A modified PET and preparation method thereof

Through chemical copolymerization and blending technology, the preparation of modified PET materials solves the problems of slow crystallization speed and poor anti-aging ability of PET materials, and realizes the high mechanical strength and self-repair ability of the material, which is suitable for extreme temperature environments.

CN118388830BActive Publication Date: 2024-12-06中威航空材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410568990.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-12-06
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

The crystallization speed of PET materials during industrial melting continuous foaming is slow, resulting in weak material stiffness, poor anti-aging ability, and poor performance in extreme temperature environments.

Method used

Through chemical copolymerization and blending technology, the esterification reaction is carried out using compounds such as carboxylic acids, acyclic alcohols, fused ring compounds and imides to form modified PET, promote crystal nucleation, and improve crystal structure stability and crosslink density. Build porous mesh structures to enhance impact resistance.

Benefits of technology

It significantly accelerates the crystallization speed of PET materials, improves its mechanical strength and aging resistance, enhances its stability and self-healing ability at extreme temperatures, and broadens the application fields of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_7
    Figure SMS_7
  • Figure SMS_13
    Figure SMS_13
  • Figure SMS_19
    Figure SMS_19
Patent Text Reader

Abstract

The present invention belongs to the field of polymer synthesis, and in particular, relates to a modified PET and a preparation method thereof. The method comprises: (1) mixing cyclic carboxylic acid, acyclic alcohol and hexanol derivatives in proportion, and performing an esterification reaction to obtain a substrate; (2) mixing the substrate, condensed ring compound and organic tin in proportion, heating and stirring, and obtaining prepolymer I; (3) mixing the substrate, imide and acyclic alcohol in proportion, heating and stirring, and obtaining prepolymer II; (4) mixing the substrate, prepolymer I, prepolymer II and foaming agent in proportion, heating and stirring, and obtaining modified polyethylene terephthalate, that is, obtaining modified PET. The present invention accelerates the crystallization speed of the modified PET material by using heteronuclear polymerization through chemical copolymerization, and constructs a stable PET crystal structure through the special grid relationship between the skeleton and the resin, thereby strengthening the stiffness of the material after curing. In addition, the material is modified by chemical copolymerization and blending, and the molecular chain structure is constructed to increase the anti-aging property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer synthesis, and in particular relates to a modified PET and a preparation method thereof. Background Art

[0002] With the rapid progress of science and technology, the mainstream foam core material technology on the market currently has several defects, such as low bonding strength with composite materials, heavy material weight, poor heat resistance, poor chemical resistance, insufficient toughness and low fatigue strength. PET materials have great application potential in the field of fillers. PET, the full name of polyethylene terephthalate, is a linear thermoplastic resin with good weather resistance, chemical stability, impact resistance, high output and relatively low price. However, in the industrial melt continuous foaming process, the crystallization rate is slow because the PET molecular chain contains rigid benzene rings and the flexible carbon chain is short. During the melt cooling process, the degree of crystallinity is low, which in turn affects the mechanical properties and mechanical stability of the product. Summary of the invention

[0003] The technical solution of the present invention aims to solve the technical problems such as slow crystallization speed and incomplete crystallization degree in the PET production process in the existing process, which lead to performance defects such as weak rigidity and poor anti-aging ability of the final production material, and provide a modified PET and a preparation method thereof.

[0004] The main purpose of the present invention is:

[0005] 1. Accelerate the crystallization speed of PET;

[0006] 2. Build a stable PET crystal structure and strengthen the rigidity of the material after curing;

[0007] 3. Increase the aging resistance of PET materials in extreme temperature environments.

[0008] To achieve the above objectives, the present invention adopts the following technical solutions.

[0009] A method for preparing modified PET,

[0010] The method comprises:

[0011] (1) mixing cyclic carboxylic acid, acyclic alcohol and hexanol derivative in proportion, and subjecting the mixture to an esterification reaction to obtain a substrate;

[0012] (2) mixing the substrate, the condensed ring compound and the organotin in proportion, heating and stirring, to obtain a prepolymer I;

[0013] (3) mixing the substrate, imide and acyclic alcohol in proportion, heating and stirring, to obtain prepolymer II;

[0014] (4) The substrate, prepolymer I, prepolymer II and foaming agent are mixed in proportion, heated and stirred to obtain modified polyethylene terephthalate, that is, modified PET.

[0015] As a preference,

[0016] The cyclic carboxylic acid in step (1) is terephthalic acid;

[0017] The acyclic alcohol in step (1) is ethylene glycol;

[0018] The hexanol derivative in step (1) is 2-ethyl-1,3-hexanediol;

[0019] In step (1), the cyclic carboxylic acid, the acyclic alcohol and the hexanol derivative are uniformly mixed in a mass ratio of 3: (2.8-3.2): (0.8-1.2).

[0020] As a preference,

[0021] The esterification reaction in step (1) is carried out under a nitrogen atmosphere at a temperature of 220-240° C. and stirred for 4-6 hours.

[0022] As a preference,

[0023] The fused ring compound in step (2) is 2,2-dimethyl-6-bromo-2H-benzo[B][1,4]oxazin-3(4H)-one;

[0024] The organotin in step (2) is dioctyltin oxide;

[0025] In step (2), the substrate, the condensed ring compound and the organotin are uniformly mixed in a mass ratio of 4: (1.3-1.7): (1.2-1.6).

[0026] As a preference,

[0027] The heating and stirring in step (2) is carried out at a temperature of 200 to 220° C. and the stirring is continued for 2 to 4 hours.

[0028] As a preference,

[0029] The imide in step (3) is N,N'-(4,4'-methylenediphenyl)bismaleimide;

[0030] The acyclic alcohol in step (3) is ethylene glycol;

[0031] In step (3), the substrate, imide and acyclic alcohol are uniformly mixed in a mass ratio of 1: (2.3-2.7): (0.2-0.4).

[0032] As a preference,

[0033] The heating and stirring in step (3) is carried out at a temperature of 150 to 190 °C and the stirring is continued for 1 to 2 hours.

[0034] As a preference,

[0035] The foaming agent in step (4) is azodicarbonamide;

[0036] In step (4), the substrate, prepolymer I, prepolymer II and foaming agent are uniformly mixed in a mass ratio of 3: (1.3-1.7): (0.8-1.2): 0.1.

[0037] As a preference,

[0038] The heating and stirring in step (4) is carried out at a temperature of 200 to 220° C., stirring is continued for 2 to 4 hours, vacuum degassing, solidification and vacuum drying are carried out to constant weight.

[0039] A modified PET.

[0040] In the technical solution of the present invention, the core lies in promoting the crystallization nucleation of the PET material after modification through chemical copolymerization and blending, and improving the crystal arrangement density after nucleation, increasing the molecular cross-linking density in the material, shortening the distance between molecular chain segments, improving the structural stability of polyethylene terephthalate, improving the mechanical properties of the PET material, and further improving the crystallization performance of the modified PET.

[0041] In the field of coordination chemistry, carboxylic acid compounds play a vital role.

[0042] On the one hand, both oxygen atoms in the carboxylic acid molecule have coordination ability and can effectively participate in the coordination process, thereby improving the thermal stability of the structural framework; on the other hand, carboxylic acid can form flexible and changeable coordination modes with various metal ions, such as monodentate, chelated bidentate, bridged multidentate, cis and trans, etc., thereby forming a coordination compound with a unique structure. These characteristics make carboxylic acid compounds have broad application prospects in the field of coordination chemistry. In the technical solution of the present invention, when terephthalic acid and ethylene glycol are esterified and polycondensed, 2-ethyl-1,3-hexanediol can be accurately blended and grafted with the rigid benzene ring of polyethylene terephthalate to preset subsequent active sites. These active sites play a role in promoting the esterification and polycondensation reaction. After the reaction, they can act as organic heteromorphic nuclei to accelerate the crystallization rate and improve the mechanical strength of the modified PET material.

[0043] In the technical solution of the present invention, a metal-organic skeleton is also constructed in the modified polyethylene terephthalate, which can improve the porosity of the modified PET material and form a dense and continuous porous network structure after curing. When subjected to external force, the network structure can provide protection and buffering, thereby improving the impact resistance of the modified PET material. However, if only the metal-organic skeleton is used to reinforce the PET material structure, it will lead to the degeneration of mechanical properties. The compatibility of the metal-organic skeleton with PET is poor, and self-agglomeration may occur. In the technical solution of the present invention, in order to solve this problem, prepolymer II is used to optimize the performance, N, N'- (4, 4'-methylenediphenyl) bismaleimide and ethylene glycol ester produce addition, and finally generate a cross-linked resin with a ladder structure. At the same time, according to the inventor's research, N, N'- (4, 4'-methylenediphenyl) bismaleimide and ethylene glycol ester react with the active sites brought by the modification of 2-ethyl-1, 3-hexanediol to produce an interpenetrating network structure, so that the cross-linking density inside the PET material is increased, the distance between the chain segments is shortened, and the rigidity of the material is further improved. In the technical solution of the present invention, when the material is subjected to external forces, the interpenetrating network structure can hinder cracks. The further expansion makes it difficult for the material to be completely destroyed. The active sites act as stress concentration points, inducing shear yield and silvering of the substrate, thereby improving the impact performance of the modified material and forming a three-dimensional stress field in the interpenetrating network structure. The N,N'-(4,4'-methylenediphenyl)bismaleimide particles are subjected to the compressive stress from the particles, thereby inducing shear yield, which leads to the formation of voids around the rubber particles. These voids change the stress state of the nearby matrix, further inducing shear yield and expanding to the surrounding areas. This process causes plastic deformation of the matrix, effectively preventing further expansion of the cracks and absorbing a large amount of impact energy, thereby improving the mechanical properties of the material.

[0044] In the technical solution of the present invention, after modification by chemical copolymerization and blending, part of the polymer side chains contain three methylene groups, so that the polymer molecular chain presents an irregular spiral structure similar to protein and shows an obvious zigzag conformation. This special structure enables the polymer macromolecular chain to have partial spring-like deformation and recovery capabilities. The polymer molecular chain can be elongated and gradually return to its original state when the external force is eliminated, thereby giving the material partial self-repairing ability, further absorbing and dispersing impact force, and improving the durability and stability of the material. The inventors have found through experiments that this type of structure in the material exists at -70 to 110°C, which broadens the applicable field of the modified PET material provided by the technical solution of the present invention.

[0045] The advantages of the present invention are:

[0046] (1) The present invention accelerates the crystallization rate of modified PET material by chemical copolymerization using heteronuclear polymers;

[0047] (2) The present invention constructs a stable PET crystal structure through a special grid relationship between the skeleton and the resin, thereby strengthening the rigidity of the material after curing;

[0048] (3) In the present invention, the PET material is modified by chemical copolymerization and blending to construct a molecular chain structure to increase the aging resistance of the PET material in an extreme temperature environment. DETAILED DESCRIPTION

[0049] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0050] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0051] Example 1: A method for preparing modified PET,

[0052] The method comprises:

[0053] (1) 99% pure terephthalic acid, 99% pure ethylene glycol and 98% pure 2-ethyl-1,3-hexanediol were uniformly mixed in a mass ratio of 3:2.8:0.8, and an esterification reaction was carried out under a nitrogen atmosphere at a temperature of 220°C and with stirring for 6 hours to obtain a substrate;

[0054] (2) The substrate, 98% pure 2,2-dimethyl-6-bromo-2H-benzo[B][1,4]oxazine-3(4H)-one and 98% pure dioctyltin oxide were mixed uniformly in a mass ratio of 4:1.3:1.2, and stirred continuously for 4 h at a temperature of 200 °C to obtain prepolymer I;

[0055] (3) The substrate, 98% pure N,N'-(4,4'-methylenediphenyl)bismaleimide and 99% pure ethylene glycol were mixed uniformly in a mass ratio of 1:2.3:0.2, and stirred continuously for 2 h at a temperature of 150 °C to obtain prepolymer II;

[0056] (4) The substrate, prepolymer I, prepolymer II and azodicarbonamide are uniformly mixed in a mass ratio of 3:1.3:0.8:0.1, stirred continuously for 4 h at a temperature of 200 °C, vacuum degassed, cured and formed, and vacuum dried to constant weight to obtain modified polyethylene terephthalate, i.e., modified PET.

[0057] The modified PET prepared in the example was subjected to performance testing, and the specific characterization results are as follows:

[0058] Crystallinity detection: During the curing and molding process of the PET material prepared in the example, a solid automatic densitometer was used for testing. The PET material before, during and after curing was made into test samples with a size of 70×20×5 mm. After vacuum drying and weighing, the sample density was detected and recorded. The crystallinity of the PET material prepared in the example was calculated according to the following formula: .

[0059] Where:

[0060] ρ——density of the sample, g / cm 3 ;

[0061] ρ c ——Density of fully crystalline state, g / cm 3 ;

[0062] ρ a ——Density of completely amorphous sample, g / cm 3 .

[0063] Stiffness test: The modified PET material prepared in the example is made into a test sample with a size of 30×5×0.4 mm. An elastic modulus tester is used to record the shear stress and shear strain of the material. The stiffness of the modified PET material is expressed by the shear elastic modulus according to the derivative calculation based on Hooke's law. The specific calculation formula is as follows.

[0064] Where:

[0065] τ——material shear stress, MPa;

[0066] γ——shear strain radian, °.

[0067] Open porosity detection: The modified PET material prepared in the example is made into a test sample with a size of 40×10×0.5 mm. With reference to the measurement method of GB5164-85, molten paraffin is used as the immersion liquid to detect the open porosity of the modified PET material prepared in the example. The test data is recorded and calculated according to the following formula.

[0068] Where:

[0069] m——mass of the test sample in air, g;

[0070] m1——the mass of the test sample in air after immersion, g;

[0071] m2——the mass of the test sample in the liquid medium after immersion, g;

[0072] ρ1——density of the impregnation solution, g / cm2.

[0073] Anti-aging test: The modified PET material prepared in the example was made into a test sample with a size of 80×40×5 mm. A xenon arc lamp aging box was used to simulate sunlight radiation. The test sample was placed in the aging box at a temperature of 100°C for 120 h, and then the stiffness test was performed. The data was recorded and the aging rate was calculated according to the following formula.

[0074] Where:

[0075] G——original stiffness of the test sample, MPa;

[0076] G0——Stiffness after solar radiation, MPa.

[0077]

[0078] In addition, an aluminum test sample A with an inner wall size of 100×60×40 mm and an aluminum test sample B with an outer wall size of 100×60×5 mm were prepared. The modified PET prepared in the embodiment was used to fill the test sample A, and the modified PET prepared in the embodiment was used to cover the test sample B with a covering thickness of 20 mm. A pendulum was used to impact the middle part of the test sample with an impact energy of 1 J and an impact speed of 2.9 m / s. The energy of the impact loss was calculated by the deflection angle before and after the pendulum impact, and the deformation degree of the aluminum part was observed to calculate the tensile strength of the test group.

[0079]

[0080] In the above characterization results, test group A is a modified PET filled test sample A prepared using the embodiment; test group B is a modified PET covered test sample B with a covering thickness of 20 mm. The present invention uses prepolymer II to optimize performance, and generates a ladder structure cross-linked resin by the addition reaction of N, N'-(4,4'-methylenediphenyl) bismaleimide and ethylene glycol ester. At the same time, the reactant reacts with the active sites produced by the modification of 2-ethyl-1,3-hexanediol to form an interpenetrating network structure, thereby increasing the cross-linking density and stiffness of the PET material. When the material is subjected to stress, the interpenetrating network structure hinders crack propagation and improves impact performance. In addition, chemical copolymerization and blending modification make some polymer side chains contain three methylene groups, forming an irregular helical structure and a zigzag conformation similar to proteins, giving the material self-healing ability and improving durability.

[0081] Example 2: A method for preparing modified PET,

[0082] The method comprises:

[0083] (1) 99% pure terephthalic acid, 99% pure ethylene glycol and 98% pure 2-ethyl-1,3-hexanediol were uniformly mixed in a mass ratio of 3:3:1, and an esterification reaction was carried out under a nitrogen atmosphere at a temperature of 230°C and with stirring for 5 hours to obtain a substrate;

[0084] (2) The substrate, 98% pure 2,2-dimethyl-6-bromo-2H-benzo[B][1,4]oxazine-3(4H)-one and 98% pure dioctyltin oxide were mixed uniformly in a mass ratio of 4:1.5:1.4, and stirred continuously for 3 h at a temperature of 210 °C to obtain prepolymer I;

[0085] (3) The substrate, 98% pure N,N'-(4,4'-methylenediphenyl)bismaleimide and 99% pure ethylene glycol were mixed uniformly in a mass ratio of 1:2.5:0.3, and stirred continuously for 1.5 h at a temperature of 170 °C to obtain prepolymer II;

[0086] (4) The substrate, prepolymer I, prepolymer II and azodicarbonamide were uniformly mixed in a mass ratio of 3:1.5:1:0.1, stirred continuously for 3 h at a temperature of 210 °C, vacuum degassed, cured and molded, and vacuum dried to constant weight to obtain modified polyethylene terephthalate, i.e., modified PET.

[0087] The modified PET prepared in the example was subjected to performance testing, and the specific characterization results are as follows:

[0088] Crystallization rate detection: During the curing and molding process of the PET material prepared in the example, a solid automatic densitometer was used for testing. The PET material before, during and after curing was made into test samples with a size of 70×20×5 mm, respectively. After vacuum drying and weighing, the density of the sample was detected and recorded, and the crystallinity of the PET material prepared in the example was calculated according to the following formula.

[0089] Where:

[0090] ρ——density of the sample, g / cm 3 ;

[0091] ρ c ——Density of fully crystalline state, g / cm 3 ;

[0092] ρ a ——Density of completely amorphous sample, g / cm 3 .

[0093] Stiffness test: The modified PET material prepared in the example is made into a test sample with a size of 30×5×0.4 mm. An elastic modulus tester is used to record the shear stress and shear strain of the material. The stiffness of the modified PET material is expressed by the shear elastic modulus according to the derivative calculation based on Hooke's law. The specific calculation formula is as follows.

[0094] Where:

[0095] τ——material shear stress, MPa;

[0096] γ——shear strain radian, °.

[0097] Open porosity detection: The modified PET material prepared in the example is made into a test sample with a size of 40×10×0.5 mm. With reference to the measurement method of GB5164-85, molten paraffin is used as the immersion liquid to detect the open porosity of the modified PET material prepared in the example. The test data is recorded and calculated according to the following formula.

[0098] Where:

[0099] m——mass of the test sample in air, g;

[0100] m1——the mass of the test sample in air after immersion, g;

[0101] m2——the mass of the test sample in the liquid medium after immersion, g;

[0102] ρ1——density of the impregnation solution, g / cm2.

[0103] Anti-aging test: The modified PET material prepared in the example was made into a test sample with a size of 80×40×5 mm. A xenon arc lamp aging box was used to simulate sunlight radiation. The test sample was placed in the aging box at a temperature of 100°C for 120 h, and then the stiffness test was performed. The data was recorded and the aging rate was calculated according to the following formula.

[0104] Where:

[0105] G——original stiffness of the test sample, MPa;

[0106] G0——Stiffness after solar radiation, MPa.

[0107]

[0108] In addition, an aluminum test sample A with an inner wall size of 100×60×40 mm and an aluminum test sample B with an outer wall size of 100×60×5 mm were prepared. The modified PET prepared in the embodiment was used to fill the test sample A, and the modified PET prepared in the embodiment was used to cover the test sample B with a covering thickness of 20 mm. A pendulum was used to impact the middle part of the test sample with an impact energy of 1 J and an impact speed of 2.9 m / s. The energy of the impact loss was calculated by the deflection angle before and after the pendulum impact, and the deformation degree of the aluminum part was observed to calculate the tensile strength of the test group.

[0109]

[0110] In the above characterization results, test group A is test sample A filled with modified PET prepared in the example; test group B is test sample B covered with modified PET having a covering thickness of 20 mm.

[0111] Example 3: A method for preparing modified PET,

[0112] The method comprises:

[0113] (1) 99% pure terephthalic acid, 99% pure ethylene glycol and 98% pure 2-ethyl-1,3-hexanediol were uniformly mixed in a mass ratio of 3:3.2:1.2, and an esterification reaction was carried out under a nitrogen atmosphere at a temperature of 240°C and stirred for 4 hours to obtain a substrate;

[0114] (2) The substrate, 98% pure 2,2-dimethyl-6-bromo-2H-benzo[B][1,4]oxazine-3(4H)-one and 98% pure dioctyltin oxide were mixed uniformly in a mass ratio of 4:1.7:1.6, and stirred continuously for 2 h at a temperature of 220 °C to obtain prepolymer I;

[0115] (3) The substrate, 98% pure N,N'-(4,4'-methylenediphenyl)bismaleimide and 99% pure ethylene glycol were mixed uniformly in a mass ratio of 1:2.7:0.4, and stirred continuously for 1 h at a temperature of 190 °C to obtain prepolymer II;

[0116] (4) The substrate, prepolymer I, prepolymer II and azodicarbonamide were uniformly mixed in a mass ratio of 3:1.7:1.2:0.1, stirred continuously for 2 h at a temperature of 220 °C, vacuum degassed, cured and molded, and vacuum dried to constant weight to obtain modified polyethylene terephthalate, i.e., modified PET.

[0117] The modified PET prepared in the example was subjected to performance testing, and the specific characterization results are as follows:

[0118] Crystallization rate detection: During the curing and molding process of the PET material prepared in the example, a solid automatic densitometer was used for testing. The PET material before, during and after curing was made into test samples with a size of 70×20×5 mm, respectively. After vacuum drying and weighing, the density of the sample was detected and recorded, and the crystallinity of the PET material prepared in the example was calculated according to the following formula.

[0119] Where:

[0120] ρ——density of the sample, g / cm 3 ;

[0121] ρ c ——Density of fully crystalline state, g / cm 3 ;

[0122] ρ a ——Density of completely amorphous sample, g / cm 3 .

[0123] Stiffness test: The modified PET material prepared in the example is made into a test sample with a size of 30×5×0.4 mm. An elastic modulus tester is used to record the shear stress and shear strain of the material. The stiffness of the modified PET material is expressed by the shear elastic modulus according to the derivative calculation based on Hooke's law. The specific calculation formula is as follows.

[0124] Where:

[0125] τ——material shear stress, MPa;

[0126] γ——shear strain radian, °.

[0127] Open porosity detection: The modified PET material prepared in the example is made into a test sample with a size of 40×10×0.5 mm. With reference to the measurement method of GB5164-85, molten paraffin is used as the immersion liquid to detect the open porosity of the modified PET material prepared in the example. The test data is recorded and calculated according to the following formula.

[0128] Where:

[0129] m——the mass of the test sample in the air, g;

[0130] m1——the mass of the test sample in air after immersion, g;

[0131] m2——the mass of the test sample in the liquid medium after immersion, g;

[0132] ρ1——density of the impregnation solution, g / cm2.

[0133] Anti-aging test: The modified PET material prepared in the example was made into a test sample with a size of 80×40×5 mm. A xenon arc lamp aging box was used to simulate sunlight radiation. The test sample was placed in the aging box at a temperature of 100°C for 120 h, and then the stiffness test was performed. The data was recorded and the aging rate was calculated according to the following formula.

[0134] Where:

[0135] G——original stiffness of the test sample, MPa;

[0136] G0——Stiffness after solar radiation, MPa.

[0137]

[0138] In addition, an aluminum test sample A with an inner wall size of 100×60×40 mm and an aluminum test sample B with an outer wall size of 100×60×5 mm were prepared. The modified PET prepared in the embodiment was used to fill the test sample A, and the modified PET prepared in the embodiment was used to cover the test sample B with a covering thickness of 20 mm. A pendulum was used to impact the middle part of the test sample with an impact energy of 1 J and an impact speed of 2.9 m / s. The energy of the impact loss was calculated by the deflection angle before and after the pendulum impact, and the deformation degree of the aluminum part was observed to measure the tensile strength of the test group.

[0139]

[0140] In the above characterization results, test group A is test sample A filled with modified PET prepared in the example; test group B is test sample B covered with modified PET having a covering thickness of 20 mm.

[0141] Comparative Example 1: A method for preparing a modified PET, the specific preparation method is the same as that of Example 2, only the preparation steps of the modified PET material unique to the present invention are changed, and the PET material is prepared using a one-step method, and the specific operations are as follows:

[0142] A method for preparing modified PET,

[0143] The method comprises:

[0144] Terephthalic acid with a purity of 99%, ethylene glycol with a purity of 99%, 2,2-dimethyl-6-bromo-2H-benzo[B][1,4]oxazine-3(4H)-one with a purity of 98%, dioctyltin oxide with a purity of 98%, N,N'-(4,4'-methylenediphenyl)bismaleimide with a purity of 98% and ethylene glycol with a purity of 99% are reacted in a nitrogen atmosphere at a temperature of 230°C with a stirring reaction for 12.5 h, vacuum degassing, solidification molding, and vacuum drying to constant weight to obtain modified polyethylene terephthalate, that is, modified PET.

[0145] The PET material prepared in the comparative example was tested for performance in the same manner as in the example, and the characterization results are as follows.

[0146]

[0147] In addition, the pendulum impact test results are as follows.

[0148]

[0149] In the above characterization results, test group A is test sample A filled with modified PET prepared in the example; test group B is test sample B covered with modified PET having a covering thickness of 20 mm.

[0150] By comparing the above characterization results with those of Example 2, it is found that the open porosity of the PET material prepared in the comparative example is improved, while the other tests are decreased to varying degrees. The inventors speculate that since the one-step reaction cannot be controlled, the expected spatial arrangement cannot be formed inside the material, resulting in the formation of a disordered structural system, which not only fails to enhance the mechanical properties of the PET material, but instead causes its performance to decline.

[0151] Comparative Example 2: A method for preparing a modified PET, the specific preparation method is the same as that of Example 2, except that the unique prepolymer II of the present invention is not prepared and used, and the PET material is prepared. The specific operations are as follows:

[0152] A method for preparing modified PET,

[0153] The method comprises:

[0154] (1) 99% pure terephthalic acid, 99% pure ethylene glycol and 98% pure 2-ethyl-1,3-hexanediol were uniformly mixed in a mass ratio of 3:3:1, and an esterification reaction was carried out under a nitrogen atmosphere at a temperature of 230°C and with stirring for 5 hours to obtain a substrate;

[0155] (2) The substrate, 98% pure 2,2-dimethyl-6-bromo-2H-benzo[B][1,4]oxazine-3(4H)-one and 98% pure dioctyltin oxide were mixed uniformly in a mass ratio of 4:1.5:1.4, and stirred continuously for 3 h at a temperature of 210 °C to obtain prepolymer I;

[0156] (3) The substrate, prepolymer I and azodicarbonamide are uniformly mixed in a mass ratio of 3:1.5:1:0.1, stirred continuously for 3 h at a temperature of 210 °C, vacuum degassed, cured and molded, and vacuum dried to constant weight to obtain modified polyethylene terephthalate, i.e., modified PET.

[0157] The PET material prepared in the comparative example was tested for performance in the same manner as in the example, and the characterization results are as follows.

[0158]

[0159] In addition, the pendulum impact test results are as follows.

[0160]

[0161] In the above characterization results, test group A is test sample A filled with modified PET prepared in the example; test group B is test sample B covered with modified PET having a covering thickness of 20 mm.

[0162] By comparing the above characterization results with those of Example 2, it is found that the stiffness and anti-aging ability of the PET material prepared in the comparative example are significantly reduced. The inventors have found through research that if the present invention only uses a metal-organic skeleton to reinforce the PET material structure, it will lead to the degeneration of mechanical properties. The compatibility of the metal-organic skeleton with PET is poor, and self-agglomeration occurs, resulting in structural collapse inside the material. When subjected to external force, the force will accumulate at the collapsed location, accelerating the destruction speed of the material, and the material will break due to excessive local stress.

[0163] Comparative Example 3: A method for preparing a modified PET, the specific preparation method is the same as that of Example 2, except that the unique prepolymer I of the present invention is not prepared and used, and the PET material is prepared. The specific operations are as follows:

[0164] A method for preparing modified PET,

[0165] The method comprises:

[0166] (1) 99% pure terephthalic acid, 99% pure ethylene glycol and 98% pure 2-ethyl-1,3-hexanediol were uniformly mixed in a mass ratio of 3:3:1, and an esterification reaction was carried out under a nitrogen atmosphere at a temperature of 230°C and with stirring for 5 hours to obtain a substrate;

[0167] (2) The substrate, 98% pure N,N'-(4,4'-methylenediphenyl)bismaleimide and 99% pure ethylene glycol were mixed uniformly in a mass ratio of 1:2.5:0.3, and stirred continuously for 1.5 h at a temperature of 170 °C to obtain prepolymer II;

[0168] (4) The substrate, prepolymer II and azodicarbonamide were mixed uniformly in a mass ratio of 3:1:0.1, stirred continuously for 3 h at a temperature of 210°C, vacuum degassed, cured and molded, and vacuum dried to constant weight to obtain modified polyethylene terephthalate, i.e., modified PET.

[0169] The PET material prepared in the comparative example was tested for performance in the same manner as in the example, and the characterization results are as follows.

[0170]

[0171] In addition, the pendulum impact test results are as follows.

[0172]

[0173] In the above characterization results, test group A is test sample A filled with modified PET prepared in the example; test group B is test sample B covered with modified PET having a covering thickness of 20 mm.

[0174] By comparing the above characterization results with Example 2, it is found that the crystallinity of the PET material prepared in the comparative example is improved, but the stiffness and aging resistance are reduced, especially the anti-aging ability is significantly reduced. According to the research and observation of the inventors, when the metal-organic skeleton is not used as the main supporting structure inside the material, as the temperature and external force gradually increase, the stiffness of the material prepared in the comparative example gradually decreases, and the yield displacement of the material itself decreases, resulting in instability inside the material, affecting the mechanical properties of the material.

[0175] Comparative Example 4: A method for preparing a modified PET, the specific preparation method is the same as that of Example 2, except that the substrate unique to the present invention is not prepared and used, and an equal amount of commercially available PET material particles are used instead to prepare the PET material, and the specific operation is as follows:

[0176] A method for preparing modified PET,

[0177] The method comprises:

[0178] (1) Commercially available PET material particles, 98% pure 2,2-dimethyl-6-bromo-2H-benzo[B][1,4]oxazine-3(4H)-one and 98% pure dioctyltin oxide were mixed uniformly in a mass ratio of 4:1.5:1.4, and stirred continuously for 3 h at a temperature of 210 °C to obtain prepolymer I;

[0179] (2) Commercially available PET material particles, 98% pure N,N'-(4,4'-methylenediphenyl) bismaleimide and 99% pure ethylene glycol were mixed in a mass ratio of 1:2.5:0.3, and stirred continuously for 1.5 hours at a temperature of 170 °C to obtain prepolymer II;

[0180] (3) Commercially available PET material particles, prepolymer I, prepolymer II and azodicarbonamide were mixed uniformly in a mass ratio of 3:1.5:1:0.1, stirred continuously for 3 h at a temperature of 210 °C, vacuum degassed, cured and formed, and vacuum dried to constant weight to obtain modified polyethylene terephthalate, that is, modified PET.

[0181] The PET material prepared in the comparative example was tested for performance in the same manner as in the example, and the characterization results are as follows.

[0182]

[0183] In addition, the pendulum impact test results are as follows.

[0184]

[0185] In the above characterization results, test group A is test sample A filled with modified PET prepared in the example; test group B is test sample B covered with modified PET having a covering thickness of 20 mm.

[0186] By comparing the above characterization results with Example 2, it is found that the crystallinity of the PET material prepared in the comparative example is increased and the rigidity is enhanced, but the anti-aging ability is significantly reduced. After research and observation by the inventors, in the technical scheme of the present invention, the carboxyl group combines with the hydroxyl group in PET to form an ester bond, thereby improving the stability of the copolyester, solving the problem that the nucleating agent is easy to break the PET molecular chain, and improving the mechanical properties of the modified copolyester. At the same time, 2-ethyl-1,3-hexanediol is blended and grafted with the rigid benzene ring of polyethylene terephthalate to create subsequent active sites, promote esterification and polycondensation reactions, blend and granulate high molecular polymers, control the arrangement order of the internal molecular chains of the modified PET, and ensure the stability of the mechanical properties of the material.

[0187] Comparative Example 5: A commercially available PET material was characterized by the same properties as those in Example 2. The specific characterization results are as follows.

[0188]

[0189] In addition, the pendulum impact test results are as follows.

[0190]

[0191] In the above characterization results, test group A is test sample A filled with modified PET prepared in the example; test group B is test sample B covered with modified PET having a covering thickness of 20 mm.

[0192] From the comparison between the above characterization results and Example 2, it is found that the commercially available filling core material has higher rigidity, but the anti-aging performance is insufficient. The material provided by the present invention is more stable inside and has a special arrangement structure, which can further absorb and disperse the impact force and improve the durability and stability of the material. The inventors have found through experiments that such structures in the material exist at -70 to 110°C, which broadens the application field of the modified PET material provided by the technical solution of the present invention.

[0193] The self-healing performance of Example 2 and Comparative Examples 1 to 5 was tested. The modified PET materials prepared in Example 2 and Comparative Examples 1 to 4 were made into I-type dumbbell molds with reference to the spline size of GB / T2567-2008. The spline was gradually stretched to 200% of the original length at a loading speed of 5 mm / min at room temperature, and then the stretching was stopped. The length data was recorded after no more deformation occurred. The specific characterization results are as follows.

[0194]

[0195] In the above characterization results, the recovery rate = (2×original spline length-length after no deformation) / original spline length×100%, and if the spline breaks, it is "-".

[0196] After in-depth analysis of the above characterization results, the technical solution of the present invention successfully induces the polymer molecular chain to exhibit a unique "Z"-shaped spiral conformation by using the modification means of chemical copolymerization and blending. This unique conformation gives the polymer macromolecular chain a deformation and recovery ability similar to a spring, which greatly enriches the performance of the polymer. The particularity of this spiral conformation is that when the polymer molecular chain is subjected to external force, it can elongate, absorb and disperse the external force, and when the external force is eliminated, the molecular chain can gradually return to its original state, showing strong elasticity. This deformation and recovery ability not only greatly improves the toughness of the material, but also gives the polymer a self-repairing ability. When the material has tiny cracks, this characteristic of the molecular chain enables the polymer around the crack to rearrange and fill the crack, thereby restoring the integrity and performance of the material. This self-repairing ability greatly extends the service life of the material, while also reducing the frequency of maintenance and replacement, and has extremely high practical value. In addition, this unique spiral conformation also enables the polymer to disperse and buffer external forces when subjected to external forces, thereby effectively preventing stress concentration and damage. This property enables the polymer to exhibit extremely high durability and stability when subjected to repeated stress or cyclic loads. In general, the technical solution of the present invention successfully induces the polymer molecular chain to exhibit a unique "zigzag" helical conformation through the modification means of chemical copolymerization and blending, giving the polymer macromolecular chain a deformation and recovery ability similar to that of a spring. This characteristic not only improves the toughness of the material, but also enables it to have the ability to self-repair. It has extremely high practical value and broad application prospects. The technical solution of the present invention realizes the effective regulation and optimization of polymer properties, and provides new ideas and approaches for the development of the field of materials science.

Claims

1. A method for preparing modified PET, It is characterized in that The method comprises: (1) mixing cyclic carboxylic acid, acyclic alcohol and hexanol derivative in proportion, and subjecting the mixture to an esterification reaction to obtain a substrate; (2) mixing the substrate, the condensed ring compound and the organotin in proportion, heating and stirring, to obtain a prepolymer I; (3) mixing the substrate, imide and acyclic alcohol in proportion, heating and stirring, to obtain prepolymer II; (4) mixing the substrate, prepolymer I, prepolymer II and foaming agent in proportion, heating and stirring, and obtaining modified polyethylene terephthalate, that is, obtaining modified PET; The cyclic carboxylic acid in step (1) is terephthalic acid; The acyclic alcohol in step (1) is ethylene glycol; The hexanol derivative in step (1) is 2-ethyl-1,3-hexanediol; The cyclic carboxylic acid, acyclic alcohol and hexanol derivative in step (1) are uniformly mixed in a mass ratio of 3: (2.8-3.2): (0.8-1.2); The fused ring compound in step (2) is 2,2-dimethyl-6-bromo-2H-benzo[B][1,4]oxazin-3(4H)-one; The imide in step (3) is N,N'-(4,4'-methylenediphenyl)bismaleimide; The acyclic alcohol in step (3) is ethylene glycol; In step (3), the substrate, imide and acyclic alcohol are uniformly mixed in a mass ratio of 1: (2.3-2.7): (0.2-0.4).

2. A method for preparing modified PET according to claim 1, It is characterized in that The esterification reaction in step (1) is carried out under a nitrogen atmosphere at a temperature of 220-240° C. and stirred for 4-6 hours.

3. A method for preparing modified PET according to claim 1, It is characterized in that The organotin in step (2) is dioctyltin oxide; In step (2), the substrate, the condensed ring compound and the organotin are uniformly mixed in a mass ratio of 4: (1.3-1.7): (1.2-1.6).

4. A method for preparing a modified PET according to claim 1 or 3, It is characterized in that The heating and stirring in step (2) is carried out at a temperature of 200 to 220° C. and the stirring is continued for 2 to 4 hours.

5. A method for preparing modified PET according to claim 1, It is characterized in that The heating and stirring in step (3) is carried out at a temperature of 150 to 190 °C and the stirring is continued for 1 to 2 hours.

6. A method for preparing modified PET according to claim 1, It is characterized in that The foaming agent in step (4) is azodicarbonamide; In step (4), the substrate, prepolymer I, prepolymer II and foaming agent are uniformly mixed in a mass ratio of 3: (1.3-1.7): (0.8-1.2): 0.

1.

7. A method for preparing a modified PET according to claim 1 or 6, It is characterized in that The heating and stirring in step (4) is carried out at a temperature of 200 to 220° C., stirring is continued for 2 to 4 hours, vacuum degassing, solidification and vacuum drying are carried out to constant weight.

8. A modified PET obtained by the method according to any one of claims 1 to 7.