A super hygroscopic polyethylene terephthalate film and preparation method thereof
By coating the polyethylene terephthalate film with cross-linked carboxymethylcellulose gel and using hydroxyl and carboxyl groups to form hydrogen bonds, the problem of poor reusability of hygroscopic films is solved and high efficiency is achieved. , environmentally friendly super hygroscopic properties, and reduces environmental pollution.
Patent Information
- Application Number
- CN202410806718.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Existing hygroscopic films have poor recyclability and cannot meet long-term use requirements. In addition, inorganic hygroscopic materials are harmful to the environment, are easily broken and fall off, and cannot be reused when dissolved in water.
Carboxymethyl cellulose and ethylene glycol diglycidyl ether are cross-linked under alkaline conditions to form a gel, which is broken into pieces, swollen and coated on a polyethylene terephthalate film, through hydroxyl and carboxyl groups. The groups form hydrogen bonds, improve the bonding strength, enhance the repeated moisture absorption performance, and improve the bonding fastness of the gel and membrane by removing sodium ions and cross-linking agents.
The highly hygroscopic polyethylene terephthalate film achieves high-efficiency repeated moisture absorption performance, maintains high moisture absorption capacity, has a biodegradation rate of 100%, is suitable for large-scale applications, and is low-cost.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of packaging materials and relates to a super hygroscopic polyethylene terephthalate film and a preparation method thereof. Background Art
[0002] During the packaging and storage of food, medicine, precision instruments and other items, the humidity requirements are often relatively high. For food and medicine, if there is too much moisture in the packaging bag, it is easy to breed microorganisms and cause the food to spoil; for precision instruments and electronic components, too high humidity environment is easy to cause metal surface corrosion and oxidation. Therefore, it is necessary to remove the humidity inside the package.
[0003] At present, in order to remove the humidity inside the package, the commonly used method is to add a small bag of independently packaged desiccant into the packaging container, which has the risk of leakage and accidental ingestion of the desiccant. Since the packaging container made of hygroscopic film can avoid leakage and accidental ingestion of the desiccant, it is of great significance to study how to prepare hygroscopic film.
[0004] The methods for preparing hygroscopic films in the prior art are generally divided into the following two categories:
[0005] One is blending, where the hygroscopic material is blended with a thermoplastic resin, and then a masterbatch with hygroscopic effect is prepared by granulation through an extruder. Finally, the masterbatch and other resins are put into a multilayer extruder to prepare a hygroscopic film by blow molding or casting. The hygroscopic materials used in the hygroscopic film prepared in this way are generally inorganic hygroscopic materials such as silica gel, activated carbon, calcium chloride, zeolite, molecular sieve, etc. The hygroscopic capacity of inorganic hygroscopic materials is low, and since inorganic hygroscopic materials will affect the film-forming properties of the film material, there is a very large limitation on the upper limit of their addition amount. Therefore, the hygroscopic effect of the hygroscopic film prepared in this way is small, and it cannot meet the use requirements after reuse, and the reusability of hygroscopicity is poor.
[0006] The other is coating, which involves coating inorganic hygroscopic materials such as silica sol and organic hygroscopic materials such as polymer absorbent resin onto the surface of the film substrate. These inorganic hygroscopic materials are easy to break and fall off, and organic hygroscopic materials will dissolve in water, so they cannot be reused.
[0007] For example, CN102838769A discloses a method for preparing a hygroscopic packaging film, which comprises using a mixture of polyvinyl alcohol resin, a polymer water-absorbing resin, methyl cellulose, a plasticizer, a stripping agent and water to form a mixed solution with bonding and film-forming properties, and subjecting the mixed solution to a coating process to form an independent hygroscopic film with hygroscopic function. However, this hygroscopic film can be completely dissolved in water, and the hygroscopic material is also easy to fall off from the substrate and cannot be reused.
[0008] For example, CN103194000A discloses a method for preparing a composite hygroscopic film, comprising the following steps: immersing a polymer hygroscopic film in a silica sol solution, treating the polymer hygroscopic film immersed in the silica sol solution under constant temperature and humidity conditions, and drying to obtain a composite hygroscopic film. However, the defect of this method is that after drying, the silica gel solution is in the form of solid particles, which are easily broken and fallen off during repeated moisture absorption, affecting the repeated moisture absorption performance of the film. In addition, silica gel is not easily degraded in nature, which has an adverse effect on the environment.
[0009] In summary, the hygroscopic films in the prior art generally have the disadvantage of poor reusability of hygroscopicity. Therefore, it is necessary to develop a hygroscopic film that can repeatedly absorb moisture. Summary of the invention
[0010] The object of the present invention is to solve the above problems existing in the prior art and to provide a super hygroscopic polyethylene terephthalate film and a preparation method thereof.
[0011] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0012] A method for preparing a super hygroscopic polyethylene terephthalate film comprises the steps of cross-linking carboxymethyl cellulose and ethylene glycol diglycidyl ether under alkaline conditions to form a gel, then placing the gel in water to swell, breaking it, coating it on a polyethylene terephthalate film, and drying it to obtain the super hygroscopic polyethylene terephthalate film.
[0013] The principle that the super hygroscopic polyethylene terephthalate film provided by the present invention can repeatedly absorb moisture is as follows:
[0014] The gel used in the present invention contains a large number of hydroxyl and carboxyl groups. Since the carboxyl and hydroxyl groups are hydrophilic, the gel does not reduce the content of the hydrophilic carboxyl and hydroxyl groups after repeated moisture absorption, and still has a high moisture absorption capacity after repeated moisture absorption;
[0015] The gel used in the present invention forms hydrogen bonds with polar groups (such as carbonyl and hydroxyl) on the surface of the polyethylene terephthalate film through hydroxyl and carboxyl groups. The polyethylene terephthalate film and the gel have high bonding strength, and the gel will not fall off after repeated use.
[0016] The present invention prepares gel first and then coats it on a polyethylene terephthalate film. Before coating, the residual sodium ions or potassium ions (sodium ions or potassium ions are introduced when forming alkaline conditions) and a cross-linking agent (ethylene glycol diglycidyl ether) in the gel are removed by swelling, so that the gel exposes more carboxyl groups to form hydrogen bonds with polar groups on the surface of the polyethylene terephthalate film. In addition, the residual cross-linking agent will also block the contact between the gel and the polyethylene terephthalate film, reducing the contact area. Therefore, preparing the gel first and then coating it is beneficial to improve the bonding strength between the gel and the polyethylene terephthalate film, thereby making the super hygroscopic polyethylene terephthalate film have excellent hygroscopicity and reusability.
[0017] As the preferred technical solution:
[0018] In the method for preparing a super hygroscopic polyethylene terephthalate film as described above, the weight ratio of carboxymethyl cellulose to ethylene glycol diglycidyl ether is 1:2.5-1:6.25, the temperature of the cross-linking reaction is 40-70° C., and the time of the cross-linking reaction is 1-4 hours.
[0019] In the method for preparing a super hygroscopic polyethylene terephthalate film as described above, the weight ratio of gel to water is 1:300-1:500, and the swelling temperature is 20-30°C.
[0020] The method for preparing a super hygroscopic polyethylene terephthalate film as described above, wherein the coating position is one side or both sides of the polyethylene terephthalate film, and the coating amount of the gel on one side of the polyethylene terephthalate film is 6-12 g / cm 2 .
[0021] The method for preparing the super hygroscopic polyethylene terephthalate film as described above comprises the following specific steps:
[0022] (1) dissolving carboxymethyl cellulose in an alkaline solution to obtain a carboxymethyl cellulose solution, adding ethylene glycol diglycidyl ether to the carboxymethyl cellulose solution, stirring evenly to obtain a mixed solution with a pH value greater than 7, and subjecting the mixed solution to a cross-linking reaction to obtain a gel;
[0023] (2) Cut the gel into blocks, place them in water to swell, and change the water and repeat the swelling process for more than one time in order to completely remove the unreacted residual substances. Use a wall breaker to break up the blocks, apply them on the surface of a polyethylene terephthalate film, and use an oven to dry them to obtain a super hygroscopic polyethylene terephthalate film.
[0024] In the method for preparing a super hygroscopic polyethylene terephthalate film as described above, in step (1), the weight ratio of carboxymethyl cellulose to alkaline solution is 1:50-1:70, the alkaline solution is a NaOH or KOH aqueous solution, and the concentration of NaOH or KOH in the alkaline solution is 0.2-0.5 mol / L.
[0025] In the method for preparing a super hygroscopic polyethylene terephthalate film as described above, in step (1), the stirring speed is 300-500 rpm and the stirring time is 10-20 min.
[0026] In the method for preparing a super hygroscopic polyethylene terephthalate film as described above, in step (1), after stirring evenly, the mixed solution is placed under vacuum conditions and allowed to stand for 5-15 minutes to remove residual bubbles before performing a cross-linking reaction.
[0027] In the method for preparing a super hygroscopic polyethylene terephthalate film as described above, in step (2), the number of times the water is changed and the swelling is repeated is 2-5, and the time for a single swelling is 24-48 hours.
[0028] The present invention also provides a super hygroscopic polyethylene terephthalate film prepared by the preparation method as described in any one of the above items, the water retention rate of the obtained super hygroscopic polyethylene terephthalate film is 81-86%, and the swelling degree after repeated moisture absorption for 5-8 times is 20-30g / g; the biodegradability of the gel on the surface of the super hygroscopic polyethylene terephthalate film is 100%, and since carboxymethyl cellulose has excellent biodegradability, the gel of the present invention has excellent biodegradability.
[0029] Beneficial effects:
[0030] (1) The gel used in the present invention contains a large number of hydroxyl and carboxyl groups. Since carboxyl and hydroxyl groups are hydrophilic, the content of hydrophilic carboxyl and hydroxyl groups will not decrease after repeated moisture absorption, and the gel still has a high moisture absorption capacity.
[0031] (2) The gel used in the present invention can form hydrogen bonds with polar groups (such as carbonyl and hydroxyl) on the surface of the polyethylene terephthalate film through hydroxyl and carboxyl groups, making the gel and the polyethylene terephthalate film more compatible and enhancing the bonding strength between the two. After repeated use, the gel will not fall off.
[0032] (3) The super hygroscopic polyethylene terephthalate film prepared by the present invention has a swelling degree of 20-30 g / g after repeated moisture absorption for 5-8 times, and has excellent repeated moisture absorption performance.
[0033] (4) The carboxymethyl cellulose used in the present invention has excellent biodegradability, and the biodegradability of the gel on the surface of the super hygroscopic polyethylene terephthalate film is 100%, which has little pollution to the environment.
[0034] (5) The raw materials used in the present invention are easily available, low in cost, and prepared under mild conditions, and are suitable for large-scale applications. DETAILED DESCRIPTION
[0035] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0036] The following are the test methods for the relevant performance indicators in each embodiment and comparative example:
[0037] (1) Swelling test after repeated moisture absorption:
[0038] A certain amount of dry hygroscopic or super hygroscopic polyethylene terephthalate film is weighed and placed in a constant temperature and humidity chamber at 25°C and 50%RH to allow it to reach hygroscopic equilibrium. The film is then taken out and weighed, and the swelling degree is calculated according to formula (1). The hygroscopic or super hygroscopic polyethylene terephthalate film after hygroscopic equilibrium is placed in a 60°C oven for drying, and then placed back in the constant temperature and humidity chamber for hygroscopic swelling, and the swelling degree is tested for the second time. The above operation is repeated until the required number of repeated hygroscopic absorptions is reached.
[0039] (1);
[0040] Where W o is the weight of dry hygroscopic or superhygroscopic polyethylene terephthalate film, in grams; W t is the weight of the hygroscopic or super hygroscopic polyethylene terephthalate film swollen to time t, in g.
[0041] (2) Water retention test:
[0042] A certain amount of hygroscopic or super hygroscopic polyethylene terephthalate film after moisture absorption and saturation was weighed, placed on a flat glass, and left to stand at 25°C for 96 hours. The weight of the hygroscopic or super hygroscopic polyethylene terephthalate film was measured, and the water retention rate was calculated according to formula (2).
[0043] (2);
[0044] Where W oW is the weight of the hygroscopic or super hygroscopic polyethylene terephthalate film after initial water saturation, in g; t It is the weight of the hygroscopic or super hygroscopic polyethylene terephthalate film when left at 25°C for 96 hours, in grams.
[0045] (3) Biodegradation rate test of gel on the surface of super hygroscopic polyethylene terephthalate film:
[0046] The super hygroscopic polyethylene terephthalate film was cut into square pieces of 5 cm × 5 cm and buried vertically in the soil at a depth of 20 cm. The day of burial in the soil was the first day. On the 30th day, the sample was taken out, the surface soil was removed, and it was dried and weighed. The biodegradation rate of the gel on the surface of the super hygroscopic polyethylene terephthalate film was calculated according to formula (3).
[0047] R (3);
[0048] Where W o is the dry weight of the initial super hygroscopic polyethylene terephthalate film, in g; W f W is the dry weight of a 5 cm × 5 cm polyethylene terephthalate film without gel coating, in g; t It is the dry weight of the super hygroscopic polyethylene terephthalate film at the 30th day, in g.
[0049] Example 1
[0050] A method for preparing a super hygroscopic polyethylene terephthalate film, the specific steps are as follows:
[0051] (1) Preparation of raw materials;
[0052] Carboxymethyl cellulose: CAS No. 9000-11-7;
[0053] Ethylene glycol diglycidyl ether: CAS No. 2224-15-9;
[0054] Polyethylene terephthalate film: 297 mm long, 210 mm wide, 12 μm thick;
[0055] Alkaline solution: NaOH aqueous solution, concentration 0.2 mol / L;
[0056] water;
[0057] (2) preparing gel;
[0058] adding carboxymethyl cellulose into an alkaline solution for dissolution, wherein the weight ratio of carboxymethyl cellulose to the alkaline solution is 1:60, to obtain a carboxymethyl cellulose solution; adding ethylene glycol diglycidyl ether into the carboxymethyl cellulose solution, wherein the weight ratio of carboxymethyl cellulose to ethylene glycol diglycidyl ether is 1:6.25; stirring at 300 rpm for 10 min to obtain a mixed solution with a pH value > 7; allowing the mixed solution to stand for 5 min under a vacuum degree <100 Pa; and then placing the mixed solution in a 40° C. thermostat for a cross-linking reaction for 1 h to obtain a gel;
[0059] (3) coating gel;
[0060] The gel obtained in step (2) is placed in water with a weight ratio of gel to water of 1:300, and swelled for 36 hours at 20°C, and the water is changed and the swelling is repeated twice. When changing the water, the original water is first siphoned off and then new water is added. The temperature, time and amount of water added for each repeated swelling are the same as those for the previous swelling. The swollen gel is then broken up with a wall breaking machine and coated on one side of a polyethylene terephthalate film. The coating amount of the gel on one side of the polyethylene terephthalate film is 6 g / cm 2 , and placed in an oven at 60°C for drying to obtain a super hygroscopic polyethylene terephthalate film.
[0061] The water retention rate of the finally prepared super hygroscopic polyethylene terephthalate film is 81%, and the swelling degree after repeated moisture absorption for 5 times is 20g / g; the biodegradation rate of the gel on the surface of the super hygroscopic polyethylene terephthalate film is 100%.
[0062] Comparative Example 1
[0063] A method for preparing a hygroscopic polyethylene terephthalate film is basically the same as that in Example 1, except that: there is no step (3); in step (2), the mixed solution is allowed to stand and then directly coated on one side of the polyethylene terephthalate film; after coating, the mixed solution is placed in a 40°C constant temperature box for a cross-linking reaction for 1 hour to form a gel on the polyethylene terephthalate film; the mixed solution is placed in a 60°C oven for drying; and the coating amount is controlled so that the thickness of the gel on the polyethylene terephthalate film is the same as that in Example 1.
[0064] The water retention rate of the finally prepared hygroscopic polyethylene terephthalate film was 45%, and the swelling degree after repeated moisture absorption for three times was 16 g / g.
[0065] Compared with Example 1, the swelling performance of the hygroscopic polyethylene terephthalate film obtained in Comparative Example 1 is significantly reduced. This is because, on the one hand, the preparation of the gel in Example 1 and then the coating is beneficial to improving the bonding strength between the gel and the polyethylene terephthalate film, thereby making the super hygroscopic polyethylene terephthalate film have excellent hygroscopic reusability. The bonding method of the gel and the polyethylene terephthalate film in Comparative Example 1 makes the bonding strength between the gel and the polyethylene terephthalate film relatively low. On the other hand, Example 1 performs a swelling treatment on the gel, while Comparative Example 1 does not perform a swelling treatment on the gel. The unswollen gel contains a large amount of sodium ions. Excessive sodium ions will combine with the negatively charged carboxyl functional groups in the gel to play a charge shielding role, inhibiting the electrostatic repulsion between the carboxyl anions, which is not conducive to the stretching of the polymer network, resulting in a decrease in the swelling degree of the gel. The combination of excessive sodium ions with the carboxyl functional groups also reduces the active sites of the gel for adsorbing water molecules, reducing the water locking ability, and thus reducing the water retention rate.
[0066] Comparative Example 2
[0067] A method for preparing a hygroscopic polyethylene terephthalate film is basically the same as that of comparative example 1, except that: after forming a gel on the polyethylene terephthalate film and before placing it in a 60°C oven for drying, the polyethylene terephthalate film with the gel loaded on the surface is placed in water, the weight ratio of the gel to the water is 1:300, and it is swollen for 36 hours at 20°C, and the water is changed and the swelling is repeated twice. When changing the water, the original water is first siphoned off and then new water is added. The temperature, time and amount of water added for each repeated swelling are the same as those of the previous swelling.
[0068] The water retention rate of the finally prepared hygroscopic polyethylene terephthalate film was 32%, and the swelling degree after repeated moisture absorption for three times was 7 g / g.
[0069] Compared with Example 1, the water retention rate and swelling degree after repeated moisture absorption for three times of Comparative Example 2 are both reduced. This is because, on the one hand, the preparation of the gel before coating in Example 1 is conducive to improving the bonding strength between the gel and the polyethylene terephthalate film, thereby making the super hygroscopic polyethylene terephthalate film have excellent moisture absorption and reusability. The bonding method of the gel and the polyethylene terephthalate film in Comparative Example 2 makes the bonding strength between the gel and the polyethylene terephthalate film relatively low. On the other hand, the gel in Comparative Example 2 is bonded to the polyethylene terephthalate film. During the formation process on the polyethylene terephthalate film, a large number of sodium ions in the reaction system combine with carboxyl anions, occupying the position of forming hydrogen bonds with the polar groups on the surface of the polyethylene terephthalate film, resulting in poor bonding strength between the formed gel and the polyethylene terephthalate film. In addition, the cross-linking agent in the reaction system will also hinder the contact between the gel and the polyethylene terephthalate film. After multiple swelling and water washing, the gel that originally had poor bonding with the polyethylene terephthalate film will be washed away, resulting in a decrease in water retention rate and swelling degree after repeated moisture absorption.
[0070] Example 2
[0071] A method for preparing a super hygroscopic polyethylene terephthalate film, the specific steps are as follows:
[0072] (1) Preparation of raw materials;
[0073] Carboxymethyl cellulose: CAS No. 9000-11-7;
[0074] Ethylene glycol diglycidyl ether: CAS No. 2224-15-9;
[0075] Polyethylene terephthalate film: 297 mm long, 210 mm wide, 12 μm thick;
[0076] Alkaline solution: KOH aqueous solution, concentration 0.3 mol / L;
[0077] water;
[0078] (2) preparing gel;
[0079] Add carboxymethyl cellulose into an alkaline solution for dissolution, the weight ratio of carboxymethyl cellulose to the alkaline solution is 1:70, to obtain a carboxymethyl cellulose solution, add ethylene glycol diglycidyl ether into the carboxymethyl cellulose solution, the weight ratio of carboxymethyl cellulose to ethylene glycol diglycidyl ether is 1:6.25, stir at 400 rpm for 15 minutes, obtain a mixed solution with a pH value>7, let the mixed solution stand for 10 minutes under a vacuum degree of <100 Pa, and then place the mixed solution in a 50° C. thermostat for a cross-linking reaction for 2 hours to obtain a gel;
[0080] (3) coating gel;
[0081] The gel obtained in step (2) is placed in water with a weight ratio of gel to water of 1:400, and swelled at 25°C for 24 hours, and the water is changed and the swelling is repeated three times. When changing the water, the original water is first siphoned off and then new water is added. The temperature, time and amount of water added for each repeated swelling are the same as those of the previous swelling. The swollen gel is then broken up with a wall breaking machine and coated on both sides of a polyethylene terephthalate film. The amount of gel coated on one side of the polyethylene terephthalate film is 10 g / cm 2 , and placed in an oven at 60°C for drying to obtain a super hygroscopic polyethylene terephthalate film.
[0082] The water retention rate of the finally prepared super hygroscopic polyethylene terephthalate film is 84%, and the swelling degree after repeated moisture absorption for 6 times is 26g / g; the biodegradation rate of the gel on the surface of the super hygroscopic polyethylene terephthalate film is 100%.
[0083] Example 3
[0084] A method for preparing a super hygroscopic polyethylene terephthalate film, the specific steps are as follows:
[0085] (1) Preparation of raw materials;
[0086] Carboxymethyl cellulose: CAS No. 9000-11-7;
[0087] Ethylene glycol diglycidyl ether: CAS No. 2224-15-9;
[0088] Polyethylene terephthalate film: 297 mm long, 210 mm wide, 12 μm thick;
[0089] Alkaline solution: NaOH aqueous solution, concentration 0.5 mol / L;
[0090] water;
[0091] (2) preparing gel;
[0092] Add carboxymethyl cellulose into an alkaline solution for dissolution, the weight ratio of carboxymethyl cellulose to the alkaline solution being 1:50, to obtain a carboxymethyl cellulose solution, add ethylene glycol diglycidyl ether into the carboxymethyl cellulose solution, the weight ratio of carboxymethyl cellulose to ethylene glycol diglycidyl ether being 1:2.5, stir at 500 rpm for 20 min, to obtain a mixed solution with a pH value > 7, let the mixed solution stand for 15 min under a vacuum degree <100 Pa, and then place the mixed solution in a 70° C. thermostat for a cross-linking reaction for 4 h to obtain a gel;
[0093] (3) coating gel;
[0094] The gel obtained in step (2) is placed in water with a weight ratio of gel to water of 1:500, and swelled at 30°C for 48 hours, and the water is changed and the swelling is repeated 4 times. When changing the water, the original water is first siphoned off and then new water is added. The temperature, time and amount of water added for each repeated swelling are the same as those of the previous swelling. The swollen gel is then broken up with a wall breaking machine and coated on both sides of a polyethylene terephthalate film. The coating amount of the gel on one side of the polyethylene terephthalate film is 12 g / cm 2 , and placed in an oven at 60°C for drying to obtain a super hygroscopic polyethylene terephthalate film.
[0095] The water retention rate of the finally prepared super hygroscopic polyethylene terephthalate film is 86%, and the swelling degree after repeated moisture absorption for 7 times is 28g / g; the biodegradation rate of the gel on the surface of the super hygroscopic polyethylene terephthalate film is 100%.
[0096] Example 4
[0097] A method for preparing a super hygroscopic polyethylene terephthalate film, the specific steps are as follows:
[0098] (1) Preparation of raw materials;
[0099] Carboxymethyl cellulose: CAS No. 9000-11-7;
[0100] Ethylene glycol diglycidyl ether: CAS No. 2224-15-9;
[0101] Polyethylene terephthalate film: 297 mm long, 210 mm wide, 12 μm thick;
[0102] Alkaline solution: NaOH aqueous solution, concentration 0.2 mol / L;
[0103] water;
[0104] (2) preparing gel;
[0105] Add carboxymethyl cellulose into an alkaline solution for dissolution, the weight ratio of carboxymethyl cellulose to the alkaline solution is 1:50, to obtain a carboxymethyl cellulose solution, add ethylene glycol diglycidyl ether into the carboxymethyl cellulose solution, the weight ratio of carboxymethyl cellulose to ethylene glycol diglycidyl ether is 1:3.75, stir at 500 rpm for 20 minutes, obtain a mixed solution with a pH value>7, let the mixed solution stand for 10 minutes under a vacuum degree of <100 Pa, and then place the mixed solution in a 60°C thermostat for a cross-linking reaction for 2 hours to obtain a gel;
[0106] (3) coating gel;
[0107] The gel obtained in step (2) is placed in water with a weight ratio of gel to water of 1:500, and swelled for 36 hours at 25°C, and the water is changed and the swelling is repeated 5 times. When changing the water, the original water is first siphoned off and then new water is added. The temperature, time and amount of water added for each repeated swelling are the same as those of the previous swelling. The swollen gel is then broken up with a wall breaking machine and coated on one side of a polyethylene terephthalate film. The coating amount of the gel on one side of the polyethylene terephthalate film is 12 g / cm 2 , and placed in an oven at 60°C for drying to obtain a super hygroscopic polyethylene terephthalate film.
[0108] The water retention rate of the finally prepared super hygroscopic polyethylene terephthalate film is 86%, and the swelling degree after repeated moisture absorption for 8 times is 30g / g; the biodegradation rate of the gel on the surface of the super hygroscopic polyethylene terephthalate film is 100%.
Claims
1. A method for preparing a super hygroscopic polyethylene terephthalate film, characterized in that: Carboxymethyl cellulose and ethylene glycol diglycidyl ether are cross-linked under alkaline conditions to form a gel, which is then placed in water to swell, broken, coated on a polyethylene terephthalate film, and dried to obtain a super hygroscopic polyethylene terephthalate film; the water retention rate of the super hygroscopic polyethylene terephthalate film is 81-86%, and the swelling degree after repeated moisture absorption for 5-8 times is 20-30g / g; the biodegradability of the gel on the surface of the super hygroscopic polyethylene terephthalate film is 100%.
2. The method for preparing a super hygroscopic polyethylene terephthalate film according to claim 1, characterized in that: The weight ratio of carboxymethyl cellulose to ethylene glycol diglycidyl ether is 1:2.5-1:6.25, the temperature of the cross-linking reaction is 40-70° C., and the time of the cross-linking reaction is 1-4 hours.
3. The method for preparing a super hygroscopic polyethylene terephthalate film according to claim 1, characterized in that: The weight ratio of gel to water is 1:300-1:500, and the swelling temperature is 20-30°C.
4. The method for preparing a super hygroscopic polyethylene terephthalate film according to claim 1, characterized in that: The coating position is one side or both sides of the polyethylene terephthalate film, and the coating amount of the gel on one side of the polyethylene terephthalate film is 6-12g / cm 2 .
5. The method for preparing a super hygroscopic polyethylene terephthalate film according to any one of claims 1 to 4, characterized in that: The specific steps are as follows: (1) dissolving carboxymethyl cellulose in an alkaline solution to obtain a carboxymethyl cellulose solution, adding ethylene glycol diglycidyl ether to the carboxymethyl cellulose solution, stirring evenly to obtain a mixed solution with a pH value greater than 7, and subjecting the mixed solution to a cross-linking reaction to obtain a gel; (2) Cut the gel into blocks, place them in water to swell, change the water and repeat the swelling process for more than one time, break them up with a wall breaker, apply them on the surface of a polyethylene terephthalate film, and dry them in an oven to obtain a super hygroscopic polyethylene terephthalate film.
6. The method for preparing a super hygroscopic polyethylene terephthalate film according to claim 5, characterized in that: In step (1), the weight ratio of carboxymethyl cellulose to alkaline solution is 1:50-1:70, the alkaline solution is a NaOH or KOH aqueous solution, and the concentration of NaOH or KOH in the alkaline solution is 0.2-0.5 mol / L.
7. The method for preparing a super hygroscopic polyethylene terephthalate film according to claim 5, characterized in that: In step (1), the stirring speed is 300-500 rpm, and the stirring time is 10-20 min.
8. The method for preparing a super hygroscopic polyethylene terephthalate film according to claim 5, characterized in that: In step (1), after being stirred evenly, the mixed solution is placed under vacuum conditions and allowed to stand for 5-15 minutes before undergoing a cross-linking reaction.
9. The method for preparing a super hygroscopic polyethylene terephthalate film according to claim 5, characterized in that: In step (2), the water is changed and the swelling is repeated 2-5 times, and the time for a single swelling is 24-48 hours.
Citation Information
Patent Citations
Process and device for treatment of water from a biodegradeable process
CA2224159A1
Preparation method of moisture absorption packaging film
CN102838769A
Method for preparing composite type moisture absorption film
CN103194000A
Crosslinked carboxymethyl cellulose superabsorbent gel for sanitary napkins and preparation method of crosslinked carboxymethyl cellulose superabsorbent gel
CN117164894A
Fine gel particle of water-absorbing resin, and coated film and laminated product made from the same
JP2009091499A