A method for manufacturing high-rigidity and low-stress machine tool cast iron and its application

By using a double-layer glow plasma infiltration metallurgical process to perform Mo infiltration in a carbon-containing atmosphere during the casting process, the impact of casting stress on the casting is solved, the hardness and tensile strength of the cast iron are improved, and the residual stress is reduced, achieving Higher mechanical properties.

CN118374765BActive Publication Date: 2024-10-18YUXI JINFU INTELLIGENT EQUIP CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410564971.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-10-18
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

Casting stress caused by volume changes during the casting process will adversely affect the strength, fatigue limit, stiffness and dimensional accuracy of the casting, resulting in reduced service life of the part.

Method used

The double-layer glow plasma metal infiltration process is used to infiltrate Mo in a carbon-containing atmosphere to improve the hardness and tensile strength of cast iron while reducing residual stress. This process forms argon ions through the glow discharge phenomenon, bombards the surface of the source material, causes the Mo element to be sputtered and diffused on the surface of the workpiece, forming an alloy layer with specific physical and chemical properties, enhancing the uniformity of graphite balls and the formation of carbides. Reduces brittleness tendency.

Benefits of technology

Significantly improves the tensile strength and elastic modulus of cast iron, reduces residual stress, reduces the tendency of brittle cracking, promotes the precipitation of pearlite through carbide nucleation, and improves the strength of ferrite with a grain size less than or equal to that of ferrite.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004828927690000091
    Figure BDA0004828927690000091
  • Figure BDA0004828927690000101
    Figure BDA0004828927690000101
Patent Text Reader

Abstract

The present application relates to an ion metallization process, which is specifically used for the manufacture of cast iron workpieces to improve their strength and reduce their stress. The present application adopts a double-layer glow plasma metallization process to perform Mo infiltration in a carbon-containing gas atmosphere, thereby improving the hardness, tensile strength and elastic modulus of cast iron, while reducing residual stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an ion metal diffusion process, which is specifically used for manufacturing cast iron workpieces to improve their strength and reduce their stress. Background Art

[0002] When the liquid metal is cooled, it will produce different degrees of liquid-solid shrinkage due to the decrease in temperature. In particular, the solid phase transformation of the alloy will be accompanied by the change of the casting volume. If these volume changes are hindered by the outside world or mutually restricted inside the casting, additional stress will be generated in the casting, which is the so-called casting stress. Residual stress refers to the stress that remains inside the casting after the external load is removed. Casting residual stress refers to the stress that remains inside the casting after the casting is completed, the casting is cooled to room temperature and without any heat treatment. Casting residual stress is generally divided into macro residual stress and micro residual stress. The uneven volume change of the casting during the solidification process and external constraints lead to macro residual stress. The residual stress inside the casting often has an adverse effect on machining and subsequent assembly and use, and affects the strength, fatigue limit, stiffness and dimensional accuracy of the parts, resulting in the deterioration of the working condition of the parts and reducing the service life of the parts; the consequences of residual stress are sometimes not immediately apparent, but the superposition of various stresses when the parts are further processed or in service. When the total stress exceeds the strength limit of the material, fracture occurs. Summary of the invention

[0003] The present application provides a method for manufacturing high-rigidity and low-stress machine tool cast iron and application of the obtained cast iron in machine tools.

[0004] The raw materials for cast iron casting in the present invention include: Q10 pig iron, 45# steel, 75 ferrosilicon, ferromolybdenum, ferrovanadium, and rare earth magnesium alloy spheroidizer. The amount of spheroidizer added is 1.3%, 75 ferrosilicon is used as inoculant, and the primary inoculation adopts bottom inoculation, the amount of addition is 1.2%, the particle size is 4-10mm, and the temperature is controlled at 1500-1550℃ before being discharged from the furnace. The bottom of the ladle is used for spheroidization inoculation treatment, and after the ladle is taken out of the resistance furnace, the primary inoculant and the spheroidizer are poured into the bottom of the ladle. After the molten iron is poured into the ladle, the secondary inoculant is poured on the surface of the molten iron, and then the perlite slag collecting agent is evenly covered on the surface of the molten iron to collect slag and slag, and then casting is performed after slag removal. Each ladle is cast with a machine tool component test block with a wall thickness of 25mm, and after casting, it is cooled for 3 hours. The composition of cast iron is (by mass percentage): C 3.8%, Si 2.7%, Mo 0.3%, Mn 0.5%, Mg<0.04%, P<0.04%, S<0.01%, and the balance is Fe.

[0005] The sample obtained after casting is polished to 2000 mesh with metallographic sandpaper from coarse to fine, and then ultrasonically cleaned for 20 minutes in a container filled with acetone or alcohol. After being taken out, it is wiped clean and dried with clean gauze. The cleaned cast iron is placed in a double-layer glow plasma infiltration furnace.

[0006] The Mo target was prepared by cold spraying process. It was polished to 1800 mesh with sandpaper from coarse to fine, and then immersed in alcohol for ultrasonic cleaning for 30 minutes to ensure the surface purity. After cleaning, it was placed in a double-layer glow plasma metal infiltration furnace.

[0007] Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to 10 -1 Below Pa;

[0008] Open the valve of the methane bottle, introduce methane into the furnace to 500Pa, adjust the air flow rate to zero, start the mechanical pump, and evacuate to 10 -1 Below Pa, repeat this step twice;

[0009] Open the methane inlet valve and adjust the gas flow rate to 30-40sccm to keep the gas intake and exhaust volume in the furnace balanced and maintain the gas pressure at 30-35Pa.

[0010] Turn on the source and workpiece voltage adjustment switch buttons on the double-brightness furnace, slowly adjust the workpiece voltage to 450-550V, the source voltage to 800-900V, the processing temperature to 900-1000℃, and the Mo infiltration holding time to 6h;

[0011] After the treatment, the workpiece and source voltage are slowly reduced to zero, and the furnace is cooled after the reaction is completed, and then taken out after cooling to room temperature;

[0012] The main principle of double-layer glow plasma metallization technology is to use the glow discharge phenomenon of gas and set a source composed of alloying elements in the device. A DC power supply is set between the source and the anode, and a glow discharge phenomenon can be generated in between. The argon ions formed by the glow discharge phenomenon bombard the surface of the source material, so that the alloying elements to be infiltrated are sputtered out, and an alloy layer with specific physical and chemical properties is formed on the surface of the workpiece through precipitation and diffusion.

[0013] The present application adopts a double-layer glow plasma metal infiltration process to perform Mo infiltration in a carbon-containing gas atmosphere, thereby improving the hardness, tensile strength and elastic modulus of the cast iron, while reducing the residual stress.

[0014] The cast iron parts prepared by the present application have a carbon equivalent of 3.8%, have high tensile strength and hardness, and the residual stress is reduced and the elastic modulus is improved. Due to the addition of a carbon-containing atmosphere during the metal infiltration process, the surface carbon content is further enhanced and the hardness is improved. Most of the graphite balls in the cast iron in the present application are relatively round and have good uniformity. At the same time, there is a small amount of deformed graphite. As the Mo content increases, the number of graphite balls decreases slightly, while the number of round graphite balls decreases slightly, and the number of deformed graphite balls increases slightly. The Mo element is a strong carbide-forming element with a strong tendency to segregate. After the spherical graphite is generated, it affects the morphology of the graphite balls. Mo atoms will form carbides with carbon atoms. This situation will consume carbon atoms in the organization, so that the number of graphite balls in the final organization is reduced. Under the action of segregation, the growth in all directions is uneven, which leads to the distortion of the graphite balls. The deformed graphite balls can effectively improve the tensile strength and elastic modulus of the cast iron.

[0015] Mo element can reduce austenite eutectoid reaction temperature, increase austenite to pearlite and ferrite transformation time, pearlite precipitation of lifting, and Mo element is strong carbide forming element, adding Mo element increases the driving force of molybdenum carbide nucleation, improves carbide nucleation on grain boundary, carbide provides ferrite and cementite nucleation core, promotes pearlite content to rise. Mo element can increase supercooling during cooling, promote nucleation, the higher the Mo content, the greater the supercooling, the higher the nucleation rate, and the smaller the grain size. At the same time, with the increase of Mo content, the number of carbides in the matrix will increase, and precipitating more carbides in austenite can increase the ferrite nucleation rate, thereby reducing the grain size of ferrite. Pearlite is a hard and brittle phase, which has a significant effect on the strength of ductile iron.

[0016] Due to the use of plasma metal infiltration, the hardness of the cross section of the infiltration layer changes gradually, thereby greatly reducing stress concentration, reducing the tendency of brittle cracking, and improving the impact resistance of the coating. In addition, in the present application, the metal infiltration is carried out at 900-1000°C, and the treatment time is extended to 6h. While promoting Mo infiltration and diffusion, the same effect of reducing residual experience as thermal aging is obtained. DETAILED DESCRIPTION

[0017] Embodiment 1:

[0018] The raw materials for cast iron casting in the present invention include: Q10 pig iron, 45# steel, 75 ferrosilicon, ferromolybdenum, ferrovanadium, and rare earth magnesium alloy spheroidizer. The amount of spheroidizer added is 1.3%, 75 ferrosilicon is used as an inoculant, and the primary inoculation adopts the bottom inoculation of the ladle, the amount of addition is 1.2%, the particle size is 8mm, and the temperature is controlled at 1550℃ before being discharged from the furnace. The bottom of the ladle is used for spheroidizing inoculation treatment, and after the ladle is taken out of the resistance furnace, the primary inoculant and the spheroidizer are poured into the bottom of the ladle. After the molten iron is poured into the ladle, the secondary inoculant is poured on the surface of the molten iron, and then the perlite slag collecting agent is evenly covered on the surface of the molten iron to collect slag and slag, and then casting is performed after slag removal. Each ladle is cast with a machine tool component test block with a wall thickness of 25mm, and after casting, it is cooled for 3 hours. The composition of cast iron is (by mass percentage): C 3.8%, Si 2.7%, Mo 0.3%, Mn 0.5%, Mg 0.02%, P 0.02%, S 0.005%, and the balance is Fe.

[0019] The sample obtained after casting is polished to 2000 mesh with metallographic sandpaper from coarse to fine, and then placed in a container filled with acetone or alcohol for ultrasonic cleaning for 20 minutes. After taking it out, wipe it clean and dry with clean gauze. The cleaned cast iron is placed in a double-layer glow plasma infiltration furnace. The Mo target is a target prepared by cold spraying process. It is polished to 1800 mesh with sandpaper from coarse to fine, and then immersed in alcohol for ultrasonic cleaning for 30 minutes to ensure the surface purity. After cleaning, it is placed in a double-layer glow plasma infiltration furnace. Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to 10 -1 Open the valve of the methane bottle, introduce methane into the furnace to 500Pa, adjust the air flow rate to zero, start the mechanical pump, and vacuumize again to 10 -1 Pa, repeat this step twice; open the methane inlet valve, adjust the gas flow rate to 40sccm, keep the air intake and exhaust volume in the furnace balanced, maintain the air pressure at 35Pa, turn on the source and workpiece voltage adjustment switch buttons on the double-brightness furnace, slowly adjust the workpiece voltage to 500V, the source voltage to 850V, the processing temperature: 1000℃, and the Mo infiltration insulation time for 6h; after the treatment is completed, slowly reduce the workpiece and source voltages to zero, cool with the furnace after the reaction is completed, and take out after cooling to room temperature.

[0020] According to the room temperature tensile test method of GB / T228-2010 for metal materials, a static tensile load is uniformly applied along the axial direction of the sample until the elongation of the sample breaks. During the whole process, the load applied to the sample is measured and the tensile strength value can be calculated. The hardness test method is carried out according to the method of GB / T231.2-2002 for metal Brinell hardness test. The elastic modulus is tested in accordance with GB / T22315-2008, and the residual stress is tested in accordance with GB / T31310-2014.

[0021] Embodiment 2:

[0022] The casting process is the same as that in Example 1. The sample obtained after casting is polished to 2000 mesh with metallographic sandpaper from coarse to fine, and then placed in a container filled with acetone or alcohol for ultrasonic cleaning for 20 minutes. After being taken out, it is wiped clean and dried with clean gauze. The cleaned cast iron is placed in a double-layer glow plasma infiltration furnace. The Mo target material is a target material prepared by a cold spraying process. After being polished to 1800 mesh with sandpaper from coarse to fine, it is immersed in alcohol for ultrasonic cleaning for 30 minutes to ensure the surface purity. After cleaning, it is placed in a double-layer glow plasma infiltration furnace. Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to 10 -1 Open the valve of the methane bottle, introduce methane into the furnace to 500Pa, adjust the air flow rate to zero, start the mechanical pump, and vacuumize again to 10 -1 Pa or less, repeat this step twice; open the methane inlet valve, adjust the gas flow rate to 30sccm, keep the air intake and exhaust volume in the furnace balanced, maintain the air pressure at 30Pa, turn on the source and workpiece voltage adjustment switch buttons on the double-brightness furnace, slowly adjust the workpiece voltage to 550V, the source voltage to 900V, the processing temperature: 900℃, and the Mo infiltration insulation time for 6h; after the treatment is completed, slowly reduce the workpiece and source voltages to zero, cool with the furnace after the reaction is completed, and take out after cooling to room temperature; then test with reference to Example 1.

[0023] Comparative Example 1:

[0024] The casting process is the same as that in Example 1. The sample obtained after casting is polished to 2000 mesh with metallographic sandpaper from coarse to fine, and then placed in a container filled with acetone or alcohol for ultrasonic cleaning for 20 minutes. After being taken out, it is wiped clean and dried with clean gauze. The cleaned cast iron is placed in a double-layer glow plasma infiltration furnace. The Mo target material is a target material prepared by a cold spraying process. After being polished to 1800 mesh with sandpaper from coarse to fine, it is immersed in alcohol for ultrasonic cleaning for 30 minutes to ensure the surface purity. After cleaning, it is placed in a double-layer glow plasma infiltration furnace. Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to 10 -1 Open the valve of the argon gas bottle, introduce argon gas into the furnace to 500Pa, adjust the gas flow rate to zero, turn on the mechanical pump, and evacuate the furnace to 10 -1 Pa or less, repeat this step twice; open the methane inlet valve, adjust the gas flow rate to 30sccm, keep the air intake and exhaust volume in the furnace balanced, maintain the air pressure at 30Pa, turn on the source and workpiece voltage adjustment switch buttons on the double-brightness furnace, slowly adjust the workpiece voltage to 550V, the source voltage to 900V, the processing temperature: 900℃, and the Mo infiltration insulation time for 6h; after the treatment is completed, slowly reduce the workpiece and source voltages to zero, cool with the furnace after the reaction is completed, and take out after cooling to room temperature; then test with reference to Example 1.

[0025] Comparative Example 2:

[0026] The casting process is the same as that in Example 1. The sample obtained after casting is polished to 2000 mesh with metallographic sandpaper from coarse to fine, and then placed in a container filled with acetone or alcohol for ultrasonic cleaning for 20 minutes. After being taken out, it is wiped clean and dried with clean gauze. The cleaned cast iron is placed in a double-layer glow plasma infiltration furnace. The Mo target material is a target material prepared by a cold spraying process. After being polished to 1800 mesh with sandpaper from coarse to fine, it is immersed in alcohol for ultrasonic cleaning for 30 minutes to ensure the surface purity. After cleaning, it is placed in a double-layer glow plasma infiltration furnace. Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to 10 -1 Open the valve of the methane bottle, introduce methane into the furnace to 500Pa, adjust the air flow rate to zero, start the mechanical pump, and vacuumize again to 10 -1 Pa, repeat this step twice; open the methane inlet valve, adjust the gas flow rate to 30sccm, keep the gas intake and exhaust volume in the furnace balanced, maintain the gas pressure at 30Pa, hit the treatment temperature: 900℃, keep warm for 6h; after the reaction is completed, cool with the furnace, take out after cooling to room temperature; then test with reference to Example 1.

[0027] Comparative Example 3:

[0028] The casting process is the same as that in Example 1. The sample obtained after casting is polished to 2000 mesh with metallographic sandpaper from coarse to fine, and then placed in a container filled with acetone or alcohol for ultrasonic cleaning for 20 minutes. After being taken out, it is wiped clean and dried with clean gauze. The cleaned cast iron is placed in a double-layer glow plasma infiltration furnace. The Mo target material is a target material prepared by a cold spraying process. After being polished to 1800 mesh with sandpaper from coarse to fine, it is immersed in alcohol for ultrasonic cleaning for 30 minutes to ensure the surface purity. After cleaning, it is placed in a double-layer glow plasma infiltration furnace. Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to 10 -1 Open the valve of the methane bottle, introduce methane into the furnace to 500Pa, adjust the air flow rate to zero, start the mechanical pump, and vacuumize again to 10 -1 Pa or less, repeat this step twice; open the methane inlet valve, adjust the gas flow rate to 30sccm, keep the air intake and exhaust volume in the furnace balanced, maintain the air pressure at 30Pa, turn on the source and workpiece voltage adjustment switch buttons on the double-brightness furnace, slowly adjust the workpiece voltage to 550V, the source voltage to 900V, the processing temperature: 800℃, and the Mo infiltration insulation time for 6h; after the treatment is completed, slowly reduce the workpiece and source voltages to zero, cool with the furnace after the reaction is completed, and take out after cooling to room temperature; then test with reference to Example 1.

[0029] Comparative Example 4:

[0030] The casting process is the same as that in Example 1. The sample obtained after casting is polished to 2000 mesh with metallographic sandpaper from coarse to fine, and then placed in a container filled with acetone or alcohol for ultrasonic cleaning for 20 minutes. After being taken out, it is wiped clean and dried with clean gauze. The cleaned cast iron is placed in a double-layer glow plasma infiltration furnace. The Mo target material is a target material prepared by a cold spraying process. After being polished to 1800 mesh with sandpaper from coarse to fine, it is immersed in alcohol for ultrasonic cleaning for 30 minutes to ensure the surface purity. After cleaning, it is placed in a double-layer glow plasma infiltration furnace. Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to 10 -1 Open the valve of the methane bottle, introduce methane into the furnace to 500Pa, adjust the air flow rate to zero, start the mechanical pump, and vacuumize again to 10 -1 Pa or less, repeat this step twice; open the methane inlet valve, adjust the gas flow rate to 30sccm, keep the air intake and exhaust volume in the furnace balanced, maintain the air pressure at 30Pa, turn on the source and workpiece voltage adjustment switch buttons on the double-brightness furnace, slowly adjust the workpiece voltage to 550V, the source voltage to 900V, the processing temperature: 900℃, and the Mo infiltration insulation time for 5h; after the treatment, slowly reduce the workpiece and source voltages to zero, cool with the furnace after the reaction is completed, and take out after cooling to room temperature; then test with reference to Example 1.

[0031] Comparative Example 5:

[0032] The casting process is the same as that in Example 1. The sample obtained after casting is polished to 2000 mesh with metallographic sandpaper from coarse to fine, and then placed in a container filled with acetone or alcohol for ultrasonic cleaning for 20 minutes. After being taken out, it is wiped clean and dried with clean gauze. The cleaned cast iron is placed in a double-layer glow plasma infiltration furnace. The Mo target material is a target material prepared by a cold spraying process. After being polished to 1800 mesh with sandpaper from coarse to fine, it is immersed in alcohol for ultrasonic cleaning for 30 minutes to ensure the surface purity. After cleaning, it is placed in a double-layer glow plasma infiltration furnace. Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to 10 -1 Open the valve of the methane bottle, introduce methane into the furnace to 500Pa, adjust the air flow rate to zero, start the mechanical pump, and vacuumize again to 10 -1 Pa or less, repeat this step twice; open the methane inlet valve, adjust the gas flow rate to 30sccm, keep the air intake and exhaust volume in the furnace balanced, maintain the air pressure at 30Pa, turn on the source and workpiece voltage adjustment switch buttons on the double-brightness furnace, slowly adjust the workpiece voltage to 550V, the source voltage to 900V, the processing temperature: 1100℃, and the Mo infiltration insulation time for 6h; after the treatment, slowly reduce the workpiece and source voltages to zero, cool with the furnace after the reaction is completed, and take out after cooling to room temperature; then test with reference to Example 1.

[0033] Table 1 Test results

[0034]

[0035]

Claims

1. A method for manufacturing high-rigidity and low-stress machine tool cast iron, characterized in that: The steps include: The cast iron obtained after casting is polished step by step from coarse to fine with metallographic sandpaper, and then placed in a container filled with acetone or alcohol for ultrasonic cleaning. After being taken out, it is wiped clean and dry with clean gauze, and the cleaned cast iron is placed in a double-layer glow plasma infiltration furnace; The Mo target material was polished with sandpaper from coarse to fine, and then immersed in alcohol for ultrasonic cleaning to ensure the surface purity. After cleaning, it was placed in a double-layer glow plasma metallization furnace; Turn on the circulating water and mechanical pump to pump the ambient air pressure in the furnace to below 10-1Pa; Open the valve of the methane bottle, introduce methane into the furnace to 500Pa, then adjust the air flow value to zero, turn on the mechanical pump, and evacuate the air again to below 10-1Pa. Repeat this step twice; Open the methane inlet valve and adjust the gas flow rate to 30-40sccm to keep the gas intake and exhaust volume in the furnace balanced and maintain the gas pressure at 30-35Pa. Turn on the source and workpiece voltage adjustment switch buttons on the double-brightness furnace, slowly adjust the workpiece voltage to 450-550V, the source voltage to 800-900V, the processing temperature to 900-1000℃, and the Mo infiltration holding time to 6h; After the treatment is completed, the workpiece and source voltage are slowly reduced to zero. After the reaction is completed, the furnace is cooled and taken out after cooling to room temperature.

2. The manufacturing method according to claim 1, characterized in that The casting temperature is controlled at 1500-1550°C.

3. The manufacturing method according to claim 1, characterized in that: The composition of cast iron is calculated by mass percentage: C 3.8%, Si 2.7%, Mo 0.3%, Mn 0.5%, Mg<0.04%, P<0.04%, S<0.01%, and the balance is Fe.

4. The manufacturing method according to claim 1, characterized in that: The cast iron obtained after casting was polished step by step from coarse to fine with metallographic sandpaper to 2000 mesh.

5. The manufacturing method according to claim 3, characterized in that: The Mo target is a target prepared by cold spraying process.

6. The manufacturing method according to claim 1, characterized in that: The Mo target is ground with sandpaper from coarse to fine to 1800 mesh.

7. The manufacturing method according to claim 1, characterized in that: The casting was ultrasonically cleaned for 20 min.

8. The manufacturing method according to claim 1, characterized in that: The Mo target was ultrasonically cleaned for 30 min.

9. A high-rigidity and low-stress machine tool cast iron produced by the manufacturing method according to claims 1-8.

10. Application of the high-rigidity and low-stress machine tool cast iron as claimed in claim 9 in the field of machine tools.

Citation Information

Patent Citations

  • Method for preparing antibacterial and wear-resistant stainless steel permeation layer

    CN101956165A

  • Production method of a thick coating with layered structure

    US20190177856A1