A method for preparing antibacterial composite polyisoprene gloves

By using synthetic polyisoprene latex and modified silica in surgical gloves, the allergy and nitrosamine toxicity problems of natural latex are solved, and gloves with high insulation and antibacterial properties are achieved, ensuring surgical safety and Achievement of performance standards.

CN118388809BActive Publication Date: 2024-10-25SUZHOU COLOR WAY ENTERPRISE DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410307088.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-18
Publication Date
2024-10-25
Estimated Expiration
2044-03-18

AI Technical Summary

Technical Problem

Problems with existing surgical glove materials such as natural latex due to protein allergy and nitrosamine biotoxicity, and the inability of synthetic materials to meet performance standards, have led to the need for a new glove material to replace natural latex.

Method used

Synthetic polyisoprene latex is used as an alternative material, and water-based polyurethane latex and modified silica are added to it to improve the strength and antibacterial properties of the gloves and enhance insulation to avoid electric shock accidents.

Benefits of technology

It provides gloves with high insulation and excellent antibacterial properties to avoid electric shock accidents during surgical operations, improves use safety and antibacterial properties, and avoids cross-infection of medical staff.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a method for preparing an antibacterial composite polyisoprene glove, comprising the following steps: preparing modified nano silicon oxide; dispersing the modified nano silicon oxide in deionized water to obtain a modified nano silicon oxide dispersion, then adding the modified nano silicon oxide dispersion into polyisoprene latex and stirring and mixing evenly, then adding a stabilizer, an aqueous polyurethane emulsion, a vulcanizing agent and an accelerator, stirring and mixing evenly, and obtaining an impregnation solution; cleaning and drying the glove mold, and then performing an impregnation treatment in a coagulation solution, then taking it out for a drying, and then performing a secondary impregnation treatment in the impregnation solution, and then taking it out for a secondary drying, and then performing a curling treatment on the product on the hand film, and then performing vulcanization, and finally demolding to obtain an antibacterial glove. The antibacterial gloves prepared by the invention not only have good mechanical properties, but also have excellent antibacterial properties, good insulation properties, and high safety in use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing antibacterial composite polyisoprene gloves. Background Art

[0002] Currently, surgical gloves on the market are all made of natural latex. However, the allergic and nitrosamine biotoxicity caused by the protein in natural latex have attracted more and more attention. However, so far, no raw material can completely replace the performance of natural latex and overcome the defects of natural latex. The performance of gloves produced by synthetic materials on the market, such as polyurethane materials, polyisoprene synthetic rubber, nitrile latex, and chloroprene latex, cannot reach the performance standards and performance of current surgical gloves. Therefore, it is necessary to provide a new glove material to solve the above technical problems. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for preparing antibacterial composite polyisoprene gloves in view of the deficiencies of the prior art. The present invention adopts synthetic polyisoprene latex instead of natural latex, and simultaneously adds a certain amount of aqueous polyurethane emulsion and modified silica to the polyisoprene latex, which increases the strength of the gloves on the one hand, and improves the antibacterial property of the gloves on the other hand. Moreover, the insulation property of the synthetic polyisoprene is much higher than that of the natural latex, which can compensate for the electric shock caused by improper use of high-frequency electric knife, and can effectively avoid accidents caused by surgical operations.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0005] A method for preparing antibacterial composite polyisoprene gloves comprises the following steps:

[0006] (1) adding dopamine hydrochloride to the nano-silicon oxide dispersion, stirring evenly, then adding Tris buffer solution, stirring to react, and then filtering, and directly dispersing the obtained solid in ethanol without drying to obtain a pretreated nano-silicon oxide dispersion;

[0007] (2) adding a curcumin derivative, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and a base catalyst to anhydrous dichloromethane, stirring until the solid is dissolved, then adding allyl polyethylene glycol, stirring to react, standing to separate the layers after the reaction is completed, extracting the organic phase with dichloromethane and drying, and finally removing the solvent to obtain a coupling compound;

[0008] (3) adding the coupling compound to the pretreated nano-silicon oxide dispersion obtained in step (1), and then adding an initiator, reacting under an inert atmosphere, filtering after the reaction is completed, and drying the solid to obtain modified nano-silicon oxide;

[0009] (4) dispersing the modified nano-silicon oxide prepared above in deionized water to prepare a modified nano-silicon oxide dispersion, then adding the dispersion into polyisoprene latex and stirring to mix evenly, then adding a stabilizer, an aqueous polyurethane emulsion, a vulcanizing agent and an accelerator, stirring to mix evenly, and preparing an impregnation solution;

[0010] (5) After cleaning and drying the glove mold, the glove mold is immersed in a coagulation liquid once, then taken out and dried once, then immersed in the dipping liquid for a second time, then taken out and dried for a second time, and then the product on the hand film is curled, then vulcanized, and finally demolded to obtain the antibacterial gloves.

[0011] Preferably, in step (1), the concentration of the Tris buffer solution is 10 mmol / L, the pH is 8.5, the dosage ratio of the nano-silicon oxide, dopamine hydrochloride, and Tris buffer solution is 2 g: (0.1-0.5) g: 10 ml; and / or the stirring reaction temperature is 50-60°C and the time is 40-50 h.

[0012] Preferably, in step (2), the mass ratio of the curcumin derivative, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, base catalyst, and allyl polyethylene glycol is (40-50):(30-40):(1-2):(90-100); and / or the stirring reaction temperature is 0°C and the time is 10-15h.

[0013] Preferably, the preparation method of the curcumin derivative is as follows: curcumin, an alkali catalyst and triethylamine are added to anhydrous tetrahydrofuran and stirred and mixed, then an acid anhydride is added, and a reflux reaction is carried out at 60-80° C. in an inert atmosphere for 10-15 hours, then the solvent is removed, and then a hydrochloric acid solution is added for neutralization, and then ethyl acetate is added for extraction, and the organic phase is separated after stirring and mixing, and the organic phase is removed The solvent is purified by column chromatography to obtain a curcumin derivative.

[0014] Preferably, the acid anhydride is glutaric anhydride, and the usage ratio of curcumin, base catalyst, triethylamine and glutaric anhydride is 2g: (0.1-0.2)g: 1-2ml: (0.5-1)g.

[0015] Preferably, in step (3), the concentration of the pretreated nano-silicon oxide dispersion is 5-10wt%, the initiator is azobisisobutyronitrile, and the mass ratio of the pretreated nano-silicon oxide dispersion, the initiator and the coupling compound is 10:(0.02-0.05):(5-10).

[0016] Preferably, in step (3), the reaction temperature is 60° C. and the reaction time is 20-30 h.

[0017] Preferably, in step (4), the concentration of the modified nano-silicon oxide dispersion is 1-2 g / L, the solid content of the polyisoprene latex is 50-60 wt %, the stabilizer is one of potassium hydroxide and sodium hydroxide, and the solid content of the aqueous polyurethane emulsion is 50-60 wt %.

[0018] Preferably, in step (4), the amounts of the components used, in parts by weight, are: 0.8-5 parts of modified nano-silicon oxide dispersion, 80-100 parts of polyisoprene latex, 0.02-0.05 parts of stabilizer, 20-50 parts of aqueous polyurethane emulsion, 0.1-0.5 parts of vulcanizing agent, and 0.1-0.2 parts of accelerator.

[0019] Preferably, in step (5), the conditions for the first dipping treatment are: temperature of 40-50°C, time of 3-8s; the conditions for the first drying are 70-80°C, time of 5-10min; the conditions for the second dipping treatment are room temperature, time of 8-10s; the conditions for the second drying are temperature of 70-80°C, time of 10-20min; the conditions for the vulcanization are: temperature of 130°C, time of 30-50min.

[0020] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:

[0021] The antibacterial gloves provided by the present invention use synthetic polyisoprene latex instead of natural latex. The insulation of synthetic polyisoprene latex is much higher than that of natural latex, which can make up for the electric shock caused by improper use of high-frequency electric knife, and can effectively avoid accidents caused by surgical operations. In addition, a certain amount of polyurethane latex and modified nano-silicon dioxide are added to the matrix to increase the strength of the product. At the same time, the modified silicon dioxide has an antibacterial effect, which can improve the antibacterial performance of the gloves.

[0022] The nano silicon oxide added in the present invention has a large specific surface area and special surface activity, and can interact with the cell membrane of microorganisms, destroy its structure, and cause the death of microorganisms. The present invention uses a homemade curcumin derivative to react with allyl polyethylene glycol, and grafts it on the surface of nano silicon oxide through an initiator, which not only improves the dispersibility of nano silicon oxide in the matrix, but also further improves the antibacterial property of nano silicon oxide. In the specific modification, the present invention first self-assembles a layer of polydopamine on the surface of nano silicon oxide, which greatly improves the roughness and adhesion of the surface of nano silicon oxide, and is convenient for subsequent modification treatment.

[0023] The material used in the preparation of the antibacterial gloves of the present invention does not contain protein and will not cause human allergies. In addition, the antibacterial gloves have excellent insulation properties, which improves the safety of the product. The antibacterial performance provided by the present invention is excellent and can effectively avoid cross infection of medical staff. DETAILED DESCRIPTION

[0024] In order to better understand the present invention, the present invention is further described below by way of examples. The examples are only used to explain the present invention and will not constitute any limitation to the present invention.

[0025] In the following embodiments, the weight average molecular weight of the allyl polyethylene glycol is 2400, and the average particle size of the nano-silicon oxide is 20±2 nm; the concentration of the Tris buffer solution is 10 mmol / L, and the pH is 8.5; the coagulation liquid in the following embodiments is a solution composed of calcium chloride, sodium dibutylnaphthalene sulfonate NF and softening water in a mass ratio of 0.1:0.015:1.

[0026] In the following embodiment, the preparation method of the curcumin derivative is as follows: 2g of curcumin, 0.15g of a base catalyst, and 1.5ml of triethylamine are added to 50ml of anhydrous tetrahydrofuran and stirred and mixed, and then 0.65g of anhydride is added, and the reaction is refluxed at 75°C in an inert atmosphere for 12h, and then the solvent is removed, and then a 1mol / L hydrochloric acid solution is added for neutralization, and then ethyl acetate is added for extraction, and the organic phase is separated after stirring and mixing, and the organic phase is purified by column chromatography after the solvent is removed to obtain a curcumin derivative.

[0027] The base catalyst is selected from 4-dimethylaminopyridine, and the acid anhydride is glutaric anhydride. Example 1

[0028] A method for preparing antibacterial composite polyisoprene gloves comprises the following steps:

[0029] (1) Add 0.2 g of dopamine hydrochloride to 2 L of 1 g / L nano-silicon oxide dispersion, stir evenly, then add 10 ml of Tris buffer solution, stir and react at 55 °C for 48 h, then filter, and directly disperse the obtained solid in ethanol without drying to obtain a pretreated nano-silicon oxide dispersion with a concentration of 6 wt%;

[0030] (2) Add 0.04 g of a curcumin derivative, 0.03 g of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and 0.001 g of 4-dimethylaminopyridine to 50 ml of anhydrous dichloromethane, stir until the solid is dissolved, then add 0.09 g of allyl polyethylene glycol, stir and react at 0°C for 12 h. After the reaction is completed, stand and separate the layers. The organic phase is extracted with dichloromethane and dried. Finally, the solvent is removed to obtain a coupling compound.

[0031] (3) Add 6 g of the above coupling compound to 10 g of the pretreated nano-silicon oxide dispersion prepared in step (1), and then add 0.02 g of azobisisobutyronitrile, and react at 60° C. in an inert atmosphere for 24 h. After the reaction is completed, filter and dry the solid to obtain modified nano-silicon oxide;

[0032] (4) dispersing the modified nano-silicon oxide prepared above in deionized water to prepare a modified nano-silicon oxide dispersion with a concentration of 1 g / L, then adding 1 part of the modified nano-silicon oxide dispersion to 80 parts of polyisoprene latex with a solid content of 50 wt% by weight, stirring and mixing evenly, then adding 0.02 parts of potassium hydroxide, 20 parts of an aqueous polyurethane emulsion with a solid content of 50 wt%, 0.1 parts of sulfur and 0.1 parts of basic calcium carbonate, stirring and mixing evenly, to prepare an impregnation solution;

[0033] (5) After cleaning and drying the glove mold, immerse it in the coagulation liquid at 40°C for 8 seconds, then take it out and dry it at 70°C for 10 minutes, then immerse it in the immersion liquid for a second time at room temperature for 10 seconds, then take it out and dry it at 70°C for a second time for 20 minutes, then curl the product on the hand film, then vulcanize it at 130°C for 30 minutes, and finally demold it to obtain the antibacterial gloves. Example 2

[0034] A method for preparing antibacterial composite polyisoprene gloves comprises the following steps:

[0035] (1) Add 0.3 g of dopamine hydrochloride to 2 L of 1 g / L nano-silicon oxide dispersion, stir evenly, then add 10 ml of Tris buffer solution, stir and react at 55 °C for 48 h, then filter, and directly disperse the obtained solid in ethanol without drying to obtain a pretreated nano-silicon oxide dispersion with a concentration of 7 wt%;

[0036] (2) Add 0.045 g of a curcumin derivative, 0.03 g of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and 0.001 g of 4-dimethylaminopyridine to 50 ml of anhydrous dichloromethane, stir until the solid is dissolved, then add 0.1 g of allyl polyethylene glycol, stir and react at 0°C for 12 h. After the reaction is completed, stand and separate the layers. The organic phase is extracted with dichloromethane and dried. Finally, the solvent is removed to obtain a coupling compound.

[0037] (3) Add 7 g of the above coupling compound to 10 g of the pretreated nano-silicon oxide dispersion prepared in step (1), and then add 0.03 g of azobisisobutyronitrile, and react at 60° C. in an inert atmosphere for 24 h. After the reaction is completed, filter and dry the solid to obtain modified nano-silicon oxide;

[0038] (4) The modified nano-silicon oxide prepared above is dispersed in deionized water to prepare a modified nano-silicon oxide dispersion with a concentration of 1 g / L, and then 2 parts of the modified nano-silicon oxide dispersion are added to 85 parts of polyisoprene latex with a solid content of 60 wt% by weight, and stirred to mix evenly, and then 0.03 parts of potassium hydroxide, 30 parts of water-based polyurethane emulsion with a solid content of 50 wt%, 0.2 parts of sulfur and 0.15 parts of basic calcium carbonate are added, and stirred to mix evenly to prepare an impregnation solution;

[0039] (5) After cleaning and drying the glove mold, immerse it in the coagulation liquid at 50°C for 5 seconds, then take it out and dry it at 70°C for 10 minutes, then immerse it in the dipping liquid for a second time at room temperature for 10 seconds, then take it out and dry it at 80°C for a second time for 10 minutes, then curl the product on the hand film, then vulcanize it at 130°C for 30 minutes, and finally demold it to obtain the antibacterial gloves. Example 3

[0040] A method for preparing antibacterial composite polyisoprene gloves comprises the following steps:

[0041] (1) Add 0.3 g of dopamine hydrochloride to 2 L of 1 g / L nano-silicon oxide dispersion, stir evenly, then add 10 ml of Tris buffer solution, stir and react at 55 °C for 48 h, then filter, and directly disperse the obtained solid in ethanol without drying to obtain a pretreated nano-silicon oxide dispersion with a concentration of 8 wt%;

[0042] (2) Add 0.05 g of a curcumin derivative, 0.04 g of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and 0.002 g of 4-dimethylaminopyridine to 50 ml of anhydrous dichloromethane, stir until the solid is dissolved, then add 0.09 g of allyl polyethylene glycol, stir and react at 0°C for 12 h. After the reaction is completed, stand and separate the layers. The organic phase is extracted with dichloromethane and dried. Finally, the solvent is removed to obtain a coupling compound.

[0043] (3) Add 8 g of the above coupling compound to 10 g of the pretreated nano-silicon oxide dispersion prepared in step (1), and then add 0.04 g of azobisisobutyronitrile, and react at 60° C. in an inert atmosphere for 24 h. After the reaction is completed, filter and dry the solid to obtain modified nano-silicon oxide;

[0044] (4) The modified nano-silicon oxide prepared above is dispersed in deionized water to prepare a modified nano-silicon oxide dispersion with a concentration of 1 g / L, and then 4 parts of the modified nano-silicon oxide dispersion are added to 90 parts of polyisoprene latex with a solid content of 50 wt% by weight, and stirred to mix evenly, and then 0.04 parts of sodium hydroxide, 30 parts of water-based polyurethane emulsion with a solid content of 50 wt%, 0.3 parts of sulfur and 0.1 parts of basic calcium carbonate are added, and stirred to mix evenly to prepare an impregnation solution;

[0045] (5) After cleaning and drying the glove mold, immerse it in the coagulation liquid at 40°C for 8 seconds, then take it out and dry it at 70°C for 10 minutes, then immerse it in the immersion liquid for a second time at room temperature for 10 seconds, then take it out and dry it at 70°C for a second time for 20 minutes, then curl the product on the hand film, then vulcanize it at 130°C for 30 minutes, and finally demold it to obtain the antibacterial gloves. Example 4

[0046] A method for preparing antibacterial composite polyisoprene gloves comprises the following steps:

[0047] (1) Add 0.5 g of dopamine hydrochloride to 2 L of 1 g / L nano-silicon oxide dispersion, stir evenly, then add 10 ml of Tris buffer solution, stir and react at 55 °C for 48 h, then filter, and directly disperse the obtained solid in ethanol without drying to obtain a pretreated nano-silicon oxide dispersion with a concentration of 10 wt%;

[0048] (2) Add 0.05 g of a curcumin derivative, 0.04 g of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and 0.002 g of 4-dimethylaminopyridine to 50 ml of anhydrous dichloromethane, stir until the solid is dissolved, then add 0.1 g of allyl polyethylene glycol, stir and react at 0°C for 12 h. After the reaction is completed, stand and separate the layers. The organic phase is extracted with dichloromethane and dried. Finally, the solvent is removed to obtain a coupling compound.

[0049] (3) Add 10 g of the above coupling compound to 10 g of the pretreated nano-silicon oxide dispersion prepared in step (1), and then add 0.05 g of azobisisobutyronitrile, and react at 60° C. in an inert atmosphere for 24 h. After the reaction is completed, filter and dry the solid to obtain modified nano-silicon oxide;

[0050] (4) dispersing the modified nano-silicon oxide prepared above in deionized water to prepare a modified nano-silicon oxide dispersion with a concentration of 1 g / L, then adding 5 parts of the modified nano-silicon oxide dispersion to 100 parts of polyisoprene latex with a solid content of 50 wt% by weight, stirring and mixing evenly, then adding 0.05 parts of sodium hydroxide, 50 parts of an aqueous polyurethane emulsion with a solid content of 50 wt%, 0.5 parts of sulfur and 0.2 parts of basic calcium carbonate, stirring and mixing evenly to prepare an impregnation solution;

[0051] (5) After cleaning and drying the glove mold, immerse it in the coagulation liquid at 40°C for 8 seconds, then take it out and dry it at 70°C for 10 minutes, then immerse it in the immersion liquid for a second time at room temperature for 10 seconds, then take it out and dry it at 70°C for a second time for 20 minutes, then curl the product on the hand film, then vulcanize it at 130°C for 30 minutes, and finally demold it to obtain the antibacterial gloves.

[0052] Comparative Example 1

[0053] In the preparation process of modified nano silicon oxide, dopamine is not used for modification, but coupling compound is used directly for modification, and other conditions are the same as those in Example 4.

[0054] Comparative Example 2

[0055] In the preparation of modified nano-silicon oxide, only dopamine was used for modification, and no coupling compound was used for modification. Other conditions were the same as those in Example 4.

[0056] Comparative Example 3

[0057] Nano-silicon oxide was directly added to the polyisoprene latex without modification, and other conditions were the same as those in Example 4.

[0058] Comparative Example 4

[0059] No modified nano-silicon oxide was added to the impregnation solution, and other conditions were the same as those in Example 4.

[0060] The gloves prepared in the above embodiments and comparative examples were tested for performance according to LST EN 455-4-2009. The test results are as follows:

[0061]

[0062] From the above tests, it can be seen that the mechanical properties and antibacterial properties of the gloves with the addition of modified nano-silica have been significantly improved. After being modified by polydopamine and coupling compounds in turn, the compatibility of nano-silica with the matrix has been significantly improved, thereby improving the performance of the material.

[0063] In addition, it should be understood that after reading the contents of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A method for preparing antibacterial composite polyisoprene gloves, characterized in that: The following steps are involved: (1) adding dopamine hydrochloride to the nano-silicon oxide dispersion, stirring evenly, then adding Tris buffer solution, stirring to react, and then filtering, and directly dispersing the obtained solid in ethanol without drying to obtain a pretreated nano-silicon oxide dispersion; (2) adding a curcumin derivative, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and a base catalyst to anhydrous dichloromethane, stirring until the solid is dissolved, then adding allyl polyethylene glycol, stirring to react, standing to separate the layers after the reaction is completed, extracting the organic phase with dichloromethane and drying, and finally removing the solvent to obtain a coupling compound; (3) adding the coupling compound to the pretreated nano-silicon oxide dispersion obtained in step (1), and then adding an initiator, reacting under an inert atmosphere, filtering after the reaction is completed, and drying the solid to obtain modified nano-silicon oxide; (4) dispersing the modified nano-silicon oxide prepared above in deionized water to prepare a modified nano-silicon oxide dispersion, then adding the dispersion into polyisoprene latex and stirring to mix evenly, then adding a stabilizer, an aqueous polyurethane emulsion, a vulcanizing agent and an accelerator, stirring to mix evenly, and preparing an impregnation solution; (5) After cleaning and drying the glove mold, dipping it in a coagulation liquid, taking it out and drying it, dipping it in the dipping liquid for a second time, taking it out and drying it for a second time, and then curling the product on the hand film, vulcanizing it, and finally demolding it to obtain the antibacterial gloves; The preparation method of the curcumin derivative comprises the following steps: adding curcumin, an alkali catalyst and triethylamine to anhydrous tetrahydrofuran and stirring and mixing, then adding anhydride, and performing reflux reaction at 60-80° C. in an inert atmosphere for 10-15 hours, then removing the solvent, then adding a hydrochloric acid solution for neutralization, then adding ethyl acetate for extraction, stirring and mixing, separating the organic phase, removing the solvent from the organic phase, and purifying by column chromatography to obtain the curcumin derivative.

2. The method for preparing an antibacterial composite polyisoprene glove according to claim 1, characterized in that: In step (1), the concentration of the Tris buffer solution is 10 mmol / L, the pH is 8.5, the dosage ratio of the nano-silicon oxide, dopamine hydrochloride, and Tris buffer solution is 2 g: (0.1-0.5) g: 10 ml; and / or the stirring reaction temperature is 50-60° C. and the time is 40-50 h.

3. The method for preparing an antibacterial composite polyisoprene glove according to claim 1, characterized in that: In step (2), the mass ratio of the curcumin derivative, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, base catalyst, and allyl polyethylene glycol is (40-50):(30-40):(1-2):(90-100); and / or the stirring reaction temperature is 0°C and the time is 10-15h.

4. The method for preparing an antibacterial composite polyisoprene glove according to claim 1, characterized in that: The acid anhydride is glutaric anhydride, and the usage ratio of the curcumin, the base catalyst, triethylamine and glutaric anhydride is 2g: (0.1-0.2)g: 1-2ml: (0.5-1)g.

5. The method for preparing an antibacterial composite polyisoprene glove according to claim 1, characterized in that: In step (3), the concentration of the pretreated nano-silicon oxide dispersion is 5-10wt%, the initiator is azobisisobutyronitrile, and the mass ratio of the pretreated nano-silicon oxide dispersion, the initiator and the coupling compound is 10:(0.02-0.05):(5-10).

6. The method for preparing an antibacterial composite polyisoprene glove according to claim 1, characterized in that: In step (3), the reaction temperature is 60°C and the reaction time is 20-30 hours.

7. The method for preparing an antibacterial composite polyisoprene glove according to claim 1, characterized in that: In step (4), the concentration of the modified nano-silicon oxide dispersion is 1-2 g / L, the solid content of the polyisoprene latex is 50-60 wt %, the stabilizer is one of potassium hydroxide and sodium hydroxide, and the solid content of the aqueous polyurethane emulsion is 50-60 wt %.

8. The method for preparing an antibacterial composite polyisoprene glove according to claim 1, characterized in that: In step (4), the amounts of the components used, in parts by weight, are: 0.8-5 parts of modified nano-silicon oxide dispersion, 80-100 parts of polyisoprene latex, 0.02-0.05 parts of stabilizer, 20-50 parts of aqueous polyurethane emulsion, 0.1-0.5 parts of vulcanizing agent, and 0.1-0.2 parts of accelerator.

9. The method for preparing an antibacterial composite polyisoprene glove according to claim 1, characterized in that: In step (5), the conditions for the first dipping treatment are: temperature of 40-50°C, time of 3-8s; the conditions for the first drying are 70-80°C, time of 5-10min; the conditions for the second dipping treatment are room temperature, time of 8-10s; the conditions for the second drying are temperature of 70-80°C, time of 10-20min; the conditions for the vulcanization are: temperature of 130°C, time of 30-50min.