Environmentally friendly nano-enhancer for high temperature resistant water-based coating, water-based coating and application thereof

By using modified carbon nanotubes, hollow ceramic beads and graphene oxide nano-enhancers in water-based coatings, the problem of insufficient high temperature resistance, salt spray resistance and water immersion resistance of air compressor air compression components at high temperatures is solved. The overall performance improvement and stability of the coating are improved.

CN118374180BActive Publication Date: 2024-10-25TIANJIN ZIMING COATINGS MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410611026.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-14
Publication Date
2024-10-25
Estimated Expiration
2044-05-14

AI Technical Summary

Technical Problem

Existing coatings used for air compression parts of air compressors are difficult to meet the comprehensive performance requirements of high temperature resistance, salt spray resistance and water immersion resistance under high temperature conditions, and the enhancement effect on high temperature resistance performance of commercially available enhancers is not obvious.

Method used

Environmentally friendly nano-enhancers are used, including modified carbon nanotubes, modified hollow ceramic beads and modified graphene oxide, and modified by silane coupling agents and water-soluble phenolic resins to form composite materials for the preparation of water-based coatings. Improve its high temperature resistance, salt spray resistance and water immersion resistance.

Benefits of technology

Significantly improves the high temperature resistance of water-based coatings, enhances its stability and thermal conductivity at high temperatures, improves salt spray resistance and wear resistance, ensures the adhesion and durability of the coating, and is suitable for spray air pressure Air compression components of the machine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004843653640000121
    Figure BDA0004843653640000121
  • Figure BDA0004843653640000131
    Figure BDA0004843653640000131
  • Figure BDA0004843653640000132
    Figure BDA0004843653640000132
Patent Text Reader

Abstract

The present invention provides an environmentally friendly high temperature resistant water-based coating nano-enhancer, a water-based coating and an application, and belongs to the technical field of coatings. The environmentally friendly high temperature resistant water-based coating nano-enhancer includes the following components by mass fraction: 3-8 parts of modified carbon nanotubes, 4-7 parts of modified hollow ceramic microbeads, 2-6 parts of modified graphene oxide and 30-40 parts of deionized water. The present invention, by compounding modified carbon nanotubes, modified hollow ceramic microbeads and graphene oxide, the three work together to achieve the improvement of multi-dimensional effects, can complement each other, form a multi-efficiency composite system, and synergistically improve the overall performance of water-based coatings, so that it can achieve better effects in terms of high temperature resistance, salt spray resistance, wear resistance, adhesion, etc. After compounding, it can better form a firm interface with the remaining components of water-based coatings such as water-based epoxy resins, and improve the stability and durability of water-based coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a nano-enhancer for an environmentally friendly high-temperature resistant water-based coating, a water-based coating and applications. Background Art

[0002] An air compressor is a mechanical device used to compress gas and increase gas pressure. It is widely used in many scenarios in industrial production and daily life. The air compression components of the air compressor do generate a lot of heat during operation, because the work done when compressing the air causes the gas temperature to rise. The air compression components of the air compressor will work under high temperature conditions, up to 250°C. If these high-temperature components do not take appropriate protective measures, their normal working life and efficiency may be affected due to high-temperature oxidation, corrosion, fatigue failure and other problems. Selecting suitable high-temperature paint to spray on the air compression components of the air compressor is one of the important means of effectively maintaining and servicing the equipment.

[0003] At present, most of the coatings for high-pressure machines on the market have a continuous maximum temperature limit of less than 250°C. Some can meet the temperature requirements, but cannot meet customer requirements in terms of salt spray resistance, water immersion resistance, etc. Therefore, there is an urgent need for a water-based coating with superior comprehensive performance for spraying air compressor parts.

[0004] Enhancer is an important auxiliary agent in the preparation process of water-based coatings. The enhancers on the market are mainly used for thickening, leveling, anti-corrosion, defoaming and other functions, and have no obvious effect on the high temperature resistance of water-based coatings. Summary of the invention

[0005] The purpose of the present invention is to provide an environmentally friendly nano-enhancer for high-temperature resistant water-based coatings, water-based coatings and applications. The nano-enhancer helps to improve the high-temperature resistance of the water-based coatings, while the salt spray resistance and water immersion resistance of the water-based coatings are improved. The water-based coatings prepared by the present invention have high storage stability.

[0006] In order to achieve the above-mentioned object, the present invention provides the following technical scheme: an environmentally friendly nano-enhancer for high temperature resistant water-based coatings, comprising the following components in parts by weight: 3-8 parts of modified carbon nanotubes, 4-7 parts of modified hollow ceramic microbeads, 2-6 parts of modified graphene oxide and 30-40 parts of deionized water;

[0007] The preparation method of the modified carbon nanotubes is as follows: 0.02-0.04 parts by mass of silane coupling agent KH560 and 1 part by mass of carbon nanotubes are added to 6-9 parts by mass of propanol, stirred at 40-45° C. for 80-100 minutes, 0.03-0.06 parts by mass of phenolic resin are added, stirred evenly, the solvent is removed, the reaction is carried out at 110-120° C. for 100-120 minutes, and the modified carbon nanotubes are obtained;

[0008] The phenolic resin has a brand name of Allnex and a model number of VPW1946 46WA. This model of phenolic resin is a water-dilutable phenolic resin.

[0009] The preparation method of the modified hollow ceramic microspheres is as follows: 1 mass part of hollow ceramic microspheres, 0.02-0.04 mass parts of silane coupling agent KH550 and 5-7 mass parts of ethanol aqueous solution with a mass fraction of 50-55% are mixed, the temperature is raised to 50-55° C. for reaction for 1-2 hours, 0.04-0.06 mass parts of polyvinyl alcohol are continuously added, the temperature is 40-45° C. for reaction for 30-50 minutes, and the modified hollow ceramic microspheres are filtered and dried to obtain the modified hollow ceramic microspheres.

[0010] Furthermore, the weight average molecular weight of the polyvinyl alcohol is 9000-10000. Merck, catalog number: 360627.

[0011] The preparation method of the modified graphene oxide is:

[0012] (1) mixing 1 part by mass of silicon nitride, 2-4 parts by mass of graphene oxide and 7-10 parts by mass of deionized water, stirring and mixing evenly to obtain a mixed solution;

[0013] (2) 12 parts by mass of the mixed solution are sprayed into liquid nitrogen in which 3-5 parts by mass of GeSbTe phase change powder is dispersed, frozen into microspheres, and dried to obtain modified graphene oxide.

[0014] Furthermore, the carbon nanotubes are a mixture of double-walled carbon nanotubes, single-walled carbon nanotubes and multi-walled carbon nanotubes in a mass ratio of 1:(2-3):(0.3-0.7); the double-walled carbon nanotubes have a diameter of 2-4 nm, a length of 40-60 μm, and a specific surface area of ​​400-600 m 2 / g; the diameter of single-walled carbon nanotubes is 1-2nm, the length is 5-30μm, and the specific surface area is 800-1200m 2 / g; the diameter of multi-walled carbon nanotubes is 5-15nm, the length is 0.5-2μm, and the specific surface area is 50-80m 2 / g.

[0015] Furthermore, the chemical composition percentage of the hollow ceramic microspheres is: 55-60% silicon dioxide, 36-40% aluminum oxide, 0.4-0.5% iron oxide, 1.4-1.6% titanium dioxide; the particle size is 20-500 μm. Produced by Dalian Yibang Technology Co., Ltd., model: E-SPHERES hollow ceramic microspheres.

[0016] Furthermore, the mass ratio of Ge, Sb and Te in the GeSbTe phase change powder is (1.4-1.7):1:(0.3-0.8).

[0017] Furthermore, the nozzle hole used in the spray method has a diameter size of 0.2 mm to 0.4 mm.

[0018] Furthermore, the graphene oxide has a particle size of 0.5-3 μm and a layer number of 1-5. Produced by Beijing Dekedaojin Technology Co., Ltd.

[0019] Furthermore, the particle size of silicon nitride is 20-50 nm. Produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0020] Furthermore, the preparation method of the environmentally friendly high temperature resistant water-based coating nano-enhancer is as follows: modified carbon nanotubes, modified hollow ceramic microbeads, modified graphene oxide and deionized water are mixed to obtain the nano-enhancer.

[0021] The second aspect of the present invention provides a water-based coating prepared using a nano-enhancer, comprising the following components in mass fractions: 45-50 parts of a water-based epoxy resin, 25-30 parts of a nano-enhancer, 2-4 parts of a curing agent, 2-3 parts of a defoaming agent, 1-2 parts of a leveling agent, 2-4 parts of a dispersant, 1-2 parts of an anti-settling agent, and 11-13 parts of deionized water.

[0022] Furthermore, the waterborne epoxy resin is a waterborne epoxy resin EP137 produced by Guangdong Qirun New Materials Co., Ltd. and Huntsman Compound of PZ 756-1 / 67 epoxy resin and Hexion Epikote 828 epoxy resin.

[0023] Furthermore, the curing agent is produced by Suzhou Meiguowang Flooring Materials Co., Ltd., model: water-based epoxy curing agent WG802.

[0024] Furthermore, the dispersant is German BYK-190 wetting dispersant.

[0025] Furthermore, the defoamer is German BYK defoamer BYK028.

[0026] Furthermore, the anti-settling agent is Evonik Degussa AEROSIL R972.

[0027] Furthermore, the preparation method of the water-based paint is: uniformly mixing and stirring the components of the water-based paint in proportion to obtain the water-based paint.

[0028] It should be noted that the nano-enhancer of the present invention is not limited to the water-based coating provided by the present invention, but can also be used in other water-based coatings.

[0029] A third aspect of the present invention provides an application of a water-based paint, wherein the water-based paint is used for spraying air compression components of an air compressor.

[0030] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0031] 1. The present invention adds modified carbon nanotubes to nano-enhancers, so that the nano-enhancers can improve the high temperature resistance of water-based coatings. The compounded carbon nanotubes are modified with silane coupling agents and water-soluble phenolic resins, and have better compatibility with water-based coating systems, and have extremely high thermal stability and thermal conductivity, which can effectively transfer the heat on the coating surface to the inside of the substrate quickly to prevent local overheating, thereby improving the temperature resistance limit of the coating; three different carbon nanotubes are compounded, and carbon nanotubes of various sizes and structures are mixed together to form a mutually supporting network structure, which jointly bears stress when heated, improves the stability and thermal stability of the overall structure, and helps prevent the coating from cracking or peeling at high temperatures; carbon nanotubes of different particle sizes can provide reinforcement effects of different scales, forming a denser filling structure, improving the density and heat conductivity resistance of the coating, optimizing the matching of thermal expansion coefficients, and reducing thermal stress; the composite structure increases the complexity of the heat diffusion path, and heat energy needs to bypass carbon nanotubes of various shapes and arrangements when passing through the coating, thereby enhancing the thermal insulation effect of the coating. In addition, different types of carbon nanotubes have different advantages. When used in combination, they can not only improve the heat resistance of the coating, but also improve the wear resistance, adhesion and salt spray resistance of the coating. The present invention can maximize the advantages of each by rationally designing and compounding different types of carbon nanotubes to form a composite material system with more comprehensive and balanced performance, thereby improving the high temperature resistance of the water-based coating.

[0032] 2. The present invention adds modified hollow ceramic microspheres to the nano-enhancer, which helps to improve the high temperature resistance of water-based coatings. Hollow ceramic microspheres have high high temperature resistance, which helps to improve the upper temperature resistance limit of the entire coating system. Their specific chemical composition helps to improve the high temperature resistance of water-based coatings. At the same time, through the modification of silane coupling agents and polyvinyl alcohol, the dispersibility in water-based coatings is improved. The modified hollow ceramic microspheres are easier to disperse evenly in the water-based epoxy resin system to form a stable suspension system, avoiding the local thermal stress concentration caused by the aggregation of microspheres. At the same time, the combination of hollow ceramic microspheres and water-based epoxy resins is strengthened, and the microstructure of the coating is optimized, thereby improving the high temperature resistance of the coating from multiple angles.

[0033] 3. The present invention adds modified graphene oxide to improve the high temperature resistance of water-based coatings. Silicon nitride is inserted between graphene oxide sheets to synergistically improve the high temperature resistance of water-based coatings. The GeSbTe (GST) phase change material composed of a specific ratio can be reversibly converted between crystals and amorphous states, and exhibits significant changes in thermal properties during the phase change process. When undergoing phase change, it absorbs and releases a large amount of heat. This characteristic helps to regulate temperature fluctuations on the surface of graphene oxide and plays a role similar to thermal buffering, especially in environments with rapid heating or cooling. Graphene oxide has a high specific surface area and good thermal conductivity, and the spray deposition of GeSbTe may form an effective thermal interface layer to improve the thermal conduction efficiency between the two. When GeSbTe is combined with graphene oxide to form a composite material, the synergistic effect of the two may enhance the thermal stability of the overall material.

[0034] 4. The present invention can achieve the improvement of multi-dimensional effects by compounding modified carbon nanotubes, modified hollow ceramic microbeads, and graphene oxide. The three can complement each other to form a multi-efficiency composite system, and synergistically improve the overall performance of water-based coatings, so that it can achieve better effects in terms of high temperature resistance, salt spray resistance, and wear resistance. The water-based coating with nano additives has excellent adhesion on cast iron and stainless steel, and is more effective as an air compression component of a spray air compressor. The nano-enhancer of the present invention can better form a firm interface with the remaining components of the water-based coating, such as water-based epoxy resin, after compounding, and improve the stability and durability of the water-based coating. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] This embodiment provides an environmentally friendly nano-enhancer for high temperature resistant water-based coatings, comprising the following components in parts by weight: 6 parts of modified carbon nanotubes, 5 parts of modified hollow ceramic microspheres, 4 parts of modified graphene oxide, and 35 parts of deionized water.

[0038] The preparation method of the modified carbon nanotubes is as follows: 0.03 parts by mass of silane coupling agent KH560 and 1 part by mass of carbon nanotubes are added to 7 parts by mass of propanol, stirred at 42°C for 90 minutes, 0.05 parts by mass of phenolic resin are added, stirred evenly and then the solvent is removed, reacted at 115°C for 110 minutes, and cooled to room temperature to obtain the modified carbon nanotubes;

[0039] The carbon nanotubes are a mixture of double-walled carbon nanotubes, single-walled carbon nanotubes and multi-walled carbon nanotubes in a mass ratio of 1:2.6:0.5; the double-walled carbon nanotubes have a diameter of 2-4 nm, a length of 40-60 μm, and a specific surface area of ​​400-600 m 2 / g; diameter of single-walled carbon nanotubes: 1-2nm, length: 5-30μm, specific surface area 800-1200m 2 / g; diameter of multi-walled carbon nanotubes: 5-15nm, length: 0.5-2μm, specific surface area: 50-80m 2 / g, produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0040] The phenolic resin has a brand name of Allnex and a model number of VPW1946 46WA. This model of phenolic resin is a water-dilutable phenolic resin.

[0041] The preparation method of the modified hollow ceramic microspheres is as follows: 1 mass part of hollow ceramic microspheres, 0.03 mass parts of silane coupling agent KH550 and 6 mass parts of 53% ethanol aqueous solution are mixed, the temperature is raised to 53° C. for reaction for 1.4 hours, 0.05 mass parts of polyvinyl alcohol are continuously added, the temperature is 42° C. for reaction for 40 minutes, and the modified hollow ceramic microspheres are filtered and dried to obtain the modified hollow ceramic microspheres.

[0042] The chemical composition percentage of hollow ceramic microspheres is: 55-60% silicon dioxide, 36-40% aluminum oxide, 0.4-0.5% iron oxide, 1.4-1.6% titanium dioxide; particle size 20-500μm. Produced by Dalian Yibang Technology Co., Ltd., model: E-SPHERES hollow ceramic microspheres.

[0043] The weight average molecular weight of polyvinyl alcohol is 9000-10000. Produced by Merck, item number: 360627.

[0044] The preparation method of the modified graphene oxide is:

[0045] (1) mixing 1 part by mass of silicon nitride, 3 parts by mass of graphene oxide and 9 parts by mass of deionized water, stirring and mixing evenly to obtain a mixed solution;

[0046] (2) 12 parts by mass of the mixed solution were sprayed into liquid nitrogen in which 4 parts by mass of GeSbTe phase change powder was dispersed, frozen into microspheres, and dried to obtain modified graphene oxide.

[0047] The mass ratio of Ge, Sb and Te in the GeSbTe phase change powder is 1.5:1:0.6.

[0048] The nozzle hole used in the spray method has a diameter size of 0.3 mm.

[0049] The graphene oxide has a particle size of 0.5-3 μm and a number of layers of 1-5. It is produced by Beijing Dekedaojin Technology Co., Ltd.

[0050] The particle size of silicon nitride is 20-50nm. Produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0051] The preparation method of the environmentally friendly high temperature resistant water-based coating nano-enhancer is as follows: modified carbon nanotubes, modified hollow ceramic microbeads, modified graphene oxide and deionized water are mixed to obtain the nano-enhancer;

[0052] The water-based coating prepared by using the nano-enhancer includes the following components in mass fractions: 48 parts of water-based epoxy resin, 28 parts of nano-enhancer, 3 parts of curing agent, 2 parts of defoaming agent, 1 part of leveling agent, 3 parts of dispersant, 1 part of anti-settling agent and 10 parts of deionized water.

[0053] The water-based epoxy resin is water-based epoxy resin EP137 produced by Guangdong Qirun New Materials Co., Ltd. with a mass ratio of 0.4:1:1.7, Huntsman Compound of PZ 756-1 / 67 epoxy resin and Hexion Epikote 828 epoxy resin.

[0054] Curing agent, produced by Suzhou Meiguowang Flooring Materials Co., Ltd., model: water-based epoxy curing agent WG802.

[0055] The dispersant is German BYK-190 wetting dispersant.

[0056] The defoamer is German BYK defoamer BYK028.

[0057] The leveling agent is German BYK306 leveling agent.

[0058] The anti-settling agent is Evonik Degussa AEROSIL R972.

[0059] The preparation method of the water-based paint comprises: uniformly mixing and stirring the components of the water-based paint according to proportion to obtain the water-based paint.

[0060] Example 2

[0061] This embodiment provides an environmentally friendly nano-enhancer for high temperature resistant water-based coatings, comprising the following components in parts by weight: 3 parts of modified carbon nanotubes, 7 parts of modified hollow ceramic microspheres, 2 parts of modified graphene oxide, and 30 parts of deionized water;

[0062] The preparation method of the modified carbon nanotubes is as follows: 0.04 parts by mass of silane coupling agent KH560 and 1 part by mass of carbon nanotubes are added to 6 parts by mass of propanol, stirred at 45°C for 80 minutes, 0.06 parts by mass of phenolic resin are added, stirred evenly and then the solvent is removed, reacted at 110°C for 100 minutes, and cooled to room temperature to obtain the modified carbon nanotubes;

[0063] The carbon nanotubes are a mixture of double-walled carbon nanotubes, single-walled carbon nanotubes and multi-walled carbon nanotubes in a mass ratio of 1:2:0.7; the double-walled carbon nanotubes have a diameter of 2-4 nm, a length of 40-60 μm, and a specific surface area of ​​400-600 m 2 / g; diameter of single-walled carbon nanotubes: 1-2nm, length: 5-30μm, specific surface area 800-1200m 2 / g; diameter of multi-walled carbon nanotubes: 5-15nm, length: 0.5-2μm, specific surface area: 50-80m 2 / g. Produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0064] The phenolic resin has a brand name of Allnex and a model number of VPW1946 46WA. This model of phenolic resin is a water-dilutable phenolic resin.

[0065] The preparation method of the modified hollow ceramic microspheres is as follows: 1 mass part of hollow ceramic microspheres, 0.04 mass part of silane coupling agent KH550 and 5 mass parts of 55% ethanol aqueous solution are mixed, the temperature is raised to 50° C. for reaction for 2 hours, 0.04 mass part of polyvinyl alcohol is continuously added, the temperature is 45° C. for reaction for 30 minutes, and the modified hollow ceramic microspheres are filtered and dried to obtain the modified hollow ceramic microspheres.

[0066] The chemical composition percentage of hollow ceramic microspheres is: 55-60% silicon dioxide, 36-40% aluminum oxide, 0.4-0.5% iron oxide, 1.4-1.6% titanium dioxide; particle size 20-500μm. Produced by Dalian Yibang Technology Co., Ltd., model: E-SPHERES hollow ceramic microspheres.

[0067] The weight average molecular weight of polyvinyl alcohol is 9000-10000. Merck, catalog number: 360627.

[0068] The preparation method of the modified graphene oxide is:

[0069] (1) mixing 1 part by mass of silicon nitride, 4 parts by mass of graphene oxide and 7 parts by mass of deionized water, stirring and mixing evenly to obtain a mixed solution;

[0070] (2) 12 parts by mass of the mixed solution were sprayed into liquid nitrogen in which 5 parts by mass of GeSbTe phase change powder was dispersed, frozen into microspheres, and dried to obtain modified graphene oxide.

[0071] The mass ratio of Ge, Sb and Te in the GeSbTe phase change powder is 1.7:1:0.3.

[0072] The nozzle hole used in the spray method has a diameter size of 0.2mm-0.4mm.

[0073] The graphene oxide has a particle size of 0.5-3 μm and a number of layers of 1-5. It is produced by Beijing Dekedaojin Technology Co., Ltd.

[0074] The particle size of silicon nitride is 20-50nm. Produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0075] The preparation method of the environmentally friendly high temperature resistant water-based coating nano-enhancer is as follows: modified carbon nanotubes, modified hollow ceramic microbeads, modified graphene oxide and deionized water are mixed to obtain the nano-enhancer;

[0076] The water-based coating prepared by using the nano-enhancer includes the following components in mass fractions: 50 parts of water-based epoxy resin, 25 parts of nano-enhancer, 4 parts of curing agent, 2 parts of defoaming agent, 2 parts of leveling agent, 2 parts of dispersant, 2 parts of anti-settling agent and 11 parts of deionized water.

[0077] The water-based epoxy resin is water-based epoxy resin EP137 produced by Guangdong Qirun New Materials Co., Ltd. with a mass ratio of 0.5:1:1.9, Huntsman Compound of PZ 756-1 / 67 epoxy resin and Hexion Epikote 828 epoxy resin.

[0078] Curing agent, produced by Suzhou Meiguowang Flooring Materials Co., Ltd., model: water-based epoxy curing agent WG802.

[0079] The dispersant is German BYK-190 wetting dispersant.

[0080] The defoamer is German BYK defoamer BYK028.

[0081] The leveling agent is German BYK306 leveling agent.

[0082] The anti-settling agent is Evonik Degussa AEROSIL R972.

[0083] The preparation method of the water-based paint comprises: uniformly mixing and stirring the components of the water-based paint according to proportion to obtain the water-based paint.

[0084] Comparative Example 1

[0085] The difference between this comparative example and Example 1 is that the modified carbon nanotubes are different.

[0086] The preparation method of the modified carbon nanotubes is as follows: 0.03 parts by mass of silane coupling agent KH560 and 1 part by mass of carbon nanotubes are added to 7 parts by mass of propanol, stirred at 42° C. for 90 minutes, filtered, and dried to obtain the modified carbon nanotubes.

[0087] Comparative Example 2

[0088] The difference between this comparative example and Example 1 is that the types of carbon nanotubes used in preparing the modified carbon nanotubes are different.

[0089] The carbon nanotubes are double-walled carbon nanotubes; the diameter of the double-walled carbon nanotubes is 2-4 nm, the length is 40-60 μm, and the specific surface area is 400-600 m 2 / g.

[0090] Comparative Example 3

[0091] The difference between this comparative example and Example 1 is that the ratios of the types of carbon nanotubes used in preparing the modified carbon nanotubes are different.

[0092] The carbon nanotubes are a mixture of double-walled carbon nanotubes, single-walled carbon nanotubes and multi-walled carbon nanotubes in a mass ratio of 1:1:1; the double-walled carbon nanotubes have a diameter of 2-4 m, a length of 40-60 μm, and a specific surface area of ​​400-600 m 2 / g; diameter of single-walled carbon nanotubes: 1-2nm, length: 5-30μm, specific surface area 800-1200m 2 / g; diameter of multi-walled carbon nanotubes: 5-15nm, length: 0.5-2μm, specific surface area: 50-80m 2 / g.

[0093] Comparative Example 4

[0094] The difference between this comparative example and Example 1 is that the preparation method of the modified hollow ceramic microspheres is different.

[0095] The preparation method of the modified hollow ceramic microspheres is as follows: 1 mass part of hollow ceramic microspheres, 0.03 mass part of silane coupling agent KH550 and 6 mass parts of 53% ethanol aqueous solution are mixed, the temperature is raised to 53° C. for reaction for 1.4 hours, and the modified hollow ceramic microspheres are filtered and dried to obtain the modified hollow ceramic microspheres.

[0096] Comparative Example 5

[0097] The difference between this comparative example and Example 1 is that the hollow ceramic microspheres are different.

[0098] The chemical composition percentage of hollow ceramic microspheres is: 55-65% silicon dioxide, 26-35% aluminum oxide, 0.2-1% Fe2O3 iron oxide, 0.2-0.6% calcium oxide, 1-2% magnesium oxide, 0.5-4.0% sodium oxide and potassium oxide, 0.01-2% carbon, 0.5-2% titanium dioxide, particle size: 1-10μm. Produced by Shanghai Gerunya Nanomaterials Co., Ltd.

[0099] Comparative Example 6

[0100] The difference between this comparative example and Example 1 is that the mass ratio of Ge, Sb and Te in the GeSbTe phase change powder is 1:3:2.

[0101] Comparative Example 7

[0102] The difference between this comparative example and Example 1 is that the graphene oxide has an average particle size of 5-10 μm and a number of layers of 15-20, and is produced by Sigma-Aldrich.

[0103] The particle size of silicon nitride is 100-150nm and it is produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0104] Performance Testing

[0105] The properties of the water-based coatings of Examples 1-2 and Comparative Examples 1-7 were measured.

[0106] 1. Temperature resistance: Refer to the standards DIN 53151 and ASTM D3359-17, test conditions: 250℃, 20 days, to determine the temperature resistance of water-based coatings.

[0107] 2. Abrasion resistance: Refer to ASTM D4060, test conditions: 1000 cycles, No. 10 wheel, load 1kg, measure weight loss.

[0108] 3. Salt spray resistance: refer to ASTM B117, test conditions: 500h.

[0109] 4. Adhesion: Refer to ASTM D3359, test conditions: spacing 1mm.

[0110] The test results are shown in Table 1.

[0111] Table 1 Performance test results

[0112]

[0113]

[0114] 5. Storage stability test

[0115] The water-based paint was stored at room temperature (25°C) for 3 months, 40°C for 3 months, -5°C for 3 months, and variable temperature for 3 months (-5°C, 25°C, 40°C for 10 days, for a total of 3 cycles) to observe whether stratification and precipitation occurred. The test results are shown in Table 2.

[0116] Table 2 Performance test results

[0117]

[0118]

[0119] The results show that the water-based resin prepared in Example 1-2 can withstand a high temperature of 250°C, and has excellent adhesion to cast iron and stainless steel, good salt spray resistance and wear resistance, and has excellent effect in spraying the air compressor housing of the air compression component. The comparative examples show that the performance of the water-based coating decreases to varying degrees when the conditions for preparing the nano-enhancer are changed.

[0120] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Environmentally friendly nano-enhancer for high temperature resistant water-based coatings, characterized in that: The invention comprises the following components in parts by weight: 3-8 parts of modified carbon nanotubes, 4-7 parts of modified hollow ceramic microbeads, 2-6 parts of modified graphene oxide and 30-40 parts of deionized water; The modified carbon nanotubes are prepared by adding 0.02-0.04 parts by mass of a silane coupling agent KH560 and 1 part by mass of carbon nanotubes to 6-9 parts by mass of propanol, stirring and reacting at 40-45°C for 80-100 minutes, adding 0.03-0.06 parts by mass of a phenolic resin, stirring evenly, removing the solvent, reacting at 110-120°C for 100-120 minutes, and cooling to room temperature to obtain the modified carbon nanotubes. The modified hollow ceramic microspheres are prepared by mixing 1 part by mass of the hollow ceramic microspheres, 0.02-0.04 parts by mass of a silane coupling agent KH550, and 5-7 parts by mass of a 50-55% ethanol aqueous solution, heating the mixture to 50-55° C. for reaction for 1-2 hours, adding 0.04-0.06 parts by mass of polyvinyl alcohol, reacting the mixture at 40-45° C. for reaction for 30-50 minutes, filtering, and drying to obtain the modified hollow ceramic microspheres. The preparation method of the modified graphene oxide is: (1) mixing 1 part by mass of silicon nitride, 2-4 parts by mass of graphene oxide, and 7-10 parts by mass of deionized water, stirring and mixing uniformly to obtain a mixed solution; (2) 12 parts by mass of the mixed solution was sprayed into liquid nitrogen in which 3-5 parts by mass of GeSbTe phase change powder was dispersed, and the mixture was frozen into microspheres and dried to obtain modified graphene oxide.

2. The environmentally friendly nano-enhancer for high-temperature resistant water-based coating according to claim 1, characterized in that: The carbon nanotubes are a mixture of double-walled carbon nanotubes, single-walled carbon nanotubes and multi-walled carbon nanotubes in a mass ratio of 1: (2-3): (0.3-0.7); the double-walled carbon nanotubes have a diameter of 2-4 nm, a length of 40-60 μm, and a specific surface area of ​​400-600 m 2 / g; the diameter of single-walled carbon nanotubes is 1-2nm, the length is 5-30μm, and the specific surface area is 800-1200m 2 / g; the diameter of multi-walled carbon nanotubes is 5-15nm, the length is 0.5-2μm, and the specific surface area is 50-80m 2 / g.

3. The environmentally friendly nano-enhancer for high temperature resistant water-based coating according to claim 1, characterized in that: The chemical composition percentages of the hollow ceramic microspheres are as follows: 55-60% silicon dioxide, 36-40% aluminum oxide, 0.4-0.5% iron oxide, 1.4-1.6% titanium dioxide, and a particle size of 20-500 μm.

4. The environmentally friendly nano-enhancer for high temperature resistant water-based coating according to claim 1, characterized in that: The weight average molecular weight of the polyvinyl alcohol is 9,000-10,000.

5. The environmentally friendly nano-enhancer for high temperature resistant water-based coating according to claim 1, characterized in that: The mass ratio of Ge, Sb and Te in the GeSbTe phase change powder is (1.4-1.7):1:(0.3-0.8).

6. The environmentally friendly nano-enhancer for high temperature resistant water-based coating according to claim 1, characterized in that: The graphene oxide has a particle size of 0.5-3 μm and a layer number of 1-5 layers.

7. The environmentally friendly nano-enhancer for high temperature resistant water-based coating according to claim 1, characterized in that: The particle size of the silicon nitride is 20-50 nm.

8. A water-based coating prepared using the nano-enhancer according to any one of claims 1 to 7, characterized in that: The invention comprises the following components in mass fractions: 45-50 parts of waterborne epoxy resin, 25-30 parts of nano-enhancer, 2-4 parts of curing agent, 2-3 parts of defoamer, 1-2 parts of leveling agent, 2-4 parts of dispersant, 1-2 parts of anti-settling agent and 11-13 parts of deionized water.

9. The water-based paint according to claim 8, characterized in that: The waterborne epoxy resin is waterborne epoxy resin EP137, Huntsman Compound of PZ 756-1 / 67 epoxy resin and Hexion Epikote 828 epoxy resin.

10. The use of the water-based paint according to claim 8, characterized in that: The water-based paint is used for spraying air compression components of an air compressor.

Citation Information

Patent Citations

  • Water-based paint applied in aluminum-plastic plates and color steel coiled material

    CN103602188A

  • Special high temperature resistant binder for lithium batteries and preparation method of special high temperature resistant binder

    CN108123139A

  • Green, environmentally-friendly, waterproof, antibacterial and mildew-resistant decoration coating and preparation method thereof

    CN108395745A

  • Fireproof coating with high-temperature resistance and preparation method of fireproof coating

    CN108641551A

  • Three-dimensional cross-linked network phenolic resin coating and preparation method thereof

    CN113913080A