous ethanol; adding 20 parts by weight of isophorone, and reacting under reflux at 70° C. for 3 hours; and removing ethanol by distillation under reduced pressure;
[0067] (3) The preparation of the composite coating liquid, the coating of the composite coating and the thermal transfer are carried out according to the method of Example 1.
[0068] Example 6
[0069] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0070] (1) The preparation of explosion-proof tempered glass, the preparation of nano-titanium dioxide-graphene oxide composite particles, the preparation of silane-modified isophorone, the preparation of the composite coating liquid and the coating of the composite coating were carried out according to the method of Example 1;
[0071] (2) Thermal transfer: prepare a thermal sublimation ink comprising 4.5 parts by weight of (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one, 15 parts by weight of poly(styrene-butyl acrylate) (styrene content 70 mol%, number average molecular weight 75,000), and 77.5 parts by weight of ethyl acetate; inkjet print a pattern on acrylic transfer paper at a resolution of 900 dpi; align the transfer paper with the composite coated glass obtained in step 1, place them in a flatbed thermal transfer machine, and apply an electrostatic field of 10 kV / cm on both sides of the transfer area; and perform thermal transfer at 190°C for 120 seconds.
[0072] Example 7
[0073] The heat transfer heat printing explosion-proof tempered glass photo frame prepared by the preparation method of the heat transfer heat printing explosion-proof tempered glass photo frame described in Examples 1-6 is as follows Figure 1 shown.
[0074] Comparative Example 1
[0075] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0076] (1) The preparation of explosion-proof tempered glass is carried out according to the method of Example 1;
[0077] (2) Preparation of silane-modified isophorone: adding 7.5 parts by weight of 3-aminopropyltriethoxysilane to 100 parts by weight of anhydrous ethanol; adding 20 parts by weight of isophorone, and reacting under reflux at 70° C. for 3 hours; and removing ethanol by distillation under reduced pressure;
[0078] (3) preparing a composite coating liquid: dissolving 30 parts by weight of a modified polyester resin having a number average molecular weight of 3000 in 200 parts by weight of xylene; adding 4.5 parts by weight of hexamethyldisiloxane and 20 parts by weight of the silane-modified isophorone obtained in step 2, and stirring evenly; adding 3 parts by weight of N-[3-(triethoxysilyl)propyl]ethylenediamine-N,N-di(2-hydroxyethyl), and stirring for 45 minutes; and ball milling at 300 rpm for 3 hours;
[0079] (4) The coating and thermal transfer of the composite coating were carried out according to the method of Example 1; in Comparative Example 1, nano-titanium dioxide-graphene oxide composite particles were not added.
[0080] Comparative Example 2
[0081] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0082] (1) The preparation of explosion-proof tempered glass is carried out according to the method of Example 1;
[0083] (2) The preparation of nano-titanium dioxide-graphene oxide composite particles was carried out according to the method of Example 4.
[0084] (3) Preparation of composite coating liquid: dissolve 30 parts by weight of modified polyester resin with a number average molecular weight of 3000 in 200 parts by weight of 1,2,4,5-tetramethylbenzene; add 5.5 parts by weight of the composite particles obtained in step 2, and ultrasonically disperse for 45 minutes; add 4.5 parts by weight of hexamethyldisiloxane, and stir evenly; add 3 parts by weight of N-[3-(triethoxysilyl)propyl]ethylenediamine-N,N-di(2-hydroxyethyl), and stir for 45 minutes; and ball mill at 300 rpm for 3 hours.
[0085] (4) The coating and thermal transfer of the composite coating were carried out according to the method of Example 1. In Comparative Example 2, no silane-modified isophorone was added.
[0086] Comparative Example 3
[0087] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0088] (1) Preparation of explosion-proof tempered glass: Select a soda-lime-silica glass sheet whose size tolerance and thickness tolerance meet the GB11614-2009 standard, keep it at 650°C for 4 hours, then quickly quench it at 0.2MPa wind pressure for 2 minutes, and then slowly cool it to room temperature at 60°C at a rate of 2°C / min;
[0089] (2) The preparation of nano-titanium dioxide-graphene oxide composite particles, the preparation of silane-modified isophorone, the preparation of composite coating liquid, the coating of composite coating and thermal transfer were carried out according to the method of Example 1. Comparative Example 3 The quenching temperature was too low.
[0090] Comparative Example 4
[0091] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0092] (1) The preparation of explosion-proof tempered glass, the preparation of nano-titanium dioxide-graphene oxide composite particles, the preparation of silane-modified isophorone and the preparation of composite coating liquid were carried out according to the method of Example 1;
[0093] (2) Applying a composite coating: applying the composite coating liquid obtained in step 1 onto the explosion-proof film, with a coating thickness of 50 μm; drying at 150° C. for 10 minutes; and hot pressing with the explosion-proof tempered glass at 120° C. for 10 minutes;
[0094] (3) Thermal transfer was carried out according to the method of Example 1. The coating drying temperature of Comparative Example 4 was too high.
[0095] Comparative Example 5
[0096] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0097] (1) The preparation of explosion-proof tempered glass, the preparation of nano-titanium dioxide-graphene oxide composite particles, the preparation of silane-modified isophorone, the preparation of the composite coating liquid and the coating of the composite coating were carried out according to the method of Example 1;
[0098] (2) Thermal transfer: prepare a thermal sublimation ink, including 4.5 parts by weight of (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one, 15 parts by weight of poly(styrene-butyl acrylate) (styrene content 70 mol%, number average molecular weight 75000), and 77.5 parts by weight of ethyl acetate; inkjet print a pattern on acrylic transfer paper at a resolution of 900 dpi; align the transfer paper with the composite coated glass obtained in step 1, place it in a flatbed thermal transfer machine, and apply a 10 kV / cm electrostatic field on both sides of the transfer area; perform thermal transfer at 160°C for 120 seconds. The thermal transfer temperature of Comparative Example 5 is too low.
[0099] Comparative Example 6
[0100] The preparation method of the heat transfer heat transfer explosion-proof tempered glass photo frame comprises the following steps:
[0101] (1) The preparation of explosion-proof tempered glass, the preparation of nano-titanium dioxide-graphene oxide composite particles, the preparation of silane-modified isophorone, the preparation of the composite coating liquid and the coating of the composite coating were carried out according to the method of Example 1;
[0102] (2) Thermal transfer: Prepare a thermal sublimation ink, including 4.5 parts by weight of (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one, 15 parts by weight of poly(styrene-butyl acrylate) (styrene content 70 mol%, number average molecular weight 75000), and 77.5 parts by weight of ethyl acetate; inkjet print a pattern on acrylic transfer paper at a resolution of 900 dpi; align the transfer paper with the composite coated glass obtained in step 1, place it in a flatbed thermal transfer machine, and perform thermal transfer at 190° C. for 120 seconds, without applying an electrostatic field during the transfer process. In Comparative Example 6, no electrostatic field was applied.
[0103] In order to evaluate the performance advantages of the explosion-proof tempered glass photo frame of the present invention, the following test scheme was designed, and the samples of Examples 1-6 and Comparative Examples 1-6 were systematically tested.
[0104] The test items and test methods are as follows:
[0105] 1. Explosion-proof performance test: Use a 50g steel ball to fall freely from a height of 1 meter and record the glass breakage.
[0106] 2. Surface water contact angle test: Use a contact angle meter to measure the static water contact angle of the composite coating surface.
[0107] 3. Coating hardness test: Use a pencil hardness tester to test the pencil hardness of the coating.
[0108] 4. Wear resistance test: Use Taber abrasion tester, under 100g weight pressure, wear with CS-10 grinding wheel for 500 turns, and record the weight loss of the sample.
[0109] 5. Transfer pattern color saturation test: Use a spectrophotometer to measure the color intensity values of the transfer pattern in the red, green and blue channels.
[0110] 6. Weathering performance test: Use a xenon lamp aging test chamber, expose continuously for 200 hours at an irradiance of 0.55W / m2, and observe the changes in the appearance of the sample.
[0111] The test results are shown in the following table:
[0112]
[0113] Table 1
[0114] According to the test results in Table 1, the explosion-proof tempered glass photo frames prepared in Examples 1-6 can all pass the explosion-proof performance test, and the surface water contact angle is above 103°, with excellent hydrophobic self-cleaning performance. The coating hardness is above 2H, the wear resistance is excellent, and the mass loss after 500 revolutions of wear is less than 13.1 mg. The color saturation of the thermal transfer pattern is high, all above 91.9%. After the accelerated weathering test, the appearance of the sample has no obvious change, showing excellent weathering performance.
[0115] In contrast, in Comparative Example 1, nano-titanium dioxide-graphene oxide composite particles were not added, and the coating had low hardness, poor wear resistance, and unsatisfactory weather resistance. In Comparative Example 2, silane-modified isophorone was not introduced, and the sample failed to pass the explosion-proof performance test, and the surface hydrophobicity was poor. In Comparative Example 3, the quenching temperature was too low, the tempering effect was poor, and it also failed to pass the explosion-proof performance test. In Comparative Example 4, the coating drying temperature was too high, resulting in yellowing of the coating and reduced appearance quality. In Comparative Example 5, the thermal transfer temperature was too low, and the color saturation of the transfer pattern was significantly reduced. In Comparative Example 6, no electrostatic field was applied to assist the transfer, which also resulted in a decrease in the color saturation of the pattern.
[0116] Based on the test results, Example 2 has the best overall performance and is the best implementation method of the present invention.
[0117] The present invention ingeniously introduces nano titanium dioxide-graphene oxide composite particles into the coating, and utilizes the photocatalytic performance of titanium dioxide and the high strength of graphene to make the coating have excellent self-cleaning and mechanical properties. The addition of silane-modified isophorone not only improves the hydrophobicity of the coating surface, but also enhances the compatibility of isophorone with the coating substrate, thereby improving the overall performance.
[0118] Another major innovation of the present invention is to apply an electrostatic field during the thermal transfer process. The electrostatic field causes the charged particles in the transfer ink to migrate in a directional manner, significantly improving the accuracy and color saturation of the pattern transfer, while also accelerating the transfer speed and improving production efficiency.
[0119] In addition, the present invention optimizes the preparation process of explosion-proof tempered glass, reasonably controls the quenching temperature and the slow cooling rate, and while ensuring the explosion-proof performance of the glass, minimizes the non-uniformity of the tempering stress, so that the glass has better comprehensive mechanical properties.
[0120] In summary, the present invention overcomes the defects of poor self-cleaning, low pattern transfer quality, and fragility of traditional glass photo frames through key innovations such as nanocomposite particles, silane-modified isophorone, and electrostatic assisted thermal transfer, and achieves a perfect combination of explosion-proof, self-cleaning, high-saturation transfer, and weather resistance, significantly improving the user experience and practical value of glass photo frames. This invention has significant innovation and practicality, represents a major technological advancement in the field of glass photo frames, and has very broad application prospects.
[0121] The above comparative examples prepared a series of explosion-proof tempered glass photo frame samples with poor performance by changing the key process parameters of the present invention or omitting key components, thereby proving the rationality and superiority of the selection of components and process parameters of the present invention. In comparison, the explosion-proof tempered glass photo frame prepared by the present invention has obvious advantages in self-cleaning, mechanical properties, surface hydrophobicity, pattern transfer quality, etc. The design of the comparative examples specifically verifies the positive effects of key factors such as nanocomposite particles, modified isophorone, and electrostatic assisted thermal transfer on product performance. The preparation method provided by the present invention is scientific and reasonable, can be industrialized, and has significant technological advancement and practical value.
[0122] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.
Claims
1. The method for preparing a heat transfer explosion-proof tempered glass photo frame is characterized in that , including the following steps: (1) Preparing explosion-proof tempered glass: selecting a soda-lime-silica glass original sheet; placing the glass original sheet in an electric heating tempering furnace, keeping the temperature at 650-700° C. for 4-6 hours, then rapidly quenching for 2-5 minutes, and then slowly cooling to room temperature at 80-120° C.; (2) Preparation of nano-titanium dioxide-graphene oxide composite particles: adding 1-3 parts by weight of graphene oxide powder to 100-300 parts by weight of deionized water, and ultrasonically dispersing for 30-60 minutes; adding 10-30 parts by weight of nano-titanium dioxide powder, and ultrasonically dispersing for 30-60 minutes; filtering, washing 3-5 times, and drying at 80-120° C. for 4-8 hours; (3) Preparation of silane-modified isophorone: adding 5-10 parts by weight of 3-aminopropyltriethoxysilane to 80-120 parts by weight of anhydrous ethanol; adding 15-25 parts by weight of isophorone, and reflux reaction at 60-80° C. for 2-4 hours; and removing ethanol by distillation under reduced pressure; (4) preparing a composite coating liquid: dissolving 25-35 parts by weight of a modified polyester resin in 150-250 parts by weight of xylene or 1,2,4,5-tetramethylbenzene; adding 3-8 parts by weight of nano-titanium dioxide-graphene oxide composite particles, and ultrasonically dispersing for 30-60 minutes; adding 3-6 parts by weight of hexamethyldisiloxane and 15-25 parts by weight of silane-modified isophorone, stirring for 30-60 minutes, and ball milling at 200-400 rpm for 2-4 hours; (5) applying a composite coating: applying the composite coating liquid obtained in step (4) onto the explosion-proof film, with a coating thickness of 50-100 μm; drying at 80-120° C. for 10-30 minutes; and hot pressing with the tempered glass obtained in step (1) at 120-180° C. for 10-30 minutes; (6) Thermal transfer: preparing a thermal sublimation ink comprising 3-6 parts by weight of (E)-3-(4-(diphenylamino)phenyl)-1-(benzothiazol-2-yl)propylene-2-ene-1-one, 10-20 parts by weight of poly(styrene-butyl acrylate), and 70-85 parts by weight of ethyl acetate; inkjet printing a pattern on a transfer paper; aligning the transfer paper with the composite coated glass obtained in step (5), placing the paper in a flat-bed thermal transfer machine, and applying an electrostatic field of 5-15 kV / cm on both sides of the transfer area; thermal transfer at 180-200° C. for 60-180 seconds to obtain the thermal transfer heat transfer explosion-proof tempered glass photo frame; The cooling rate of the slow cooling in step (1) is 2-5°C / min; The surface stress of the explosion-proof tempered glass obtained in step (1) is 90-120 MPa, and the impact resistance is such that a 50-gram steel ball falls freely from a height of 1 meter without breaking or cracking. The particle size of the nano titanium dioxide powder in step (2) is 20-50 nanometers; The number average molecular weight of the modified polyester resin in step (4) is 1000-5000; The poly(styrene-butyl acrylate) in step (6) has a styrene content of 60-80 mol % and a number average molecular weight of 50,000-100,000.
2. The method for preparing the heat transfer explosion-proof tempered glass photo frame according to claim 1, characterized in that The size tolerance and thickness tolerance of the soda-lime-silica glass original sheet conform to the provisions of GB11614-2009 standard.
3. The method for preparing the heat transfer explosion-proof tempered glass photo frame according to claim 1, characterized in that , the cooling air pressure for rapid quenching in step (1) is 0.2-0.4 MPa.
4. The method for preparing the heat transfer heat transfer explosion-proof tempered glass photo frame according to claim 1, characterized in that ,The transfer paper used for thermal transfer in step (6) is acrylic transfer paper, and the resolution of inkjet printing is 600-1200 dpi.
5. The thermal transfer heat printing explosion-proof tempered glass photo frame prepared by the method for preparing the thermal transfer heat printing explosion-proof tempered glass photo frame as described in any one of claims 1 to 4.