A doped activated carbon-nickel oxide composite antibacterial agent and its preparation method and application

Through Bi-doped activated carbon-loaded nickel oxide composite antibacterial agent, the problem of difficulty and cost of recycling antibacterial agents in water environments is solved, the antibacterial effect and recovery are improved, and effective inhibition and environmental protection and safety of water bacteria are achieved.

CN118383385BActive Publication Date: 2024-11-22YUNNAN FORESTRY & GRASSLAND TECH PROMOTION STATION +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410721480.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-11-22
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

The existing water antibacterial agents are difficult to recover after use in water environments, and photocatalytic antibacterial methods have a great impact on light reflection and refraction, resulting in limited antibacterial effects and high cost.

Method used

The nickel oxide composite antibacterial agent with doped activated carbon-loaded nanoparticles is used, and the antibacterial effect and magnetism are improved by doping Bi elements, thereby reducing the difficulty and cost of separation and recovery.

Benefits of technology

It improves the antibacterial effect and separation and recovery effect of the composite antibacterial agent, reduces the actual application cost, avoids the secondary pollution of the water body by chemical residues, and achieves effective inhibition of bacteria in the water environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118383385B_ABST
    Figure CN118383385B_ABST
Patent Text Reader

Abstract

The present invention discloses a doped activated carbon-nickel oxide composite antibacterial agent and a preparation method and application thereof, and belongs to the technical field of antibacterial material preparation. The present invention includes a doped activated carbon-nickel oxide composite antibacterial agent, wherein the composite antibacterial agent is doped with bismuth element, and the activated carbon is loaded with nickel oxide in the form of nanoparticles. The composite antibacterial agent is prepared by the preparation method of the present invention, and the composite antibacterial agent is used as an antibacterial agent for Gram-positive bacteria and Gram-negative bacteria in a water environment, which can safely and efficiently kill bacteria in a water environment and remove dye pollutants, so that the water body is purified, while reducing the comprehensive cost of water environment management.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of antibacterial material preparation, and specifically relates to a doped activated carbon (AC)-nickel oxide (NiO) composite antibacterial agent and a preparation method and application thereof. Background Art

[0002] The aquatic environment contains a large number of bacteria that can infect individuals directly or indirectly through aquatic plants, animals or water sources. Waterborne pathogens cause more than 2 million deaths each year, most of which are children under the age of five. With the advancement of industrialization, especially in newly industrialized countries, biohazard pollution has become more and more common and serious. Therefore, even in today's rapidly changing medical conditions, inhibiting and removing the growth and reproduction of harmful bacteria in water is still an important task related to human health.

[0003] Traditional methods of water bacterial disinfection include chlorination, ozone disinfection, ultraviolet (UV) disinfection, filtration and heat sterilization. These methods have a long history of use, are mature, easy to operate, and can effectively inactivate pathogenic microorganisms. However, they have inherent limitations such as easy production of chemical residues, easy resurrection of eliminated pathogenic microorganisms, and high energy consumption. As a result, their antibacterial properties are limited.

[0004] Taking into account the original ecological balance in the water environment, sterilization and disinfection of the water environment requires materials that inhibit the growth and reproduction of water bacteria in a safe and environmentally friendly manner.

[0005] In recent years, inorganic antibacterial materials have been widely used in inhibiting the growth and reproduction of aquatic bacteria due to their stable properties, good heat resistance, high safety, and low resistance to drug resistance. Among them, inorganic antibacterial materials using photocatalytic technology to kill bacteria have become a hot topic in research. This method mainly generates reactive oxygen species (ROS) such as superoxide radicals (O 2- ), hydroxyl radicals (OH-) and hydrogen peroxide (H2O2) to kill bacteria. When ROS enter cells, an oxidative stress reaction occurs, leading to damage to cell components, protein oxidation, reduced enzyme activity and DNA damage, which inactivates pathogens. This method has the advantages of mild reaction conditions, no need for additional oxidants and simple operation process. However, photocatalytic antibacterial requires efficient use of visible light, near-infrared light or ultraviolet light excitation. In a water environment, the water body will produce certain reflection and refraction effects on light, which limits the antibacterial effect of photocatalytic antibacterial agents in aquatic environments. At the same time, the particularity of the aquatic environment has also formed a major obstacle to the recycling and reuse of antibacterial agents, making it difficult to recycle antibacterial agents in aquatic environments, resulting in relatively high costs.

[0006] Therefore, it is necessary to provide a doped AC-NiO composite antibacterial agent and its preparation method and application, successfully prepare a NiO composite antibacterial agent with the morphology of AC loaded nanoparticles doped with Bi, and apply it in a water environment to mainly kill Gram-positive bacteria and Gram-negative bacteria. Reduce the negative impact of the water environment on the antibacterial effect of the composite antibacterial agent. At the same time, reduce the difficulty of separation and recovery of the composite antibacterial agent after use in the water environment, reduce the actual application cost of the composite antibacterial agent, and improve the environmental safety of the composite antibacterial agent for water treatment. Summary of the invention

[0007] In order to overcome the problems in the background technology, the present invention proposes a doped AC-NiO composite antibacterial agent and a preparation method and application thereof. By loading nickel oxide in the form of nanoparticles on activated carbon, on the one hand, the problem of difficulty in separation and recovery caused by the direct entry of nickel oxide in powder form into the water body is solved; on the other hand, the activated carbon itself has certain adsorption properties, which can enhance the adsorption effect of the composite antibacterial agent, which is beneficial to the improvement of the antibacterial effect of the composite antibacterial agent. However, loading nickel oxide on activated carbon will have a great impact on the antibacterial effect of nickel oxide itself, so that the overall antibacterial effect of the AC-NiO composite antibacterial agent is greatly reduced. Therefore, by doping Bi, the band gap is reduced and the recombination of electrons and holes is hindered, thereby improving the antibacterial effect of the AC-NiO composite antibacterial agent. At the same time, doping Bi can also enhance the magnetism of the composite antibacterial agent, which is helpful to improve the separation and recovery effect of the composite antibacterial agent.

[0008] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0009] On one hand, the present invention provides a doped AC-NiO composite antibacterial agent, wherein the composite antibacterial agent is doped with bismuth element, and the activated carbon is loaded with nickel oxide in the shape of nanoparticles.

[0010] Another aspect of the present invention provides a method for preparing a doped AC-NiO composite antibacterial agent, the preparation method comprising the following steps:

[0011] S1: Weigh 0.24g NiCl2·6H2O and dissolve it in 25ml ethanol to form a green transparent solution, weigh 1.46g sodium acetate and dissolve it in 10ml distilled water, weigh 0.59g trisodium citrate and dissolve it in 15ml distilled water;

[0012] S2: The three solutions obtained in step S2 are mixed and stirred to obtain a transparent solution, and 0.5 g of activated carbon powder and 0.2 g of Bi(NO3)3·5H2O are added to the transparent solution to obtain a mixed solution;

[0013] S3: performing a sealed hydrothermal reaction treatment on the mixed solution obtained in step S3, and then naturally cooling it to room temperature to obtain a blue-green product;

[0014] S4: washing the blue-green product obtained in step S3 with deionized water for 5 times, and then washing the blue-green product obtained in step S4 with ethanol for 5 times, and then drying and calcining the product to obtain a bismuth-doped activated carbon-nickel oxide composite antibacterial agent.

[0015] Preferably, the activated carbon is prepared by the following steps:

[0016] (1) Wash the macadamia shells, dry and crush them, then take 3g of shell powder and mix them with 10ml of activator and soak them for a certain period of time;

[0017] (2) vacuum filtering the husk powder soaked in step (1), and after drying, calcining the husk powder at high temperature;

[0018] (3) The material calcined in step (2) is washed with a dilute hydrochloric acid solution, and then repeatedly washed with distilled water until the eluate is neutral, and then the material is dried to a constant weight, and then quickly ground and sieved to obtain activated carbon.

[0019] Preferably, in step S2, the stirring speed is 500 r / min and the stirring time is 30 min.

[0020] Preferably, in step S3, the hydrothermal reaction temperature is 140° C. and the hydrothermal reaction time is 18 h.

[0021] Preferably, in step S4, the drying temperature is 60° C. and the drying time is 4 hours.

[0022] Preferably, in step S4, the calcination temperature is 500° C. and the calcination time is 2 h.

[0023] Preferably, in step (1), the activator is one of H3PO4, ZnCl2, and KOH, the concentration of the activator is 10%-50%, and the immersion time is 24 hours.

[0024] Preferably, in step (2), the calcination temperature is 600° C. and the calcination time is 2 h; in step (3), the concentration of dilute hydrochloric acid is 5%, the drying temperature is 100° C., and the product is sieved through a 200-mesh sieve.

[0025] The invention also proposes the use of a bismuth-doped activated carbon-nickel oxide composite antibacterial agent as an antibacterial agent for Gram-positive bacteria and Gram-negative bacteria in a water environment.

[0026] Beneficial effects of the present invention:

[0027] 1. The present invention loads NiO in nanoparticle morphology on activated carbon, making it easier to separate and recover the composite antibacterial agent after use. At the same time, the adsorption properties of activated carbon are effectively utilized, so that the composite antibacterial agent has relatively rich antibacterial methods, thereby improving the applicability of the composite antibacterial agent.

[0028] 2. The present invention improves the negative impact of AC-loaded NiO on the antibacterial effect of NiO by doping Bi, while enhancing the magnetic properties of the composite antibacterial agent, improving the separation and recovery effect of the composite antibacterial agent after use, reducing the actual use cost of the composite antibacterial agent, and further avoiding secondary pollution of water bodies caused by chemical residues.

[0029] 3. The present invention uses macadamia nut shells as raw materials to prepare activated carbon. On the one hand, it realizes the recycling of macadamia nut shells and avoids the waste caused by direct disposal. On the other hand, the raw materials are widely available and easy to obtain, and the cost is relatively low.

[0030] 4. The composite antibacterial agent prepared by the present invention not only has a relatively obvious antibacterial effect on Gram-positive bacteria such as Escherichia coli and Staphylococcus aureus, Gram-negative bacteria, etc., but also exhibits an adsorption and degradation effect on organic dyes such as malachite green, methylene blue and methyl orange, and has a good comprehensive antibacterial effect.

[0031] 5. The composite antibacterial agent prepared by the present invention can achieve good antibacterial performance against the more complex bacterial environment in the water environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 These are SEM images of AC prepared by adding different activators according to the present invention, wherein ZnCl2 is added in (a), KOH is added in (b), and H3PO4 is added in (c).

[0033] Figure 2 3 and 4 are BET and BJH pore size distribution diagrams of AC prepared by adding different activators in the present invention, wherein Figure (a) is a nitrogen adsorption-desorption isotherm curve, and Figure (b) is a pore size distribution diagram.

[0034] Figure 3 These are SEM images of NiO with different morphologies, where (a) is a nanoparticle morphology, (b) is a flocculent morphology, (c) is a flake morphology, (d) is a flower-like morphology, (e) is a camellia-like morphology, and (f) is a spherical morphology.

[0035] Figure 4 It is a comparison chart of the antibacterial properties of NiO with different morphologies, where Figure (a) is the antibacterial effect diagram and Figure (b) is the antibacterial histogram.

[0036] Figure 5This is a comparison chart of the antibacterial properties of AC, NiO, and AC-NiO with different concentrations. The upper picture is the antibacterial effect chart, and the lower picture is the antibacterial effect histogram.

[0037] Figure 6 These are SEM and EDS images of the composite antibacterial agent of the present invention, wherein Figure (a) is the SEM image of the composite antibacterial agent of the present invention (magnified 10,000 times), Figure (b) is the SEM image of the composite antibacterial agent of the present invention (magnified 200,000 times), Figure (c) is the EDS image of the carbon element, Figure (d) is the EDS image of the nickel element, Figure (e) is the EDS image of the oxygen element, and Figure (f) is the EDS image of the bismuth element.

[0038] Figure 7 1 is an XPS spectrum diagram of the composite antibacterial agent of the present invention, wherein Figure (a) is the full XPS spectrum diagram, Figure (b) is the Ni 2p spectrum diagram, Figure (c) is the O1s spectrum diagram, and Figure (d) is the Bi 4f spectrum diagram.

[0039] Figure 8 It is the EPR spectrum diagram of AC-NiO and the composite antibacterial agent of the present invention.

[0040] Fig. 9 It is the ultraviolet diffuse reflection result diagram of AC-NiO and the composite antibacterial agent of the present invention, wherein the left diagram is the ultraviolet spectrum diagram and the right diagram is the band gap diagram.

[0041] Fig.10 It is a comparison chart of the antibacterial effects of other antibacterial agents and the composite antibacterial agent of the present invention, wherein Figure (a) is the inhibition zone of Escherichia coli, Figure (b) is the inhibition zone of Staphylococcus aureus, the middle figure is the antibacterial effect diagram, and the lower figure is the antibacterial effect histogram.

[0042] Fig.11 It is a graph showing the results of a cyclic antibacterial test of the composite antibacterial agent of the present invention, wherein the upper graph is a graph showing the results of a cyclic antibacterial test of Escherichia coli, and the lower graph is a graph showing the results of an antibacterial test of Staphylococcus aureus.

[0043] Fig.12 These are SEM images of the composite antibacterial agent of the present invention in contact with bacteria, wherein Figure (a) is a SEM image of untreated Escherichia coli, Figure (b) is a SEM image of Escherichia coli treated with the composite antibacterial agent of the present invention, Figure (c) is a SEM image of untreated Staphylococcus aureus, and Figure (d) is a SEM image of Staphylococcus aureus treated with the composite antibacterial agent of the present invention.

[0044] Fig.13 This is a diagram showing the antibacterial effect of the composite antibacterial agent of the present invention on Dianchi Lake water.

[0045] Fig.14The ultraviolet spectrum scanning diagrams of the composite antibacterial agent of the present invention in the adsorption and degradation of different dyes, wherein Figure (a) is malachite green dye, Figure (b) is methylene blue dye, and Figure (c) is methyl orange dye.

[0046] Fig.15 It is the magnetic result diagram of AC, AC-NiO and the composite antibacterial agent of the present invention. DETAILED DESCRIPTION

[0047] The present invention is further described in detail below in conjunction with specific embodiments.

[0048] In the examples and comparative examples of the present invention, chemical reagents not specifically described were all commercially available analytically pure for the experiments. Macadamia nut shells used in the examples and comparative examples of the present invention were produced in Lincang, Yunnan.

[0049] Example 1

[0050] In this embodiment, activated carbon is prepared by the following steps:

[0051] (1) Wash the macadamia shells, dry and crush them, then take 3g of shell powder and mix it evenly with 10ml of 10% ZnCl2 and soak it for 24h.

[0052] (2) The husk powder soaked in step (1) is vacuum filtered, and after being dried, the husk powder is calcined at 600° C. for 2 h.

[0053] (3) The material calcined in step (2) is washed with a 5% dilute hydrochloric acid solution, and then repeatedly washed with distilled water until the eluate is neutral (pH = 6-7), and then the material is dried to constant weight at 100°C, and then quickly ground and passed through a 200-mesh sieve to obtain activated carbon.

[0054] In this embodiment, the composite antibacterial agent is prepared by the following steps:

[0055] S1: Weigh 0.24g NiCl2·6H2O and dissolve it in 25ml ethanol to form a green transparent solution, weigh 1.46g sodium acetate and dissolve it in 10ml distilled water, weigh 0.59g trisodium citrate and dissolve it in 15ml distilled water;

[0056] S2: The three solutions obtained in step S2 are mixed and stirred at a speed of 500 r / min to obtain a transparent solution after stirring for 30 minutes, and 0.5 g of activated carbon powder and 0.2 g of Bi(NO3)3·5H2O are added to the transparent solution to obtain a mixed solution;

[0057] S3: subjecting the mixed solution obtained in step S3 to a sealed hydrothermal reaction at 140° C., reacting for 18 hours and then naturally cooling to room temperature to obtain a blue-green product;

[0058] S4: Wash the blue-green product obtained in step S3 with deionized water for 5 times, and then wash the blue-green product obtained in step S4 with ethanol for 5 times, and then dry the product at 60°C. After drying for 4 hours, calcine the product at 500°C for 2 hours to obtain a bismuth-doped activated carbon-nickel oxide composite antibacterial agent.

[0059] The SEM image of the activated carbon (AC) prepared in this example is as follows Figure 1 (a) is shown. The BET and BJH pore size distribution diagrams of AC are shown in Figure 2 In the obtained composite antibacterial agent, nickel oxide is in the form of nanoparticles, as shown in Figure 3 (a) shown.

[0060] pass Figure 1 (a) It can be seen that AC activated by ZnCl2 shows a larger pore structure and the AC surface is relatively smooth. Although the effect of ZnCl2 activation on regulating pore formation is not obvious, it has an obvious effect on deep pore formation.

[0061] pass Figure 2 (a) It can be seen that the adsorption isotherm of the ZnCl2 activator is type I, without obvious hysteresis loop, indicating that the activated carbon prepared in this example contains a relatively high microporous structure.

[0062] Example 2

[0063] This embodiment adopts the same method as that of embodiment 1 to prepare the composite antibacterial agent, except that: in this embodiment, the activator is KOH, and the concentration of the activator is 50%.

[0064] The SEM image of the activated carbon (AC) prepared in this example is as follows Figure 1 (b) The BET and BJH pore size distribution diagrams of AC are shown in Figure 2 In the obtained composite antibacterial agent, nickel oxide is in the form of nanoparticles, as shown in Figure 3 (a) shown.

[0065] pass Figure 1 (b) It can be seen that the pores of AC activated by KOH are dense and evenly distributed.

[0066] pass Figure 2 (a) It can be seen that the adsorption isotherm with KOH as the activator is type I with no obvious hysteresis loop, indicating that the activated carbon contains a high microporous structure.

[0067] Example 3

[0068] This embodiment adopts the same method as that of embodiment 1 to prepare the composite antibacterial agent, except that: in this embodiment, the activator is H3PO4, and the concentration of the activator is 35%.

[0069] The SEM image of the activated carbon (AC) prepared in this example is as follows Figure 1 (c) The BET and BJH pore size distribution diagrams of AC are shown in Figure 2 In the obtained composite antibacterial agent, nickel oxide is in the form of nanoparticles, as shown in Figure 3 The SEM and EDS images of the AC-NiO / Bi composite antibacterial agent prepared in this embodiment are shown in FIG. Figure 6 The XPS image is shown in Figure 7 The EPR spectrum is shown in Figure 8 The UV diffuse reflection result is shown in the figure below. Fig. 9 The antibacterial effect on Escherichia coli and Staphylococcus aureus is shown in Fig.10 The antibacterial effect of the cycle is shown in Fig.11 The SEM image of the contact with bacteria is shown in Fig.12 Its antibacterial effect on Dianchi Lake water is shown in Fig.13 Its adsorption and degradation performance for dye-related pollutants is shown in Fig.14 Its magnetic results are shown in Fig.15 shown.

[0070] pass Figure 1 (c) It can be seen that the AC activated by H3PO4 presents an irregular shape, a loose surface structure, and clearly visible pores.

[0071] pass Figure 2 (a) It can be seen that the adsorption isotherm of the activated carbon obtained with H3PO4 as the activating agent is type II, indicating that macroporous adsorption is the main process in the adsorption process, indicating that the activated carbon contains a macroporous structure.

[0072] pass Figure 1 as well as Figure 2 (a) It can be seen that all three activators can activate AC and produce a porous structure. However, the activated carbon activated by H3PO4 has the largest specific surface area of ​​1039.32 m 2 / g, with a total pore volume of 1.43 cm 2 / g; followed by ZnCl2 activated carbon, which has a specific surface area of ​​315.12m 2 / g, and the total pore volume is 0.33cm 2 / g; the surface area and total pore volume of KOH-activated activated carbon are the lowest, which are 162.57m 2 / g,0.19cm 2 / g. By Figure 2(b) The specific surface area and total pore volume of AC activated by three different activators show that the average pore sizes of activated carbon activated by H3PO4, ZnCl2, and KOH are 2.8nm, 1.9nm, and 2.3nm, respectively. Among the three activators, H3PO4 shows obvious advantages over the other two in terms of specific surface area, total volume, and average pore size, which is beneficial to improving the antibacterial effect. At the same time, AC prepared with H3PO4 as the activator has the highest yield and is inexpensive. Considering the comprehensive factors of the construction of antibacterial materials, H3PO4 as an activator is the best choice for the preparation of macadamia shell activated carbon.

[0073] pass Figure 6 (a) and (b) show that there are many metal particles dispersed in the randomly dispersed pore structure of activated carbon. The metal particles are NiO, indicating that AC and NiO are successfully combined. Figure 6 (cf) It can be seen that C, Ni, O, and Bi elements are well dispersed on the surface of the material, confirming the successful incorporation of Bi.

[0074] pass Figure 7 (a) It can be seen that Bi 4f, Bi 4d and O1s states exist in the AC-NiO / Bi composite antibacterial agent prepared by the present invention; Figure 7 (b) It can be seen that Figure 7 There are five peaks in (b), among which the peaks at 853.6 eV and 872.4 eV are attributed to the surface Ni 2+ In addition, three satellite peaks (Sat1 and Sat2) were identified at 855.4, 861.8 and 879.3 eV, which were attributed to the paramagnetic Ni 2+ After adding Bi, the binding energy changes slightly. The presence of Bi weakens the Ni-O bond and facilitates the formation of surface oxygen vacancies. Figure 7 (c) Three peaks appear in O 1s, of which 529.2 eV is attributed to the lattice oxygen of Ni-O, and 531.2 eV is attributed to the oxygen vacancies adsorbed on the surface of the material. The binding energy in O1s remains basically unchanged after doping with Bi. Figure 7 The binding energies of 163.9 eV and 158.6 eV in (d) coincide with the peaks of Bi 4f7 / 2 and Bi 4f5 / 2, respectively, indicating that Bi exists in a trivalent form. Figure 7 (ab) It can be seen that Bi is successfully doped, and the change in binding energy caused by Bi doping is conducive to the formation of surface oxygen vacancies, thereby improving the antibacterial performance.

[0075] pass Fig.11It can be seen that after four cycles, the antibacterial rate of the composite antibacterial agent of the present invention against Escherichia coli dropped to 74.89%, a decrease of 24.61%, and an average decrease of only about 6% per cycle, and the antibacterial rate against Staphylococcus aureus dropped to 69.84%, a decrease of 28.6%, and an average decrease of only about 7% per cycle. Although the antibacterial rate of the composite antibacterial agent of the present invention decreased to a certain extent during the cycle, the decrease was small, indicating that the composite antibacterial agent of the present invention has good stability and good reusability.

[0076] pass Fig.12 It can be seen that the composite antibacterial agent of the present invention can effectively destroy the bacterial cell structure, thereby achieving the antibacterial purpose.

[0077] Fig.13 In the antibacterial experiment, water from Dianchi Lake in Kunming City, Yunnan Province was used for antibacterial experiments. After 24 hours of culture, a variety of bacteria (such as Fig.13 As shown in the left figure), after adding the composite antibacterial agent of the present invention to the culture medium, more than 99% of the bacteria in the water can be removed (such as Fig.13 As shown in the right figure), it shows that the composite antibacterial agent of the present invention not only has excellent antibacterial properties against Escherichia coli and Staphylococcus aureus, but also can achieve excellent antibacterial effects when there are more complex bacterial types in the water environment.

[0078] pass Fig.14 It can be seen that the composite antibacterial agent prepared by the present invention also has significant adsorption and degradation performance for dye pollutants such as malachite green, methylene blue and methyl orange.

[0079] Comparative Example 1

[0080] This comparative example prepares nickel oxide with flocculent morphology (such as Figure 3 (b)), and the antibacterial properties of nickel oxide were tested, and the results are shown in Figure (4).

[0081] Comparative Example 2

[0082] This comparative example prepares nickel oxide with a flake morphology (such as Figure 3 (c)), and the antibacterial properties of nickel oxide were tested, and the results are shown in Figure (4).

[0083] Comparative Example 3

[0084] This comparative example prepares nickel oxide with a flower-shaped morphology (such as Figure 3 (d)), and the antibacterial properties of nickel oxide were tested, and the results are shown in Figure (4).

[0085] Comparative Example 4

[0086] This comparative example prepares nickel oxide with a camellia-like morphology (such as Figure 3(e)), and the antibacterial properties of nickel oxide were tested, and the results are shown in Figure (4).

[0087] Comparative Example 5

[0088] This comparative example prepares spherical nickel oxide (such as Figure 3 (f)), and the antibacterial properties of nickel oxide were tested, and the results are shown in Figure (4).

[0089] pass Figure 4 It can be seen that the nano-particle NiO has higher antibacterial activity than other morphologies, and the inactivation rate of Escherichia coli can reach 99.73%. Therefore, the nano-morphology of nickel oxide helps to improve the antibacterial effect of the composite antibacterial agent prepared by the present invention.

[0090] Comparative Example 6

[0091] This comparative example adopts the same method as Example 1 to prepare the composite antibacterial agent, except that Bi is not doped in this comparative example.

[0092] After the composite antibacterial agent in this comparative example was prepared into antibacterial liquids of different concentrations, an antibacterial effect experiment was conducted. For example, an antibacterial liquid with a concentration of 50 μg / ml was prepared by adding 50 μg of the antibacterial agent in this comparative example to 1 ml of water. The antibacterial effect of the composite antibacterial agent prepared in this comparative example is shown in FIG. Figure 5 As shown, the EPR spectrum is Figure 8 As shown, the UV diffuse reflection results are as follows Fig. 9 As shown in Figure 2, the antibacterial effect on E. coli (Escherichia coli) and S. aureus (Staphylococcus aureus) is as follows: Fig.10 The magnetic test results are shown in Fig.15 shown.

[0093] Oxygen vacancies can not only provide sufficient adsorption sites to adsorb O2, but also act as active sites to activate O2 to produce more O 2 – , and is conducive to the separation of photogenerated carriers, thereby generating more ROS to enhance the antibacterial properties of the material. Figure 8 It can be seen that both AC-NiO and AC-NiO / Bi have paramagnetic resonance signals at g = 2.003, indicating that both antibacterial agents have oxygen vacancies. At the same time, compared with AC-NiO, the oxygen vacancy signal of AC-NiO / Bi sample is enhanced, indicating that the incorporation of Bi promotes the generation of more surface oxygen vacancies, thereby improving the antibacterial properties of the material.

[0094] pass Fig. 9 It can be seen that after doping with Bi, the band gap of the composite antibacterial agent of the present invention is significantly reduced, and the recombination rate of photogenerated carriers is slowed down, which is beneficial to improving the antibacterial performance of the composite antibacterial agent of the present invention.

[0095] Comparative Example 7

[0096] In this comparative example, AC was used as an antibacterial agent to prepare antibacterial solutions of different concentrations for antibacterial effect experiments.

[0097] The antibacterial effect of the antibacterial agent in this comparative example is as follows Figure 5 As shown in Figure 2, the antibacterial effect on E. coli (Escherichia coli) and S. aureus (Staphylococcus aureus) is as follows: Fig.10 The magnetic test results are shown in Fig.15 shown.

[0098] pass Fig.10 It can be seen that the AC antibacterial agent did not show an inhibition zone for the two bacteria, indicating that AC had no ion dissolution and had poor antibacterial performance. The composite antibacterial agent of the present invention has a significant inhibition zone for both bacteria. AC-NiO has the largest inhibition width, with the inhibition zone widths for E. coli and S. aureus being 15.31 mm and 18.43 mm, respectively. AC-NiO / Bi is slightly lower than AC-NiO, with the inhibition zone widths for E. coli and S. aureus being 13.24 mm and 14.71 mm, respectively. This indicates that after doping with Bi, the dissolution of antibacterial agent ions is reduced, and the specific gravity of the ion sterilization portion is reduced, thereby enhancing the safety of the material. At the same time, by Fig.10 It can also be seen that under the same antibacterial liquid concentration (300 μg), the antibacterial rates of AC-NiO against E. coli and S. aureus were 66.87% and 44.22%, respectively, while the antibacterial rates of the composite antibacterial agent of the present invention reached 98.77% and 78.90%, and the antibacterial rate was significantly improved. At the same time, after NiO was combined with AC, the antibacterial rate of AC-NiO decreased more than that of NiO, and after doping with Bi, the antibacterial rate of the composite antibacterial agent was significantly improved, and was higher than that of NiO, indicating that doping with Bi can not only make up for the decrease in the antibacterial rate caused by the combination of NiO and AC, but also promote the further improvement of the antibacterial rate of the composite antibacterial agent.

[0099] pass Fig.15 It can be seen that the composite antibacterial agent of the present invention has the best magnetism, which is conducive to the recycling of the composite antibacterial agent of the present invention.

[0100] Comparative Example 8

[0101] In this comparative example, NiO was used as an antibacterial agent to prepare antibacterial solutions of different concentrations for antibacterial effect experiments.

[0102] The antibacterial effect of the antibacterial agent in this comparative example is as follows Figure 5 shown.

[0103] pass Figure 5It can be seen that when the concentration of the antibacterial liquid increases from 50μg / ml to 400μg / ml, the antibacterial rates of NiO are 14.12%, 30.45%, 34.75%, 94.10%, and 94.38% respectively; the antibacterial rates of AC-NiO are 20.30%, 21.15%, 40.13%, 61.04%, and 69.83% respectively. When the concentration of NiO antibacterial liquid increases from 200μg / ml to 300μg / ml, its antibacterial rate is greatly improved, and when the concentration is increased to 400μg / ml, its antibacterial rate is not improved much, indicating that the appropriate concentration of NiO antibacterial liquid is 300μg / ml. At 300μg / ml, the combination of NiO and AC will cause the antibacterial rate of NiO to decrease significantly, thus resulting in poor comprehensive performance of the antibacterial agent.

[0104] In summary, the AC-NiO / Bi composite antibacterial agent in the present invention has excellent antibacterial properties, and also has relatively excellent adsorption and degradation properties for dye-type pollutants, and also has good recovery and safety. The composite antibacterial agent of the present invention is used in water environment treatment, which can effectively remove water environmental pollutants and harmful substances, and at the same time has high removal safety and low comprehensive cost. The composite antibacterial agent of the present invention has high applicability.

[0105] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A method for preparing a doped activated carbon-nickel oxide composite antibacterial agent, characterized in that: The composite antibacterial agent is doped with bismuth element, and the activated carbon is loaded with nickel oxide in nanoparticle morphology. The preparation method comprises the following steps: S1: Weigh 0.24g NiCl2·6H2O and dissolve it in 25ml ethanol to form a green transparent solution, weigh 1.46g sodium acetate and dissolve it in 10ml distilled water, weigh 0.59g trisodium citrate and dissolve it in 15ml distilled water; S2: The three solutions obtained in step S1 are mixed and stirred to obtain a transparent solution, and 0.5 g of activated carbon powder and 0.2 g of Bi(NO3)3·5H2O are added to the transparent solution to obtain a mixed solution; S3: performing a sealed hydrothermal reaction treatment on the mixed solution obtained in step S2, and then naturally cooling it to room temperature to obtain a blue-green product; S4: washing the blue-green product obtained in step S3 with deionized water for 5 times, and then washing the blue-green product obtained in step S3 with ethanol for 5 times, and then drying the product, and calcining it to obtain a bismuth-doped activated carbon-nickel oxide composite antibacterial agent.

2. The method for preparing a doped activated carbon-nickel oxide composite antibacterial agent according to claim 1, characterized in that: The activated carbon is prepared by the following steps: (1) Wash the macadamia shells, dry and crush them, then take 3g of shell powder and mix it evenly with 10ml of activator and soak it for a certain period of time; (2) vacuum filtering the husk powder soaked in step (1), and after drying, calcining the husk powder at high temperature; (3) The material calcined in step (2) is washed with a dilute hydrochloric acid solution, and then repeatedly washed with distilled water until the eluate is neutral, and then the material is dried to a constant weight, and then quickly ground and sieved to obtain activated carbon.

3. The method for preparing a doped activated carbon-nickel oxide composite antibacterial agent according to claim 1, characterized in that: In step S2, the stirring speed is 500 r / min and the stirring time is 30 min.

4. The method for preparing a doped activated carbon-nickel oxide composite antibacterial agent according to claim 1, characterized in that: In step S3, the hydrothermal reaction temperature is 140° C. and the hydrothermal reaction time is 18 h.

5. The method for preparing a doped activated carbon-nickel oxide composite antibacterial agent according to claim 1, characterized in that: In step S4, the drying temperature is 60° C. and the drying time is 4 hours.

6. The method for preparing a doped activated carbon-nickel oxide composite antibacterial agent according to claim 1, characterized in that: In the step S4, the calcination temperature is 500° C. and the calcination time is 2 hours.

7. The method for preparing a doped activated carbon-nickel oxide composite antibacterial agent according to claim 2, characterized in that: In the step (1), the activator is one of H3PO4, ZnCl2, and KOH, the concentration of the activator is 10%-50%, and the immersion time is 24 hours.

8. The method for preparing a doped activated carbon-nickel oxide composite antibacterial agent according to claim 2, characterized in that: In the step (2), the calcination temperature is 600° C. and the calcination time is 2 h. In the step (3), the concentration of dilute hydrochloric acid is 5%, the drying temperature is 100° C., and the product is sieved through a 200-mesh sieve.

9. Use of the bismuth-doped activated carbon-nickel oxide composite antibacterial agent prepared by the preparation method according to any one of claims 1 to 8 as an antibacterial agent for Gram-positive bacteria and Gram-negative bacteria in aquatic environments.