A supported catalyst and preparation method thereof, and a method for producing ammonia and denitrification from urea

The supported catalyst is prepared by the ion exchange method and combined with the catalytic hydrolysis method to solve the efficiency problem of the SCR catalyst in high temperature and high SO2 environments, achieving efficient degradation of nitrogen oxides and cost reduction.

CN118384913BActive Publication Date: 2024-10-18INNER MONGOLIA JINGNENG KANGBASHI THERMAL POWER CO LTD +1

Patent Information

Application Number
CN202410810808.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-18
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing SCR catalysts have low catalytic efficiency at 300-400°C and are easily affected by the aging of sulfur dioxide, making it difficult to achieve efficient degradation of nitrogen oxides.

Method used

The zeolite carrier is loaded with zirconium, cerium, and gallium elements using the ion exchange method. The supported catalyst is prepared through multiple ion exchange and roasting treatments, and combined with the catalytic hydrolysis method to prepare ammonia gas, which is used in the urea-to-ammonia denitrification method in the SCR catalytic unit.

Benefits of technology

It achieves a catalytic efficiency of more than 95%, reducing costs, and the supported catalyst maintains catalytic efficiency under high temperature and high SO2 environments, effectively degrading nitrogen oxides in flue gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118384913B_ABST
    Figure CN118384913B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of new materials, and discloses a method for preparing a supported catalyst, comprising the following steps: step 11: placing zeolite powder in a soluble zirconium salt solution to obtain a first powder; step 12: placing the first powder in a soluble cerium salt solution to obtain a second powder; step 13: repeating steps 1 and 2 to obtain a third powder; step 14: placing the third powder in a soluble gallium salt solution to obtain a fourth powder; step 15: preparing the fourth powder into a slurry, and obtaining a supported catalyst through molding and calcination. The method of the present invention can achieve a catalytic efficiency of more than 95% at 300-400°C by ion exchange and zeolite carrier loading zirconium, cerium and gallium elements. At the same time, the present invention also discloses a supported catalyst and a preparation method thereof, and a method for denitrification of urea to produce ammonia.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new materials, and in particular to a supported catalyst and a preparation method thereof, and a method for producing ammonia from urea and denitrification. Background Art

[0002] Before 2023, the applicant used liquid ammonia as the ammonia source to react with nitrogen oxides in the SCR reactor, but liquid ammonia has the risk of flammability and leakage. Based on comprehensive considerations, the applicant modified the currently permitted denitrification system.

[0003] In the early stage of transformation, the catalytic hydrolysis method was selected through comparison of the three major ammonia production processes; at the same time, the early delayed emission system was transformed into ultra-low emission system, the boiler was equipped with a low-nitrogen burner, and the SCR inlet NO x The concentration is greatly reduced, basically not exceeding 250mg / Nm 3 (Standard state, dry basis, 6% O2).

[0004] In the subsequent transformation, the focus is on two aspects: one is the optimization of the ammonia production process, and the other is the optimization of the SCR catalytic process. For SCR catalysis, there are many factors that restrict the catalytic efficiency, such as the mixing uniformity of flue gas and ammonia, the catalytic activity of the catalyst, etc.

[0005] The technical problem to be solved in this case is: how to improve the SCR catalytic effect. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing a supported catalyst. The method of the present invention can achieve a catalytic efficiency of more than 95% at 300-400°C by loading zirconium, cerium and gallium on a zeolite carrier through an ion exchange method.

[0007] To achieve the above object, the present invention provides the following technical solution: A method for preparing a supported catalyst, comprising the following steps: Step 11: placing zeolite powder in a soluble zirconium salt solution, performing ion exchange for 12 to 24 hours at 50 to 90° C. with stirring, and then filtering, washing, and drying to obtain a first powder;

[0008] Step 12: placing the first powder in a soluble cerium salt solution, performing ion exchange at 50 to 90° C. for 12 to 24 hours with stirring, and then filtering, washing, and drying to obtain a second powder;

[0009] Step 13: Repeat step 1 and step 2 to obtain a third powder;

[0010] Step 14: placing the third powder in a soluble gallium salt solution, performing ion exchange at 50 to 90° C. for 12 to 24 hours with stirring, and then filtering, washing, and drying to obtain a fourth powder;

[0011] Step 15: preparing the fourth powder into a slurry, and performing molding and calcination to obtain a supported catalyst;

[0012] The concentration of metal ions in the soluble zirconium salt solution and the soluble cerium salt solution is 0.15-0.3 mol / L;

[0013] The concentration of metal ions in the soluble gallium salt solution is 0.05-0.1 mol / L.

[0014] In the above-mentioned method for preparing a supported catalyst, in step 15, the calcination temperature is 500-700° C., the calcination atmosphere is oxygen calcination, and the calcination time is 3-5 hours.

[0015] In the above-mentioned method for preparing a supported catalyst, in step 11 to step 13, the ratio of the powder added to each solution is 50-100 g / L.

[0016] In the above-mentioned method for preparing a supported catalyst, the zeolite in the supported catalyst is 3A molecular sieve, 4A molecular sieve or 5A molecular sieve.

[0017] Meanwhile, the present invention also discloses a supported catalyst, which is prepared by any of the above methods.

[0018] Finally, the present invention also discloses a method for producing ammonia from urea and denitrification, the method comprising the following steps:

[0019] Step 1: using urea as a raw material to prepare ammonia by catalytic hydrolysis;

[0020] Step 2: The ammonia obtained in step 1 is mixed with the dilution air and then mixed with the flue gas, and then enters the SCR catalytic unit for catalytic denitration;

[0021] In the step 1, the catalyst used is ammonium dihydrogen phosphate;

[0022] In step 2, the catalyst used in the SCR catalytic unit is the supported catalyst as described above; the flue gas temperature is 368±3°C under stable working conditions; the sulfur dioxide content is 0.04-0.06 vol%; the nitrogen oxide content in the flue gas is 200-300 mg / Nm 3 .

[0023] In the above-mentioned urea-to-ammonia denitrification method, in step 1, the pressure of the catalytic hydrolysis method is 0.5 MPa, the temperature is 130-140° C., the concentration of urea in the solution is 40-55wt%; and the ammonia concentration in the gas after hydrolysis is controlled to be 35-40vol%.

[0024] In the above-mentioned urea-to-ammonia denitrification method, the temperature of the dilution air is 200-220° C. The dilution air dilutes the ammonia gas to an ammonia concentration of 5 vol% or less;

[0025] The ammonia gas and the dilution air are mixed in the ammonia-air mixing unit, and the dilution air is heated by a first heat exchanger, which is located inside the outlet end of the SCR catalytic unit, and the inlet of the tube side of the heat exchanger is connected to a blower.

[0026] In the above-mentioned urea-to-ammonia denitrification method, an ammonia injection unit and a catalyst layer are provided in the SCR catalytic unit; the catalyst layer is filled with a loaded catalyst; the channel on the inlet side of the SCR catalytic unit is divided into a plurality of fine channels by a partition; there are a plurality of ammonia injection units, each of which corresponds to a fine channel and is located inside the fine channel; the ammonia injection unit includes an ammonia-air mixed gas input pipe connected to the ammonia-air mixing unit, and a plurality of first nozzles connected to the ammonia-air mixed gas input pipe; the first nozzle includes an output pipe and a conical head located at the output end of the output pipe; the tip of the conical head extends to the inside of the output pipe, and a gap is left between the conical head and the output pipe; the conical head and the output pipe are connected by a connecting plate; the connecting plate extends to the edge of the conical head; adjacent connecting plates constitute a gas flow channel; the diameter of the thick end of the conical head is larger than the diameter of the output pipe; the direction from the tip of the conical head to the thick end of the conical head is the direction of flue gas flow.

[0027] In the above-mentioned urea-to-ammonia denitrification method, the diameter of the thick end of the conical head is 1.8-2.2 times the diameter of the output pipe; each ammonia injection unit includes 9 first nozzles; the 9 first nozzles are arranged in a 3×3 form; in the direction of flue gas flow, the middle first nozzle is located behind the remaining first nozzles; the cross-sectional dimensions of the fine channel are 1.45m×2.5m; the diameter of the thick end of the first nozzle is 5cm; the width of the gap is 8-10mm; and the cross-section of the conical head is an equilateral triangle.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. The present invention uses an ion exchange method and a zeolite carrier to load zirconium, cerium and gallium elements, and can achieve a catalytic efficiency of more than 95% at 300-400°C;

[0030] 2. The present invention uses zeolite as a carrier, which reduces its cost by 90% compared with SSZ-13 molecular sieve. At the same time, through the optimization of metal ions, it achieves a catalytic effect similar to that of SSZ-13 molecular sieve loaded with metal ions.

[0031] 3. The supported catalyst of the present invention is resistant to sulfur dioxide aging, and can maintain substantially unchanged catalytic efficiency after an aging test at 500 ppm SO2, 368°C, and 240 h.

[0032] 4. The present invention achieves degradation of nitrogen oxides in flue gas by producing ammonia by catalytic hydrolysis and reducing nitrogen oxides by loading catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a structural schematic diagram of system embodiment 1 of the present invention;

[0034] Figure 2 It is a schematic structural diagram of the SCR catalytic unit of system embodiment 1 of the present invention;

[0035] Figure 3 for Figure 2 EE cross-sectional view;

[0036] Figure 4 It is a front view of the ammonia injection unit of system embodiment 1 of the present invention;

[0037] Figure 5 A three-dimensional diagram of a first nozzle of system embodiment 1 of the present invention;

[0038] Figure 6 It is a front view of the first nozzle of the system embodiment 1 of the present invention;

[0039] Figure 7 An axial cross-sectional view of a first nozzle of system embodiment 1 of the present invention;

[0040] Figure 8 It is a structural schematic diagram of an ammonia-air mixing unit of system embodiment 1 of the present invention;

[0041] Fig. 9 is a cross-sectional view of the first nozzle of system comparative example 1;

[0042] Fig.10 A three-dimensional diagram of the first nozzle of system comparative example 1;

[0043] Fig.11 is a cross-sectional view of the first nozzle of system comparative example 2;

[0044] Fig.12 is a cross-sectional view of the first nozzle of system comparative example 3;

[0045] The symbols in the accompanying drawings are:

[0046] 1. Urea hydrolysis unit; 2. Ammonia-air mixing unit; 3. SCR catalytic unit; 4. Ammonia injection unit; 5. Urea solution tank; 6. Sensor; 7. Heat exchanger; 8. Blower; 11. Urea hydrolyzer; 12. Urea solution inlet pipe; 13. Catalyst solution inlet pipe; 14. Waste liquid discharge pipe; 15. Discharge port; 21. Diffuser; 22. Ammonia inlet pipe; 23. Throat; 24. Guide plate; 31. Partition plate; 32. Fine channel; 41. Ammonia-air mixture inlet pipe; 42. Output pipe; 43. Conical head; 44. Gap; 45. Connecting plate; 46. Control valve; C. First guide plate; A. Plug; B. First connecting plate. DETAILED DESCRIPTION

[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Part I Preparation of supported catalysts

[0049] Example 1

[0050] Step 1: Use 1000g of 4A molecular sieve powder (silicon-aluminum ratio is 2) for later use;

[0051] Step 2: prepare 0.2 mol / L zirconium nitrate solution, 0.2 mol / L cerium nitrate solution, and 0.08 mol / L gallium nitrate solution;

[0052] Step 3: Disperse 1000g of 4A molecular sieve powder into 10L of zirconium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain a first powder;

[0053] Step 4: Disperse the first powder into 10L of cerium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain the second powder.

[0054] Step 5: Repeat steps 3 and 4 to obtain a third powder;

[0055] Step 6: placing the third powder in 10 L of gallium nitrate solution, reacting at 60° C. and 70 r / min for 24 h, then filtering, washing, and drying to obtain a fourth powder;

[0056] Step 7: Mix 100 g of the fourth powder, 5 g of glass fiber, 1 g of carboxymethyl cellulose, and 30 g of water, place them in a mold and press them into the desired shape (when used in the SCR catalytic unit, press them into a structure with a square shape and a honeycomb inner pore), and bake them at 650°C in air atmosphere for 4 hours.

[0057] Example 2

[0058] The method is substantially the same as Example 1, except that the concentrations of the zirconium nitrate solution and the cerium nitrate solution are 0.3 mol / L, and the concentration of the gallium nitrate solution is 0.1 mol / L.

[0059] Example 3

[0060] The method is substantially the same as Example 1, except that the concentrations of the zirconium nitrate solution and the cerium nitrate solution are 0.15 mol / L, and the concentration of the gallium nitrate solution is 0.05 mol / L.

[0061] Example 4

[0062] The method is substantially the same as Example 1, except that the order of using zirconium nitrate and cerium nitrate is reversed; the details are as follows:

[0063] Step 1: Use 1000g of 4A molecular sieve powder (silicon-aluminum ratio is 2) for later use;

[0064] Step 2: prepare 0.2 mol / L zirconium nitrate solution, 0.2 mol / L cerium nitrate solution, and 0.08 mol / L gallium nitrate solution;

[0065] Step 3: Disperse 1000g of 4A molecular sieve powder into 10L of cerium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain a first powder;

[0066] Step 4: Disperse the first powder into 10L zirconium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain the second powder.

[0067] Step 5: Repeat steps 3 and 4 to obtain a third powder;

[0068] Step 6: placing the third powder in 10 L of gallium nitrate solution, reacting at 60° C. and 70 r / min for 24 h, then filtering, washing, and drying to obtain a fourth powder;

[0069] Step 7: Mix 100 g of the fourth powder, 5 g of glass fiber, 1 g of carboxymethyl cellulose, and 30 g of water, place them in a mold and press them into the desired shape (when used in the SCR catalytic unit, press them into a structure with a square shape and a honeycomb inner pore), and bake them at 650°C in air atmosphere for 4 hours.

[0070] Example 5

[0071] The method is similar to Example 1, except that the use of gallium nitrate is placed in the first step of the entire preparation process; the details are as follows:

[0072] Step 1: Use 1000g of 4A molecular sieve powder (silicon-aluminum ratio is 2) for later use;

[0073] Step 2: prepare 0.2 mol / L zirconium nitrate solution, 0.2 mol / L cerium nitrate solution, and 0.08 mol / L gallium nitrate solution;

[0074] Step 3: Disperse 1000g of 4A molecular sieve powder into 10L of gallium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain a first powder;

[0075] Step 4: Disperse the first powder into 10L zirconium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain the second powder.

[0076] Step 5: Disperse the second powder into 10L of cerium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain a third powder.

[0077] Step 6: Repeat steps 4 and 5 to obtain a fourth powder;

[0078] Step 7: Mix 100 g of the fourth powder, 5 g of glass fiber, 1 g of carboxymethyl cellulose, and 30 g of water, place them in a mold and press them into the desired shape (when used in the SCR catalytic unit, press them into a structure with a square shape and a honeycomb inner pore), and bake them at 650°C in air atmosphere for 4 hours.

[0079] Comparative Example 1

[0080] Step 1: Use 1000g of 4A molecular sieve powder (silicon-aluminum ratio is 2) for later use;

[0081] Step 2: prepare 0.2 mol / L zirconium nitrate solution and 0.2 mol / L cerium nitrate solution;

[0082] Step 3: Disperse 1000g of 4A molecular sieve powder into 10L of zirconium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain a first powder;

[0083] Step 4: Disperse the first powder into 10L of cerium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain the second powder.

[0084] Step 5: Repeat steps 3 and 4 to obtain a third powder;

[0085] Step 6: Mix 100 g of the third powder, 5 g of glass fiber, 1 g of carboxymethyl cellulose and 30 g of water, place in a mold and press into the desired shape (when used in the SCR catalytic unit, press into a structure with a square shape and a honeycomb inner hole), and bake at 650°C in air atmosphere for 4 hours.

[0086] Comparative Example 2

[0087] Step 1: Use 1000g of 4A molecular sieve powder (silicon-aluminum ratio is 2) for later use;

[0088] Step 2: prepare 0.2 mol / L zirconium nitrate solution, 0.2 mol / L cerium nitrate solution, and 0.08 mol / L yttrium nitrate solution;

[0089] Step 3: Disperse 1000g of 4A molecular sieve powder into 10L of zirconium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain a first powder;

[0090] Step 4: Disperse the first powder into 10L of cerium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain the second powder.

[0091] Step 5: Repeat steps 3 and 4 to obtain a third powder;

[0092] Step 6: placing the third powder in 10 L of yttrium nitrate solution, reacting at 60° C. and 70 r / min for 24 h, then filtering, washing, and drying to obtain a fourth powder;

[0093] Step 7: Mix 100 g of the fourth powder, 5 g of glass fiber, 1 g of carboxymethyl cellulose, and 30 g of water, place them in a mold and press them into the desired shape (when used in the SCR catalytic unit, press them into a structure with a square shape and a honeycomb inner pore), and bake them at 650°C in air atmosphere for 4 hours.

[0094] Comparative Example 3

[0095] Step 1: Use 1000g of 4A molecular sieve powder (silicon-aluminum ratio is 2) for later use;

[0096] Step 2: prepare 0.2 mol / L zirconium nitrate solution, 0.2 mol / L cerium nitrate solution, and 0.08 mol / L praseodymium nitrate solution;

[0097] Step 3: Disperse 1000g of 4A molecular sieve powder into 10L of zirconium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain a first powder;

[0098] Step 4: Disperse the first powder into 10L of cerium nitrate solution, stir at 70r / min at 60°C, and react for 24h. After the reaction, filter, wash, and dry to obtain the second powder.

[0099] Step 5: Repeat steps 3 and 4 to obtain a third powder;

[0100] Step 6: placing the third powder in 10 L of praseodymium nitrate solution, reacting at 60° C. and 70 r / min for 24 h, then filtering, washing, and drying to obtain a fourth powder;

[0101] Step 7: Mix 100 g of the fourth powder, 5 g of glass fiber, 1 g of carboxymethyl cellulose, and 30 g of water, place them in a mold and press them into the desired shape (when used in the SCR catalytic unit, press them into a structure with a square shape and a honeycomb inner pore), and bake them at 650°C in air atmosphere for 4 hours.

[0102] Performance Testing

[0103] NOx conversion efficiency test

[0104] The products of Examples 1-5 and Comparative Examples 1-3 were tested for nitrogen oxide conversion efficiency in a fixed bed reactor.

[0105] The simulated gas composition during the test was: NO = NH3 = 300ppm, O2 = 6%, H2O = 9.4%, N2 as the balance gas, and the air velocity was 40000h -1, the reaction temperature is 200-450°C; the gas components are all detected by infrared.

[0106] The conversion efficiency of nitrogen oxides can be found in Table 1:

[0107] Table 1 Unit %

[0108] 200℃ 250℃ 300℃ 350℃ 400℃ 450℃ Example 1 83.5 84.1 89.5 96.1 98.5 92.5 Example 2 84 86.4 90.8 97 97.9 92.2 Example 3 82.2 83.8 88.7 96.5 98.2 92.6 Example 4 83.1 84.2 89.4 95.3 98 93.1 Example 5 82.9 83.9 88.4 95.5 97.7 94.1 Comparative Example 1 83.6 85.3 91 95.8 97.5 92.2 Comparative Example 2 84.1 85.5 92.3 96.2 98.1 93.4 Comparative Example 3 82.5 84.2 90.5 94.7 98 93

[0109] Sulfur dioxide aging test

[0110] On the basis of the above test, 500ppm of sulfur dioxide was added to the simulated gas. After aging for 240h at 368℃, the conversion efficiency of nitrogen oxides was tested at 300℃, 350℃ and 400℃. The test gas was simulated gas.

[0111] The test results refer to Table 2:

[0112] Table 2 Unit %

[0113] 300℃ 350℃ 400℃ Example 1 88.2 95.8 96.3 Example 2 89.3 96.3 95.6 Example 3 87.5 95 95.5 Example 4 89.1 93.5 94.7 Example 5 83.5 87.7 85.2 Comparative Example 1 83 86.2 85.5 Comparative Example 2 83.4 89.5 88.3 Comparative Example 3 86.3 92.4 92.4

[0114] Part II Optimization of ammonia denitrification system

[0115] System Example 1

[0116] The transformation of this project is based on the 4 sets of SCR catalytic units 3 before the transformation of the original plant area. During the transformation process, one set of SCR catalytic units 3 was selected for transformation, and the other three sets of SCR catalytic units 3 operated normally. Before the design of this project, after demonstration and analysis, the design of ammonia spraying grid with finer nozzles was excluded. This design is not suitable for the hydrolysis of ammonia process and is prone to reverse reaction and clogging of the pipeline. At the same time, the solution of ammonia spraying by vortex mixer is also excluded. This system has high cost and complex structure. This project finally chose to optimize and finalize the design based on the design of expanding the inner diameter of the ammonia spraying pipeline for multiple times.

[0117] After many experiments, this project finally selected the solution of this embodiment.

[0118] The details are as follows:

[0119] refer to Figures 1 to 8 A urea-to-ammonia denitrification system includes a urea hydrolysis unit 1, an ammonia-air mixing unit 2 for diluting ammonia gas input from the urea hydrolysis unit 1, and an SCR catalytic unit 3; an ammonia injection unit 4 is provided in the SCR catalytic unit 3.

[0120] The denitration system has a working principle similar to that of a conventional denitration system. Urea is hydrolyzed by a urea hydrolysis unit 1 to produce ammonia gas, which enters an ammonia-air mixing unit 2 to mix with heated air and is diluted to an ammonia concentration of 5%. The ammonia gas then enters an SCR catalytic unit 3 through an ammonia injection unit 4 to catalytically convert ammonia nitrogen compounds into nitrogen gas.

[0121] In the existing technology, the control of flow field uniformity is a key factor affecting catalytic efficiency. A uniform and strong flow field creates the necessary conditions for the redox reaction between NOx and the reducing agent on the catalyst surface. The desired goal is to reduce fluid resistance on the basis of sufficient reduction. To achieve this goal, uniform mixing of ammonia and flue gas is particularly important.

[0122] This embodiment can effectively improve the uniformity of the flow field without increasing the fluid resistance by modifying the channel on the inlet side of the SCR catalytic unit 3 and the ammonia injection unit 4;

[0123] Specifically, the channel on the inlet side of the SCR catalytic unit 3 is divided into multiple fine channels 32 by a partition 31; there are multiple ammonia injection units 4, each of which corresponds to a fine channel 32 and is located inside the fine channel 32; the ammonia injection unit 4 includes an ammonia-air mixed gas input pipe 41 connected to the ammonia-air mixing unit 2, and multiple first nozzles connected to the ammonia-air mixed gas input pipe 41; the first nozzle includes an output pipe 42 and a conical head 43 located at the output end of the output pipe 42; the tip of the conical head 43 extends to the inside of the output pipe 42, and a gap 44 is left between the conical head 43 and the output pipe 42; the conical head 43 and the output pipe 42 are connected by a connecting plate 45; the connecting plate 45 extends to the edge of the conical head 43; adjacent connecting plates 45 constitute a gas flow channel; the diameter of the thick end of the conical head 43 is larger than the diameter of the output pipe 42; the direction from the tip of the conical head 43 to the thick end of the conical head 43 is the direction of flue gas flow.

[0124] The present invention divides the channel at the inlet side of the SCR catalytic unit 3 into a plurality of fine channels 32. Each fine channel 32 is isolated from each other when spraying ammonia, which can avoid the influence between adjacent ammonia spraying units 4. The separation into a plurality of fine channels 32 does not increase the smoke resistance. At the same time, the uniformity of the mixing of the smoke and ammonia in each channel can be ensured.

[0125] The uniformity of ammonia spraying is inseparable from the modification of the nozzle. In this embodiment, by providing a conical head 43 at the end of the first nozzle and a gas flow channel formed by a connecting plate 45, the gas can be made to spin. The degree of gas spin is closely related to the mixing uniformity of the flue gas.

[0126] In order to improve the spin of ammonia, the conical head 43 is introduced into the inside of the output pipe 42, and an ammonia output channel with a gradually reduced cross-sectional area is formed in the output pipe 42. At the same time, through the high-speed flow of smoke on the outer wall of the output pipe 42, a low-pressure area created by the rapid fluid flow will be formed at the position of the gap 44. Ammonia quickly enters the low-pressure area from the output pipe 42 and mixes with the smoke flowing there, and flows along the outer wall of the conical head 43, and finally forms an outward divergent airflow to achieve the mixing of smoke and ammonia farther away. In this embodiment, the flow of ammonia starts from the inside of the output pipe 42 and flows along the wall of the conical head 43, and the smoke flows along the output pipe 42 before colliding with the wall of the conical head 43. At the intersection of the two fluids, the smoke impacts the ammonia, forming a strong spin. Therefore, in this embodiment, the mixed fluid of smoke and ammonia can not only diverge outward along the cone, but also has a strong spin, further improving the mixing effect with the smoke farther away.

[0127] In order to verify the relevant technical effects of this embodiment, the parameters of this embodiment are specifically as follows:

[0128] This project is based on the transformation of the original SCR system of the factory. The channel size of the inlet side of the SCR catalytic unit 3 of the original system is 2.9m×7.5m, with a cross-sectional area of ​​21.75m 2 , the channel is divided into 6 small channels 32; the cross-sectional dimensions of the small channels 32 are 1.45m×2.5m; the length of the small channels 32 is 1.6m;

[0129] Each ammonia spray unit 4 includes 9 first nozzles; the 9 first nozzles are arranged in a 3×3 form; the diameter of the thick end of the first nozzle is 5 cm; the width of the gap 44 is 7.3 mm; the cross-section of the conical head 43 is an equilateral triangle; the diameter of the output pipe 42 is 32 mm; the length of the connecting plate 45 is 43.4 mm, the width is 9.2 mm, and the thickness does not affect the result.

[0130] The first nozzle at the center of each ammonia spraying unit 4 extends to a position of about 1.3 m inside the fine channel 32; the remaining first nozzles extend to a position of about 0.5 m inside the system and maintain a distance of 0.36 m from the inner wall of the fine channel 32;

[0131] The main test items are the CV deviation of the ammonia nitrogen molar ratio distribution in each partition of the catalyst inlet flue section and the average relative standard CV deviation of the velocity distribution in the first layer catalyst inlet section.

[0132] System Comparison Example 1

[0133] refer to Fig. 9 and Fig.10, which is basically the same as system embodiment 1, except that the cone of the first nozzle is cancelled and replaced by two first guide plates C arranged in a V-shape.

[0134] The tip of the first guide plate C is welded to the end of the output pipe 42; its length is 60 mm; and the maximum distance between the two first guide plates C is 5 cm.

[0135] System Comparison Example 2

[0136] refer to Fig.11 , which is basically the same as system embodiment 1, except that the conical head 43 of the first nozzle is moved forward so that the tip of the conical head 43 is flush with the end of the output pipe 42.

[0137] System Comparison Example 3

[0138] refer to Fig.12 , which is basically the same as system embodiment 1, except that the cone of the first nozzle is moved forward so that the tip of the cone head 43 is flush with the end of the output pipe 42, and a plug A is welded to the tip of the cone head 43, which occupies part of the space of the output pipe 42, and the end of the plug away from the cone head 43 is a hemispherical ball head; the distance between the plug and the output pipe 42 is 7.3 mm, and at the same time, the first connecting plate B is moved to the inside of the output pipe 42 to connect the plug and the output pipe 42. The first connecting plate B is the same as in embodiment 1, and there are also 4 pieces.

[0139] System Comparison Example 4

[0140] The system is basically the same as the first embodiment, except that the partition 31 is eliminated.

[0141] System Comparison Example 5

[0142] It is basically the same as system embodiment 1, except that all the first nozzles of each ammonia spraying unit 4 are flush, and the first nozzles extend to a position of about 1 m in the fine channel 32 .

[0143] Performance Testing

[0144] This system corresponds to a 350MW domestically produced steam extraction heating type air cooling unit;

[0145] Test the CV deviation A of the ammonia nitrogen molar ratio distribution in each partition of the catalyst inlet flue section under full load conditions and the average relative standard CV deviation B of the velocity distribution of the first layer catalyst inlet section;

[0146] The test results are shown in Table 3:

[0147] Table 3

[0148] Ammonia nitrogen molar ratio distribution CV deviation A Velocity distribution average relative standard CV deviation B System Example 1 1.31% 5.6% System Comparison Example 1 2.5% 9.3% System Comparison Example 2 2.44% 11.2% System Comparison Example 3 1.96% 8.5% System Comparison Example 4 2.39% 10.5% System Comparison Example 5 1.66% 8.1%

[0149] It can be seen from the above tests that after the comprehensive optimization of Example 1 of the present invention, the CV deviation of the ammonia nitrogen molar ratio distribution in each partition of the catalyst inlet flue cross section is less than 2.5%, and the average relative standard deviation CV of the velocity distribution of the first layer catalyst inlet cross section is less than 10%.

[0150] Referring to the comparison between Example 1 and Comparative Example 4, after the partition 31 is removed, the ammonia spraying in adjacent intervals will affect each other, reducing the uniformity of ammonia nitrogen distribution between the areas, indicating that the multi-zone mixed ammonia design using the partition 31 of the present invention is effective.

[0151] Referring to the comparison between Example 1 and Comparative Example 5, the inward extension of the central nozzle is beneficial to the mixing of ammonia nitrogen.

[0152] By comparing Example 1 with Comparative Examples 1-3, it can be seen that the diffusible and spinnable fluid formed by the nozzle of the present invention can effectively improve the uniformity of ammonia nitrogen mixing.

[0153] System Example 2

[0154] This embodiment is further optimized on the basis of embodiment 1, and the optimization measures are as follows:

[0155] refer to Figures 1 to 8 On the basis of Example 1, each ammonia injection unit 4 is provided with a control valve 46; six sensors 6 for detecting nitrogen oxides are provided in each fine channel 32; and the control valve 46 is adjusted according to the detection result of the sensor 6.

[0156] Through the above optimization, it can be achieved that the ammonia injection control in each fine channel 32 is independent, which can solve the problem of difficult control of ammonia spray caused by different concentrations of flue gas near the wall and the middle position in the channel on the inlet side of the SCR catalytic unit 3.

[0157] As a further preferred embodiment of the present invention, the ammonia-air mixing unit 2 comprises a diffusion tube 21 and an ammonia gas inlet pipe 22 located in the diffusion tube 21; the middle portion of the diffusion tube 21 is a throat 23; one end of the diffusion tube 21 is an inlet for inputting hot air; the other end of the diffusion tube 21 is an outlet connected to the ammonia-air mixed gas inlet pipe 41; the outlet of the ammonia gas inlet pipe 22 is located near the throat 23; the throat 23 is provided with a plurality of guide plates 24 with the same inclination direction; due to the increase in the gas flow rate of the throat 23 of the diffusion tube 21, especially near the wall, the gas flow rate of the throat 23 of the diffusion tube 21 increases. The increase in flow velocity is more obvious. By arranging an inclined guide plate 24 at the throat 23, the gas in the throat 23 can be rotated. When the gas leaves the throat 23, a strong cyclone can be formed for mixing, thereby improving the uniformity of mixing. Further preferably, a second nozzle is provided at the outlet of the ammonia inlet pipe 22. The second nozzle has the same structure as the first nozzle. The structural characteristics of the second nozzle that can generate airflow spin can further improve the uniformity of air-ammonia mixing, and the ammonia concentration entering the SCR catalytic unit 3 can be stabilized at 5%, and the ammonia uniformity is good.

[0158] As a further preference of this embodiment, the inlet of the diffusion tube 21 is connected to the tube side of a heat exchanger 7, and the heat exchanger 7 is located inside the outlet end of the SCR catalytic unit 3. The inlet of the tube side of the heat exchanger 7 is connected to the blower 8, and the axis of the ammonia inlet pipe 22 coincides with the axis of the diffusion tube 21; the dilution air flue gas heating scheme is to use the hot flue gas with low flow rate at the bottom of the SCR reactor to exchange heat with the cold air from the dilution fan. Since the pipeline wear is proportional to the 2.7th power of the flue gas flow rate, the flow rate here is much lower than the flow rate at the economizer, and the wear is slight. When designing, the wear allowance of the tube wall of the heat exchanger 7 can be appropriately increased to ensure stable operation. At the same time, due to the small heat exchange area, the effect on the flue gas side resistance can be ignored, and the effect on the flue gas temperature at the air preheater inlet is small, and the daily maintenance of the flue gas heat exchanger 7 is small. With a dilution air temperature of 200°C and a single air volume of 4000Nm 3 / h (maintaining the ammonia concentration in the ammonia mixed gas at 5%), the heat source calculation is divided into three types of heat sources: (1) electric heating; (2) SCR outlet flue gas heating; (3) auxiliary steam heating. The energy consumption calculation results are summarized as follows: (1) Electric heating - 235kW; (2) Steam heating - 0.3t / h (temperature 290℃, pressure 1.0MPa); (3) Flue gas heating - overall temperature drop 0.3℃ (heat exchanger 7 total area 200m 2 ).

[0159] As a further preference of this embodiment, the urea hydrolysis unit 1 includes a urea hydrolyzer 11, a urea solution input pipe 12 connected to the urea hydrolyzer 11, a catalyst solution input pipe 13, and a waste liquid discharge pipe 14; a discharge port 15 is provided on the top of the urea hydrolysis unit 1, and a steam-water separator is provided in the discharge port 15; the discharge port 15 is connected to the ammonia input pipe 22, and the waste liquid discharge pipe 14 is connected to the urea solution tank 5.

[0160] According to tests, the nitrogen oxide conversion rate at the outlet of the SCR catalytic unit of this embodiment is higher than 98%.

[0161] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for producing ammonia from urea and denitrification, characterized in that: The method comprises the following steps: Step 1: using urea as a raw material to prepare ammonia by catalytic hydrolysis; Step 2: The ammonia obtained in step 1 is mixed with the dilution air and then mixed with the flue gas, and then enters the SCR catalytic unit for catalytic denitration; In the step 1, the catalyst used is ammonium dihydrogen phosphate; In step 2, the catalyst used in the SCR catalytic unit is a supported catalyst; the flue gas temperature is 368±3°C under stable working conditions; the sulfur dioxide content is 0.04-0.06 vol%; the nitrogen oxide content in the flue gas is 200-300 mg / Nm 3 ; The preparation method of the supported catalyst comprises the following steps: Step 11: placing the zeolite powder in a soluble zirconium salt solution, performing ion exchange at 50 to 90° C. for 12 to 24 hours with stirring, and then filtering, washing, and drying to obtain a first powder; Step 12: placing the first powder in a soluble cerium salt solution, performing ion exchange at 50 to 90° C. for 12 to 24 hours with stirring, and then filtering, washing, and drying to obtain a second powder; Step 13: Repeat step 1 and step 2 to obtain a third powder; Step 14: placing the third powder in a soluble gallium salt solution, performing ion exchange at 50 to 90° C. for 12 to 24 hours with stirring, and then filtering, washing, and drying to obtain a fourth powder; Step 15: preparing the fourth powder into a slurry, and performing molding and calcination to obtain a supported catalyst; The concentration of metal ions in the soluble zirconium salt solution and the soluble cerium salt solution is 0.15-0.3 mol / L; The concentration of metal ions in the soluble gallium salt solution is 0.05-0.1 mol / L; The temperature of the dilution air is 200-220°C; the dilution air dilutes the ammonia to an ammonia concentration of 5 vol% or less; The ammonia gas and the dilution air are mixed in the ammonia-air mixing unit, and the dilution air is heated by a first heat exchanger, the first heat exchanger is located inside the outlet end of the SCR catalytic unit, and the inlet of the tube side of the heat exchanger is connected to a blower; The SCR catalytic unit is provided with an ammonia injection unit and a catalyst layer; the catalyst layer is filled with a supported catalyst; the channel on the inlet side of the SCR catalytic unit is divided into a plurality of fine channels by a partition; There are multiple ammonia spraying units, each of which corresponds to a thin channel and is located inside the thin channel; The ammonia injection unit includes an ammonia-air mixed gas input pipe connected to the ammonia-air mixing unit, and a plurality of first nozzles connected to the ammonia-air mixed gas input pipe; the first nozzle includes an output pipe and a conical head located at the output end of the output pipe; the tip of the conical head extends to the interior of the output pipe, and a gap is left between the conical head and the output pipe; the conical head and the output pipe are connected by a connecting plate; the connecting plate extends to the edge of the conical head; adjacent connecting plates form a gas flow channel; the diameter of the thick end of the conical head is larger than the diameter of the output pipe; the direction from the tip of the conical head to the thick end of the conical head is the direction of flue gas flow.

2. The method for producing ammonia from urea according to claim 1, characterized in that: In step 1, the pressure of the catalytic hydrolysis method is 0.5 MPa, the temperature is 130-140° C., the concentration of urea in the solution is 40-55 wt %; and the concentration of ammonia in the gas after hydrolysis is controlled to be 35-40 vol %.

3. The method for producing ammonia from urea according to claim 1, characterized in that: In the step 15, the calcination temperature is 500-700° C., the calcination atmosphere is oxygen calcination, and the calcination time is 3-5 hours.

4. The method for preparing ammonia and denitrification from urea according to claim 1, characterized in that: In the steps 11 to 13, the ratio of the powder added to each solution is 50-100 g / L.

5. The method for preparing ammonia and denitrification from urea according to claim 1, characterized in that: The zeolite in the supported catalyst is 3A molecular sieve, 4A molecular sieve or 5A molecular sieve.

6. The method for preparing ammonia and denitrification from urea according to claim 1, characterized in that: The diameter of the thick end of the conical head is 1.8-2.2 times the diameter of the output pipe; each ammonia spraying unit includes 9 first nozzles; the 9 first nozzles are arranged in a 3×3 form; in the direction of flue gas flow, the middle first nozzle is located behind the other first nozzles; the cross-sectional dimensions of the fine channel are 1.45m×2.5m; the diameter of the thick end of the first nozzle is 5cm; the width of the gap is 8-10mm; the cross-section of the conical head is an equilateral triangle.

Citation Information

Patent Citations

  • Denitrification catalyst, honeycomb structure type denitrification catalyst, and method of denitrification with the same

    CN101296748A

  • Selective catalytic reduction processes using doped cerias

    CN105939775A

Cited By

  • Heat recovery unit of denitration system

    CN223542741U