A high-performance TPU composite material for cables and preparation method thereof
By combining thermoplastic polyurethane TPU, polyolefin elastomer and other components in the cable material, high-performance TPU composite materials are formed, which solves the problem of multiple performance requirements of charging pile cable materials and achieves the improvement of reliability and safety of electric vehicle charging cables.
Patent Information
- Application Number
- CN202410485568.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-22
AI Technical Summary
The existing charging pile cable sheath material is difficult to meet the multiple performance requirements such as ultraviolet resistance, high temperature resistance, low temperature resistance, water resistance, acid and alkali resistance, and oil resistance. At the same time, the flexibility and mechanical properties are insufficient, making it difficult to meet the needs of electric vehicle charging cables.
Thermoplastic polyurethane TPU is used as the basic material, combining polyolefin elastomer, HDPE, composite flame retardant, hydrolyzer, silicone masterbatch, modified nanotitanium dioxide, ultraviolet absorbers and antioxidants to form high-performance TPU composite materials, improving Its flexibility, wear resistance, mechanical properties, weather resistance and flame retardancy.
It has achieved the flexibility, wear resistance, mechanical properties, weather resistance and flame retardancy of high-performance TPU composite materials, and complies with the standards for charging cables for electric vehicles, ensuring the reliability and safety of the cables in harsh environments.
Smart Images

Figure BDA0004803611870000081 
Figure BDA0004803611870000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of cable materials, and in particular to a high-performance TPU composite material for cables and a preparation method thereof. Background Art
[0002] As the country pays more and more attention to environmental protection, new energy electric vehicles have emerged. At present, my country is the country with the largest production and sales of new energy vehicles in the world, and also the country with the largest number of electric vehicle users. Under such a background, the charging pile industry chain supporting electric vehicles has become a hot industry, and a large number of charging piles have been built rapidly. The accompanying electric vehicle charging cables have also brought unprecedented market prospects.
[0003] Electric vehicle charging cables are used to transmit power between electric vehicles and charging piles. They are generally installed outdoors and therefore have to withstand harsh climates such as wind, sun, and cold. Therefore, the sheath material of the charging pile cable is required to be resistant to ultraviolet rays, high temperature, low temperature, water, acid, alkali, and oil. For easy wiring and use, the cable is required to be flexible and have a small bending radius; in the process of charging electric vehicles, the cable is subject to dragging and friction, so the cable sheath material is required to be wear-resistant, have good mechanical properties, tensile resistance, tear resistance, twisting resistance, and water resistance.
[0004] The materials currently used in the market for producing charging pile cable sheaths can also meet the above requirements. Therefore, it is necessary to develop a high-performance TPU composite material that has good flexibility, excellent mechanical properties, water resistance and flame retardancy, and meets the standards for electric vehicle charging cables. Summary of the invention
[0005] The purpose of this application is to provide a high-performance TPU composite material for cables and a preparation method thereof in response to the deficiencies of current technology. The high-performance TPU composite material prepared in this application has good flexibility and wear resistance, as well as excellent mechanical properties, water resistance and flame retardancy, and meets the standards for electric vehicle charging cables.
[0006] In the first aspect, the present application provides a high-performance TPU composite material for cables, which adopts the following technical solution:
[0007] A high-performance TPU composite material for cables comprises the following raw materials by weight: 60-65 parts of thermoplastic polyurethane TPU, 15-20 parts of polyolefin elastomer, 5-8 parts of HDPE, 6-8 parts of composite flame retardant, 0.05-0.1 parts of hydrolysis resistance agent, 3-5 parts of silicone masterbatch, 5-7 parts of modified nano titanium dioxide, 0.1-0.2 parts of ultraviolet absorber, 0.2-0.5 parts of calcium stearate, and 0.3-0.5 parts of antioxidant; wherein the composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage polysilsesquioxane.
[0008] By adopting the above technical solutions, thermoplastic polyurethane TPU: as a basic material, provides the flexibility and wear resistance of the material. Polyolefin elastomer: increases the elasticity and toughness of the material, improves the wear resistance and impact resistance. HDPE: increases the hardness and strength of the material, improves the wear resistance and mechanical properties. Composite flame retardant: composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage polysilsesquioxane. The composite flame retardant can provide the flame retardant properties of the material, and at the same time improve the water resistance and mechanical properties through compatibility with the substrate. Hydrolysis resistance agent: improves the water resistance of the material and avoids the degradation of the material in a humid environment. Silicone masterbatch: provides the thickening effect of the material and improves the processing performance of the material. Modified nano titanium dioxide: increases the weather resistance and UV resistance of the material and improves the wear resistance of the material. UV absorber: absorbs ultraviolet rays, protects the material from damage by ultraviolet rays, and improves weather resistance. Antioxidant: inhibits the oxidative degradation process of the material and extends the service life of the material. In summary, the effects and synergy of the components can provide the flexibility, wear resistance, mechanical properties, weather resistance, water resistance and flame retardancy of high-performance TPU composites, making them meet the standards for electric vehicle charging cables.
[0009] Preferably, the mass ratio of the modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage polysilsesquioxane is 7:2:1-3.
[0010] By adopting the above technical scheme, modified phenyl aluminum phosphite: has excellent flame retardant properties, and improves the water resistance, flame retardant properties and mechanical properties of the composite material through the compatibility of the flame retardant and the substrate. The modified phenyl aluminum phosphite has a large contact area with the substrate, which can better improve the compatibility of the composite flame retardant and the substrate. Octave vinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane: as auxiliary flame retardants, through the synergistic effect with modified phenyl aluminum phosphite, the flame retardant properties of the composite material are further improved. In summary, the modified phenyl aluminum phosphite, octavinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane in the composite flame retardant can improve the water resistance, flame retardant properties and mechanical properties of high-performance TPU composite materials for cables through compatibility and synergy.
[0011] Preferably, the preparation method of the modified phenyl aluminum hypophosphite is as follows: according to the mass fractions, under nitrogen protection, phenyl aluminum hypophosphite, polymethylphenylsiloxane and trimethyl borate are added to a reactor and placed in a heating jacket for heating and stirring, the heating temperature is set to 190-210°C, the heating rate is 6°C / minute, the stirring rate is 300rpm, and water is distilled off at the same time; after reacting for 30-40 minutes, the product is placed in anhydrous ethanol and completely dissolved, and then deionized water is poured into it to precipitate the product, the precipitated product is filtered and vacuum dried at 80°C for 36 hours, and then ground and sieved to obtain modified phenyl aluminum hypophosphite.
[0012] By adopting the above technical solution, the modified phenyl aluminum hypophosphite is used as one of the key components of the composite flame retardant, which can improve the flame retardant properties of the composite material. Its large contact area with the substrate helps to improve the compatibility of the composite flame retardant and the substrate, thereby improving the water resistance, flame retardant properties and mechanical properties of the composite material.
[0013] Preferably, the mass ratio of the phenyl aluminum hypophosphite, polymethylphenylsiloxane, trimethyl borate, anhydrous ethanol and deionized water is 10:(3-5):(1-3):30:200.
[0014] Preferably, the preparation method of the modified nano titanium dioxide is to add 500 parts of nano titanium dioxide and 190 parts of calcium peroxide to 500 parts of a phosphoric acid solution with a mass concentration of 12 g / L, and continue the reaction for 30-40 minutes, then filter and dry to obtain modified nano titanium dioxide, wherein the average particle size of the nano titanium dioxide is 30 nm.
[0015] By adopting the above technical scheme, hydroxyl radicals can be continuously formed after calcium peroxide reacts and dissolves in dilute phosphoric acid, and hydroxyl radicals can be replenished at a uniform rate. The number of hydroxyl groups on the surface of nano-titanium dioxide is increased by the above surface treatment, and the other end of the hydroxyl group can copolymerize or bond with the vacant functional group of the substrate to form an interpenetrating network structure, thereby improving the water resistance and mechanical properties of the composite material, while also improving the weather resistance.
[0016] Preferably, the ultraviolet absorber is composed of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a mass ratio of 2:(3-5):(1-3).
[0017] By adopting the above technical scheme, the compounds in the UV absorber can absorb UV light, thereby protecting the composite material from the influence of UV light. This helps to extend the service life of the material and improve its weather resistance. UV light can cause material aging, including fading of color, reduction of mechanical properties, etc. Adding UV absorbers can effectively prevent material aging caused by UV light and maintain the appearance and performance of the material stable. The synergistic effect of UV absorbers and other raw materials helps to improve the weather resistance of high-performance TPU composite materials. In summary, UV absorbers play a role in protecting materials from the influence of UV light in high-performance TPU composite materials, and through synergistic effect with other raw materials, they can improve the weather resistance and stability of the material.
[0018] Preferably, the anti-hydrolysis agent is composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:(1-3):(2-4).
[0019] By adopting the above technical solution, the main function of the anti-hydrolysis agent is to improve the hydrolysis resistance of the composite material, that is, the performance of the material can remain stable under humid conditions. By forming compatibility with the substrate and preventing moisture from penetrating into the material, the water resistance of the composite material is improved. The addition of the anti-hydrolysis agent can improve the flexibility and plasticity of the material, thereby improving the wear resistance of the composite material. This is because the anti-hydrolysis agent can copolymerize or bond with the substrate to form an interpenetrating network structure, thereby increasing the flexibility of the material.
[0020] Preferably, the antioxidant is tris(2,4-di-tert-butylphenyl) phosphite.
[0021] In a second aspect, the present application provides a method for preparing a high-performance TPU composite material for cables, using the following technical solution:
[0022] As a general technical concept, the present application also provides a method for preparing the above-mentioned high-performance TPU composite material for cables, comprising the following steps:
[0023] S91. Place thermoplastic polyurethane, polyolefin elastomer, HDPE, composite flame retardant, hydrolysis resistance agent, silicone masterbatch, modified nano titanium dioxide, ultraviolet absorber, calcium stearate and antioxidant in a high-speed mixer according to their mass fractions, and mix for 5-10 minutes to obtain a mixture;
[0024] S92, putting the mixed material into a twin-screw extruder, melting and mixing, extruding and granulating, and obtaining a high-performance TPU composite material for cables.
[0025] Preferably, in step S92, the processing parameters of the twin-screw extruder are: extrusion temperature is 180-200°C, and screw speed is 200-240rpm.
[0026] In summary, the beneficial technical effects of this application are:
[0027] 1. Good flexibility and wear resistance: By adding thermoplastic polyurethane TPU and polyolefin elastomer, the composite material has good flexibility and wear resistance, and can withstand long-term use and frequent bending without being easily damaged.
[0028] 2. Excellent mechanical properties and weather resistance: Due to the raw materials such as HDPE, silicone masterbatch, modified nano titanium dioxide and antioxidants, the composite material has excellent mechanical strength, impact resistance and weather resistance, and can adapt to use in harsh environmental conditions.
[0029] 3. Excellent water resistance and flame retardancy: The composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage polysilsesquioxane, which can improve the compatibility of the composite flame retardant with the substrate, thereby making the composite material have excellent water resistance and flame retardancy.
[0030] 4. Comply with the standard requirements of electric vehicle charging cables: The high-performance TPU composite material used in cables has passed the requirements of electric vehicle charging cable standards, ensuring its reliability and safety in the field of electric vehicle charging. DETAILED DESCRIPTION
[0031] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0032] Preparation Example 1 Preparation of modified phenyl aluminum hypophosphite
[0033] The preparation method of modified phenyl aluminum hypophosphite is as follows: according to the mass fraction, under nitrogen protection, 10 kg of phenyl aluminum hypophosphite, 4 kg of polymethylphenylsiloxane and 2 kg of trimethyl borate are added into a reactor and placed in a heating jacket for heating and stirring, the heating temperature is set to 200°C, the heating rate is 6°C / minute, the stirring rate is 300 rpm, and water is distilled off at the same time; after reacting for 35 minutes, the product is placed in 30 kg of anhydrous ethanol and completely dissolved, and then 200 kg of deionized water is poured into it to precipitate the product, the precipitated product is filtered and vacuum dried at 80°C for 36 hours, and then ground and sieved to obtain modified phenyl aluminum hypophosphite.
[0034] The modified phenyl aluminum hypophosphite prepared above was applied to various examples and comparative examples.
[0035] Preparation Example 2 Preparation of modified nano titanium dioxide
[0036] The preparation method of modified nano titanium dioxide is as follows: 500 parts of nano titanium dioxide and 190 parts of calcium peroxide are added to 500 parts of a phosphoric acid solution with a mass concentration of 12 g / L according to the mass fraction, the reaction is continued for 30-40 minutes, and then filtered and dried to obtain modified nano titanium dioxide, wherein the average particle size of the nano titanium dioxide is 30 nm.
[0037] The modified nano titanium dioxide prepared above was applied to various examples and comparative examples.
[0038] Example 1
[0039] A high-performance TPU composite material for cables comprises the following raw materials, measured by weight: 60 kg of thermoplastic polyurethane TPU, 15 kg of polyolefin elastomer, 5 kg of HDPE, 6 kg of composite flame retardant, 0.05 kg of hydrolysis resistance agent, 3 kg of silicone masterbatch, 5 kg of modified nano titanium dioxide, 0.1 kg of ultraviolet absorber, 0.2 kg of calcium stearate, and 0.3 kg of tris(2,4-di-tert-butylphenyl) phosphite; wherein the composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane in a weight ratio of 7:2:1; and the ultraviolet absorber is composed of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a weight ratio of 2:3:1. The anti-hydrolysis agent is composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:1:2.
[0040] The method for preparing the high-performance TPU composite material for cables comprises the following steps:
[0041] S91. Place thermoplastic polyurethane, polyolefin elastomer, HDPE, composite flame retardant, hydrolysis resistance agent, silicone masterbatch, modified nano titanium dioxide, ultraviolet absorber, calcium stearate and tris(2,4-di-tert-butylphenyl) phosphite in a high-speed mixer according to their mass fractions, and mix for 5 minutes to obtain a mixture;
[0042] S92, putting the mixed material into a twin-screw extruder, melt-mixing, extruding and granulating, the extrusion temperature is 180° C., the screw speed is 240 rpm, and a high-performance TPU composite material for cables is obtained.
[0043] Example 2
[0044] A high-performance TPU composite material for cables comprises the following raw materials, measured by weight: 65 kg of thermoplastic polyurethane TPU, 20 kg of polyolefin elastomer, 8 kg of HDPE, 8 kg of composite flame retardant, 0.1 kg of hydrolysis resistance agent, 5 kg of silicone masterbatch, 7 kg of modified nano titanium dioxide, 0.2 kg of ultraviolet absorber, 0.5 kg of calcium stearate, and 0.5 kg of tris(2,4-di-tert-butylphenyl) phosphite; wherein the composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane in a weight ratio of 7:2:3; and the ultraviolet absorber is composed of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a weight ratio of 2:5:3. The anti-hydrolysis agent is composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:3:4.
[0045] The method for preparing the high-performance TPU composite material for cables comprises the following steps:
[0046] S91. Place thermoplastic polyurethane, polyolefin elastomer, HDPE, composite flame retardant, hydrolysis resistance agent, silicone masterbatch, modified nano titanium dioxide, ultraviolet absorber, calcium stearate and tris(2,4-di-tert-butylphenyl) phosphite in a high-speed mixer according to their weight fractions, and mix for 10 minutes to obtain a mixture;
[0047] S92. The mixed material is put into a twin-screw extruder for melt mixing and extrusion granulation. The extrusion temperature is 200° C. and the screw speed is 200 rpm to obtain a high-performance TPU composite material for cables.
[0048] Example 3
[0049] A high-performance TPU composite material for cables comprises the following raw materials, measured by weight: 63 kg of thermoplastic polyurethane TPU, 18 kg of polyolefin elastomer, 7 kg of HDPE, 7 kg of composite flame retardant, 0.08 kg of hydrolysis resistance agent, 4 kg of silicone masterbatch, 6 kg of modified nano titanium dioxide, 0.15 kg of ultraviolet absorber, 0.4 kg of calcium stearate, and 0.4 kg of tris(2,4-di-tert-butylphenyl) phosphite; wherein the composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane in a weight ratio of 7:2:2; and the ultraviolet absorber is composed of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a weight ratio of 2:4:2. The anti-hydrolysis agent is composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:2:3.
[0050] The method for preparing the high-performance TPU composite material for cables comprises the following steps:
[0051] S91. According to the mass fractions, thermoplastic polyurethane, polyolefin elastomer, HDPE, composite flame retardant, hydrolysis resistance agent, silicone masterbatch, modified nano titanium dioxide, ultraviolet absorber, calcium stearate and tris(2,4-di-tert-butylphenyl) phosphite are placed in a high-speed mixer and mixed for 8 minutes to obtain a mixture;
[0052] S92. The mixed material is put into a twin-screw extruder for melt mixing and extrusion granulation. The extrusion temperature is 190° C. and the screw speed is 220 rpm to obtain a high-performance TPU composite material for cables.
[0053] Example 4
[0054] The same as Example 3, except that an equal amount of 2,4-dihydroxybenzophenone is used instead of the ultraviolet absorber, and the ultraviolet absorber is composed of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a mass ratio of 2:4:2.
[0055] Example 5
[0056] The same as Example 3, except that an equal amount of phenyl o-hydroxybenzoate is used instead of the ultraviolet absorber, and the ultraviolet absorber is composed of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a mass ratio of 2:4:2.
[0057] Example 6
[0058] The same as Example 3, except that an equal amount of N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine is used instead of the ultraviolet absorber, and the ultraviolet absorber is composed of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a mass ratio of 2:4:2.
[0059] Example 7
[0060] The same as Example 3, except that an equal amount of carbodiimide is used to replace the anti-hydrolysis agent, and the anti-hydrolysis agent is composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:2:3.
[0061] Example 8
[0062] The same as Example 3, except that an equal amount of phenyl glycidyl ether is used to replace the anti-hydrolysis agent, and the anti-hydrolysis agent is composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:2:3.
[0063] Example 9
[0064] The same as Example 3, except that an equal amount of bisphenol A diglycidyl ester is used to replace the anti-hydrolysis agent, and the anti-hydrolysis agent is composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:2:3.
[0065] Comparative Example 1
[0066] The same as Example 3, except that an equal amount of nano titanium dioxide with an average particle size of 30 nm is used to replace the modified nano titanium dioxide prepared in Preparation Example 2.
[0067] Comparative Example 2
[0068] The same as Example 3, except that an equal amount of phenyl aluminum phosphite is used to replace the modified phenyl aluminum phosphite prepared in Preparation Example 1.
[0069] Comparative Example 3
[0070] The same as Example 3, except that an equal amount of modified phenyl aluminum phosphite is used instead of the composite flame retardant, and the composite flame retardant is composed of modified phenyl aluminum phosphite, octavinyl cage polysilsesquioxane and octaphenyl cage polysilsesquioxane in a mass ratio of 7:2:2.
[0071] Comparative Example 4
[0072] The same as Example 3, except that an equal amount of octavinyl cage polysilsesquioxane is used to replace the composite flame retardant, and the composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane in a mass ratio of 7:2:2.
[0073] Comparative Example 5
[0074] The same as Example 3, except that an equal amount of octaphenyl cage silsesquioxane is used to replace the composite flame retardant, and the composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane in a mass ratio of 7:2:2.
[0075] Performance Testing
[0076] The high-performance TPU composite materials for cables prepared in Examples 1 to 9 and Comparative Examples 1 to 5 were sampled and tested. The test results are shown in Table 1.
[0077] The tensile strength and elongation at break were tested according to the standard ASTM-D412;
[0078] The tear strength is tested according to the standard ASTM-D624;
[0079] The flame retardancy level is tested according to the UL94 vertical burning test method, and the flame retardancy levels are V-0, V-1, and V-2 from high to low; the high temperature aging test conditions are: place the sample at 100°C for 168 hours, take it out and let it stand at room temperature for 2 hours, and test the tensile strength and elongation at break;
[0080] The water resistance test conditions are as follows: place the sample in 80°C water for 168 hours, take it out and let it stand at room temperature for 1 hour, and then test the tensile strength and elongation at break.
[0081] Table 1 Performance test
[0082]
[0083]
[0084] Analyzing the data in Table 1, we can see that:
[0085] 1) The high-performance TPU composite materials for cables prepared in Examples 1 to 3 have high flame retardancy, good mechanical properties, and good heat resistance and water resistance.
[0086] 2) A comparative analysis of the performance of the high-performance TPU composite materials for cables prepared in combination with Examples 3 and 4 to 6 shows that the use of an ultraviolet absorber consisting of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a mass ratio of 2:4:2 and the synergistic effect therebetween can improve the heat resistance and water resistance of the high-performance TPU composite material for cables.
[0087] 3) A comparative analysis of the performance of the high-performance TPU composite materials for cables prepared in combination with Example 3 and Example 7-Example 9 shows that the use of a hydrolysis-resistant agent composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:2:3 and the synergistic effect therebetween can improve the water resistance of the high-performance TPU composite materials for cables.
[0088] 4) The comparative analysis of the performance of the high-performance TPU composite materials for cables prepared in combination with Example 3 and Comparative Example 1 shows that the modified nano-titanium dioxide prepared in Preparation Example 2 can continuously form hydroxyl radicals after calcium peroxide is reacted and dissolved in dilute phosphoric acid by adopting the above-mentioned technical scheme, and the hydroxyl radicals can be replenished at a uniform rate. The number of hydroxyl groups on the surface of the nano-titanium dioxide is increased by the above-mentioned surface treatment, and the other end of the hydroxyl group can copolymerize or bond with the vacant functional group of the substrate to form an interpenetrating network structure, thereby improving the comprehensive performance of the composite material.
[0089] 5) The comparative analysis of the performance of the high-performance TPU composite materials for cables prepared in Example 3 and Comparative Example 2 shows that the modified phenyl aluminum hypophosphite has a large contact area with the substrate, which helps to improve the compatibility of the composite flame retardant and the substrate, thereby improving the flame retardant properties and mechanical properties of the composite material.
[0090] 6) The performance comparison analysis of the high-performance TPU composite material for cables prepared in combination with Example 3 and Comparative Examples 3 to Comparative Examples 5 shows that the composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane in a mass ratio of 7:2:2. The modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage silsesquioxane in the composite flame retardant can improve the flame retardant properties and mechanical properties of the high-performance TPU composite material for cables through compatibility and synergy.
[0091] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.
Claims
1. A high-performance TPU composite material for cables, characterized in that: The preparation material comprises the following raw materials by weight: 60-65 parts of thermoplastic polyurethane TPU, 15-20 parts of polyolefin elastomer, 5-8 parts of HDPE, 6-8 parts of composite flame retardant, 0.05-0.1 parts of hydrolysis resistance agent, 3-5 parts of silicone masterbatch, 5-7 parts of modified nano titanium dioxide, 0.1-0.2 parts of ultraviolet absorber, 0.2-0.5 parts of calcium stearate, and 0.3-0.5 parts of antioxidant; wherein the composite flame retardant is composed of modified phenyl aluminum hypophosphite, octavinyl cage polysilsesquioxane and octaphenyl cage polysilsesquioxane in a weight ratio of 7:2:1-3; The preparation method of the modified phenyl aluminum hypophosphite is as follows: according to the mass fractions, under the protection of nitrogen, phenyl aluminum hypophosphite, polymethylphenylsiloxane and trimethyl borate are added into a reactor and placed in a heating jacket for heating and stirring, the heating temperature is set to 190-210° C., the heating rate is 6° C. / minute, the stirring rate is 300 rpm, and water is removed by distillation; after reacting for 30-40 minutes, the product is placed in anhydrous ethanol to be completely dissolved, and then deionized water is poured into it to precipitate the product, the precipitated product is filtered and vacuum dried at 80° C. for 36 hours, and then ground and sieved to obtain the modified phenyl aluminum hypophosphite; the mass fraction ratio of the phenyl aluminum hypophosphite, polymethylphenylsiloxane, trimethyl borate, anhydrous ethanol and deionized water is 10:(3-5):(1-3):30:200; The preparation method of the modified nano titanium dioxide comprises the following steps: adding 500 parts of nano titanium dioxide and 190 parts of calcium peroxide to 500 parts of a phosphoric acid solution with a mass concentration of 12 g / L, reacting for 30-40 minutes, filtering, and drying to obtain the modified nano titanium dioxide, wherein the average particle size of the nano titanium dioxide is 30 nm.
2. The high-performance TPU composite material for cables according to claim 1, characterized in that: The ultraviolet absorber is composed of 2,4-dihydroxybenzophenone, phenyl o-hydroxybenzoate and N-(ethoxycarbonylphenyl)-N'-methyl-N'-phenylamidine in a mass ratio of 2:(3-5):(1-3).
3. A high-performance TPU composite material for cables according to claim 1, characterized in that The anti-hydrolysis agent is composed of carbodiimide, phenyl glycidyl ether and bisphenol A diglycidyl ester in a mass ratio of 6:(1-3):(2-4).
4. The high-performance TPU composite material for cables according to claim 1, characterized in that: The antioxidant is tris(2,4-di-tert-butylphenyl) phosphite.
5. A method for preparing a high-performance TPU composite material for cables according to any one of claims 1 to 4, characterized in that: The following steps are involved: S81. Place thermoplastic polyurethane, polyolefin elastomer, HDPE, composite flame retardant, hydrolysis resistance agent, silicone masterbatch, modified nano titanium dioxide, ultraviolet absorber, calcium stearate and antioxidant in a high-speed mixer according to their weight fractions, and mix for 5-10 minutes to obtain a mixture; S82, putting the mixed material into a twin-screw extruder, melt-mixing, extruding and granulating, and obtaining a high-performance TPU composite material for cables.
6. The method for preparing a high-performance TPU composite material for cables according to claim 5, characterized in that: In step S82, the processing parameters of the twin-screw extruder are: extrusion temperature is 180-200°C, and screw speed is 200-240rpm.