A composite material with oxygen ion conductor and oxygen vacancy variable valence metal oxide and lithium battery thereof
Coating an oxygen vacancy variable valence metal oxide with an oxygen ion conductor improves the reaction specificity and stability of lithium-ion batteries by facilitating rapid oxygen transmission and protecting against oxidation, addressing thermal runaway issues.
Patent Information
- Application Number
- CN202410832509.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-26
AI Technical Summary
Ternary cathode materials in lithium-ion batteries undergo phase changes under high temperature conditions, leading to thermal runaway due to reactive oxygen, which is not effectively managed by existing solutions, resulting in poor cycle stability.
Coating an oxygen vacancy variable valence metal oxide with an oxygen ion conductor, such as a fluorite or perovskite structure, to facilitate rapid oxygen transmission and protect the inner layer from oxidation, thereby improving chemical and electrochemical stability.
The coating enhances the reaction specificity between the oxygen vacancy metal oxide and active oxygen, preventing thermal runaway and maintaining stability under extreme conditions.
Smart Images

Figure CN118405726B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to an oxygen vacancy variable-valence metal oxide material coated with an oxygen ion conductor, a preparation method and an application thereof. Background Art
[0002] Ternary cathode materials are prone to phase change when cycled under high temperature conditions, producing reactive oxygen with high chemical reactivity. The heat release caused by the side reaction caused by reactive oxygen is one of the main causes of thermal runaway of batteries. At present, it is proposed to use the chemical reaction between oxygen vacancies in metal oxides and reactive oxygen to delay the degree of thermal runaway.
[0003] For example, Chinese patent application CN102376946A discloses a positive electrode active material including a lithium composite oxide and a transition metal oxide, wherein the metal element in the transition metal oxide has an oxidation value smaller than the oxidation value of the transition metal in the most stable state, and can absorb oxygen generated by the positive electrode active material during the cycle.
[0004] The reactive oxygen side reaction process is relatively rapid, and the corresponding solution design needs to pay attention to timeliness. Highly reactive oxygen vacancy materials are very susceptible to partial oxidation under air conditions, which leads to reduced reactivity; this also leads to poor cycle stability of batteries using highly reactive oxygen vacancy materials, so the stability problem of highly reactive oxygen vacancies needs to be solved. Summary of the invention
[0005] The present application provides an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor, a preparation method and a use thereof. The oxygen ion conductor of the material coating layer has the ability to quickly transmit active oxygen, thereby improving the specificity of the reaction between the oxygen vacancy variable valence metal oxide material and active oxygen.
[0006] The specific technical solutions of this application are as follows:
[0007] The present application provides an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor, wherein the coating layer is an oxygen ion conductor and the inner layer is an oxygen vacancy variable valence metal oxide.
[0008] Preferably, for the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor described above, the oxygen ion conductor is selected from at least one of a fluorite structure, a pyrochlore structure, a perovskite structure, an apatite structure, La2Mo2O9 and their corresponding dopants; and / or
[0009] The oxygen vacancy variable valence metal oxide is MO y-x , wherein M is selected from metal elements, y=a / 2, wherein a is the highest stable valence state of M in the oxide, and 0<x<0.5.
[0010] Preferably, for the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor described above, M is selected from metal elements with an electronegativity greater than 1.5, preferably transition metal elements with multiple stable valences, and further preferably selected from one or more of Ti, Mn, V, Co, W and Mo.
[0011] Preferably, for the oxygen ion conductor coated oxygen vacancy variable valence metal oxide material described above, a transition layer containing oxygen ion conductor and oxygen vacancy variable valence metal oxide is further included between the coating layer and the inner layer.
[0012] Preferably, for the oxygen vacancy variable-valence metal oxide material coated with the oxygen ion conductor described above, the transition layer is a doping layer, a solid solution layer or a mixed layer consisting of the doping layer and the solid solution layer.
[0013] Preferably, for the oxygen vacancy variable-valence metal oxide material coated with an oxygen ion conductor as described in any one of the above items, the particle size D50 of the material is 50-2000 nm, preferably 300-1000 nm.
[0014] Preferably, for the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor as described in any of the above items, the degree of coverage of the oxygen vacancy variable valence metal oxide by the oxygen ion conductor is above 10%, preferably above 30%, preferably above 50%, and further preferably above 80%.
[0015] The present application provides a method for preparing an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor, which comprises: mixing an oxygen ion conductor and a variable valence metal oxide by a sol-gel method, a coprecipitation method or a high-temperature solid phase method, and sintering to obtain the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor.
[0016] Preferably, for the above method, the oxygen ion conductor is selected from at least one of a fluorite structure, a pyrochlore structure, a perovskite structure, an apatite structure, La2Mo2O9 and their corresponding dopants; and / or
[0017] The variable valence metal oxide is MO y and its corresponding dopants, wherein M is selected from metals, y=a / 2, wherein a is the highest stable valence state of M in the oxide, and 0<x<0.5.
[0018] Preferably, for the method described above, M is selected from metal elements with an electronegativity greater than 1.5, preferably transition metal elements with multiple stable valences, and further preferably selected from one or more of Ti, Mn, V, Co, W and Mo.
[0019] Preferably, for any of the above methods, the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor is the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor described above.
[0020] The present application provides an oxygen vacancy variable-valence metal oxide material coated with an oxygen ion conductor, which is prepared by any of the methods described above.
[0021] The present application provides a diaphragm, which includes:
[0022] a separator substrate; and
[0023] A coating comprising an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor as described in any one of the above or a coating comprising an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor prepared by any one of the above methods.
[0024] The present application provides a pole piece, which includes:
[0025] A current collector, and an active material layer disposed on the current collector;
[0026] The active material layer comprises the oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor as described in any one of the above items or the oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor prepared by any one of the methods described in the above items.
[0027] Preferably, for the pole piece described above, the pole piece is a positive pole piece and / or a negative pole piece.
[0028] The present application provides a lithium-ion battery, which comprises the above-mentioned diaphragm and / or any one of the above-mentioned pole pieces.
[0029] Effects of the Invention
[0030] The oxygen ion conductor coated oxygen vacancy variable valence metal oxide material described in the present application has the ability to quickly transmit active oxygen in the oxygen ion conductor of the coating layer, thereby improving the specificity of the reaction between the oxygen vacancy variable valence metal oxide material and active oxygen. At the same time, the inner layer of highly active oxygen vacancy variable valence metal oxide is prevented from directly contacting and oxidizing with air, thereby improving the chemical and electrochemical stability of the oxygen vacancy variable valence metal oxide without affecting its reactivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the structure of an oxygen ion conductor.
[0032] Figure 2 This is a schematic diagram of measuring the coating thickness in four directions per particle.
[0033] Figure 3It is a schematic diagram of the structure of a base membrane formed by coating an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor on a diaphragm substrate.
[0034] Figure 4 It is a comparison chart of the electrochemical stability of Example 1 and Comparative Example 1.
[0035] Figure 5 It is a schematic diagram of superoxide anion scavenging rates of Example 1, Comparative Example 1 and a blank group. DETAILED DESCRIPTION
[0036] The embodiments described below are described in detail for the present application. Although specific embodiments of the present application are shown, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present application and to fully convey the scope of the present application to those skilled in the art.
[0037] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the functional differences of components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" are open-ended terms and should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the present application, but the description is based on the general principles of the specification and is not intended to limit the scope of the present application. The scope of protection of the present application shall be determined by the attached claims.
[0038] The present application provides an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor, wherein the coating layer is an oxygen ion conductor and the inner layer is an oxygen vacancy variable valence metal oxide.
[0039] In the present application, the oxygen ion conductor refers to a type of solid oxide ion conductive material that contains a large number of oxygen ions that can migrate at high speed and use them as carriers. Figure 1 In the fluorite structure shown, the octahedral voids formed by cations are empty, and these empty octahedral voids provide transmission channels for oxygen ions to diffuse in the crystal lattice.
[0040] The oxygen vacancy variable valence metal oxide refers to a metal oxide particle lattice structure in which oxygen is removed by a reduction method such as heating hydrogenation, inert atmosphere deoxidation, or chemical reaction to form low-valent metal ions with unpaired electrons, such as titanium in titanium oxide (TiO2) changes from +4 to +3. 3+The formation of ions is usually accompanied by the presence of oxygen vacancies on the surface and the bulk. In addition, oxygen vacancies can be produced on the surface of variable valence metal oxides by a one-step method while sintering and coating the surface oxygen ion conductor at high temperature.
[0041] The general chemical formula of the variable valence metal oxide is MO y , which refers to an oxide material containing a metal M having multiple stable valences.
[0042] In some embodiments, the oxygen ion conductor is selected from at least one of a fluorite structure, a pyrochlore structure, a perovskite structure, an apatite structure, La2Mo2O9 and their corresponding dopants; and / or
[0043] The oxygen vacancy variable valence metal oxide is MO y-x , wherein M is selected from metals; further selected from metal elements having an electronegativity greater than 1.5, preferably transition metal elements having multiple stable valences, further preferably selected from one or more of Ti, Mn, V, Co, W and Mo;
[0044] y=a / 2, wherein a is the highest stable valence state of M in the oxide, 0<x<0.5, and x can be 0.1, 0.2, 0.3, 0.4, etc.
[0045] Electronegativity is a measure of an element's ability to attract electrons. An element with higher electronegativity can attract electrons, making it easier for oxygen ions to escape from the crystal lattice, and the oxygen vacancies formed are more active.
[0046] For example, the oxygen ion conductor may be selected from a fluorite structure or a dopant thereof, a pyrochlore structure or a dopant thereof, a perovskite structure or a dopant thereof, an apatite structure or a dopant thereof, or La2Mo2O9 or a dopant thereof.
[0047] For the fluorite structure, it can be D 1 Doped zirconium oxide, ceria or thoria, D 2 Doped bismuth oxide-based electrolyte; wherein D 1 At least one selected from alkaline earth metals and rare earth metals, D 2 At least one selected from metal cations Ni, V, W, etc. having a higher stable valence than Bi, such as Ce 0.5 Zr 0.5 O2.
[0048] For the pyrochlore structure, its molecular formula is A 1 2B 1 2O7, A 1 , B 1 are +3 and +4 cations, respectively, where A 1is at least one of the rare earth metals, B 1 is at least one of Zr, Sn, Ti and Sn; preferably, D 3 Can be doped in A 1 or B 1 The position has a metal element with a lower valence state and a higher ionic radius, preferably at least one of Ca, Mo, Al, In, Mg and Mn, such as Y2Ti2O7.
[0049] For the perovskite structure, its molecular formula is A 2 B 2 O3, where A 2 is at least one of the rare earth metals, B 2 is at least one of the transition metal ions that form 6 coordination with the oxygen ion; preferably, D 4 Can be doped in A 2 or B 2 The position is preferably selected from at least one of alkaline earth metals, such as LaGa 0.9 Mg 0.1 O 2.95 .
[0050] For the apatite structure, its molecular formula is A 3 9.333+Z (B 3 O4)6O 2+1.5Z2 (where 0≤Z<0.667), where A 3 is at least one of the rare earth metals, B 3 =Si and / or Ge; preferably, D 5 Can be in A 3 or B 3 La and Si are doped to increase the amount of interstitial oxygen in the structure or to increase the migration channel of interstitial oxygen, preferably at least one of B, Ca, Sr, Ba, Mg, Ti, V, Cr, Mn, Fe, Co, Zn, Ga, In, Sc, Sn, Nb, W, Al, Ge, etc., such as La 9.7 Si 5.7 Mg 0.3 O 26.3 .
[0051] For La2Mo2O9, if La is doped, D 6 is at least one of K, Sr, Ba, Bi, etc. If Mo is doped D 6 It is at least one of V, S, Cr, W, etc.
[0052] The present invention can prevent the oxidation of the oxygen vacancy variable valence metal oxide and improve its chemical and electrochemical stability by coating the oxygen ion conductor on the outer layer of the oxygen vacancy variable valence metal oxide.
[0053] The oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor described in the present application further comprises a transition layer containing an oxygen ion conductor and an oxygen vacancy variable valence metal oxide between the coating layer and the inner layer. In some embodiments, the transition layer is a doping layer, a solid solution layer, or a mixed layer composed of the doping layer and the solid solution layer.
[0054] In some embodiments, the coating layer has a thickness of 10-800 nm.
[0055] For example, the thickness of the coating layer can be 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, etc., and more preferably 50-200 nm. The present application sets the thickness of the coating layer within a specific range, which can effectively protect the inner layer, so that there are many effective oxygen vacancies, good safety performance, and good high-temperature cycle performance. If the thickness of the coating layer is lower than the above range, the protection effect on the inner layer is poor, the effective oxygen vacancies are small, the safety performance is affected, and the high-temperature cycle performance is poor; if the coating thickness is too high, the reaction efficiency is affected, the safety performance is affected, but the high-temperature cycle has little effect.
[0056] In the present application, there is no limitation on the method for measuring the coating layer, and the coating layer can be measured by conventional methods in the art, such as using an ultrathin slicer with a diamond blade or laser cutting to prepare a measurement sample of an oxygen vacancy variable-valence metal oxide material coated with an oxygen ion conductor, placing the cross-sectional structure in a transmission electron microscope and taking a photograph, and the magnification of the electron microscope is set in such a way that the cross section of one particle enters the field of view.
[0057] In this application, the coating degree Rc (%) is determined by determining the mass of the inner layer and the outer layer and then by the mass ratio. The mass ratio required for feeding is calculated based on the coating degree of the material, the density and particle size of the inner layer material, the density of the outer layer material and the thickness of the coating layer.
[0058] In some embodiments, the coverage degree of the oxygen ion conductor on the oxygen vacancy variable-valence metal oxide is greater than 10%, preferably greater than 30%, preferably greater than 50%, and more preferably greater than 80%.
[0059] For example, the coverage degree of the oxygen ion conductor on the oxygen vacancy variable valence metal oxide may be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%, etc.
[0060] In the present application, the method for measuring the coating thickness is not limited in any way, and the coating thickness can be measured according to conventional methods in the art. For example, the coating thickness can be measured according to the following steps:
[0061] The core layer material (variable valence metal oxide) is sampled before coating;
[0062] The core layer material before coating and the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor were placed in a transmission electron microscope to take pictures. The magnification of the electron microscope was set so that one particle entered the field of view. Each particle was Figure 2 The diameters R in four directions are shown, and 10 particles of each type of sample are measured. The average particle size R1 of the core layer oxygen vacancy variable valence metal oxide material before coating and the average particle size R2 of the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor are measured and calculated, and the coating layer thickness H=(R1-R2) / 2.
[0063] The oxygen vacancy variable valence metal oxide used in the present application has the characteristics of removing active oxygen and adsorbing anions, has extremely high reactivity, and its oxygen vacancies are easily oxidized and deactivated at room temperature. The present application uses an oxygen ion conductor for coating, which can adsorb and transfer active oxygen and adsorb cations. In addition, under its protection, the oxygen vacancies of the oxygen vacancy variable valence metal oxide are not easily deactivated.
[0064] The oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor described in the present application, the oxygen vacancy variable valence metal oxide can capture the active oxygen generated by the positive electrode during the battery cycle, especially under extreme abnormal working conditions such as hot box or overcharging, through the action of charge, to prevent the exothermic redox reaction between the active oxygen and the negative electrode active material, and avoid thermal runaway caused by continuous temperature rise inside the battery cell. In addition, the oxygen vacancies of the oxygen vacancy variable valence metal oxide provide Lewis acid center sites for the adsorption of anions, thereby increasing the dissociation degree of lithium salts and limiting the diffusion of anions.
[0065] The present application provides a method for preparing an oxygen vacancy valence-varied metal oxide material coated with an oxygen ion conductor, which comprises:
[0066] The oxygen ion conductor and the variable valence metal oxide are mixed by a sol-gel method, a coprecipitation method or a high-temperature solid phase method, and then sintered to obtain the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor.
[0067] In the present application, the sol-gel method, the coprecipitation method or the high temperature solid phase method are all conventional methods in the art. For example, the sol-gel method includes the following steps:
[0068] The precursor used for synthesizing the oxygen ion conductor is dissolved in a solvent, a variable valence metal oxide is added and mixed, and an appropriate amount of polyol is added to promote complexation to form a milky white sol, and the gel is continuously stirred to obtain a gel, and the gel is sintered to obtain an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor.
[0069] In the present application, the precursor used for synthesizing the oxygen ion conductor may be an organic acid salt solution or an inorganic acid salt solution or an alkyl ester metal alkoxide containing metal elements in the oxygen ion conductor; preferably, the organic acid salt solution may be an oxalate solution, an acetate solution or a tannate solution;
[0070] The inorganic acid salt solution may be sulfate, phosphate, nitrate, chloride, etc.;
[0071] The polyol may be ethylene glycol, propylene glycol, etc.;
[0072] The solvent can be water, ethanol, etc.
[0073] The coprecipitation method comprises the following steps:
[0074] The precursor used for synthesizing the oxygen ion conductor is dissolved in a solvent, and the variable valence metal oxide is added and stirred to be evenly dispersed, and then the pH is adjusted to precipitate and crystallize. After freeze-drying, the generated powder is sintered to obtain the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor.
[0075] In the present application, the precursor used for synthesizing the oxygen ion conductor may be an organic acid salt solution or an inorganic acid salt solution or an alkyl normal ester metal alkoxide containing the metal element in the oxygen ion conductor; preferably, the organic acid salt solution may be an oxalate solution, an acetate solution or a tannate solution;
[0076] The inorganic acid salt solution may be sulfate, phosphate, nitrate, chloride, etc.;
[0077] The solvent can be water, ethanol, etc.
[0078] The high temperature solid phase method comprises the following steps:
[0079] The variable valence metal oxide and oxygen ion conductor are added to a ball mill, and then a solvent and ball mill beads are added, and the mixture is dispersed in a heated constant temperature magnetic stirrer in an inert atmosphere to a paste solid. The paste solid is sintered in an inert atmosphere or in a vacuum to obtain an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor.
[0080] The present application adopts the above method to generate oxygen vacancies on the surface of the variable-valence metal oxide while coating the oxygen ion conductor.
[0081] In the present application, there is no limitation on the method of using variable-valence metal oxides to prepare oxygen vacancy variable-valence metal oxides, and the oxides can be prepared according to conventional methods in the art, for example, at least one of heating hydrogenation, vacuum deoxygenation, inert atmosphere deoxygenation, high-energy particle bombardment, ion doping, mechanochemical force or chemical reaction can be used for preparation, preferably heating hydrogenation, inert atmosphere deoxygenation or vacuum deoxygenation can be used for preparation.
[0082] In the present application, the heating hydrogenation method can be prepared by a method comprising the following steps:
[0083] (1) placing a variable-valence metal oxide in a reaction chamber, and evacuating the reaction chamber using a vacuum pump;
[0084] (2) repeatedly introducing an inert gas into the reaction chamber, and then evacuating the reaction chamber using a vacuum pump to clean the reaction chamber;
[0085] (3) introducing a reducing gas into the reaction chamber to reach a preset pressure; turning on a heating device to heat the reaction chamber to a preset temperature, and continuing the reaction to prepare an oxygen vacancy variable valence metal oxide.
[0086] For the inert atmosphere deoxidation method, it can be prepared by a method comprising the following steps:
[0087] (1) placing a variable-valence metal oxide in a reaction chamber, and evacuating the reaction chamber using a vacuum pump;
[0088] (2) repeatedly introducing an inert gas into the reaction chamber, and then evacuating the reaction chamber using a vacuum pump to clean the reaction chamber;
[0089] (3) introducing an inert gas into the reaction chamber to reach a preset pressure or evacuating the reaction chamber by a vacuum pump; turning on a heating device to heat the reaction chamber to a preset temperature and continuing the reaction to prepare an oxygen vacancy variable valence metal oxide.
[0090] In the present application, the reaction chamber includes but is not limited to a tube furnace or a box furnace.
[0091] In the present application, the inert gas includes but is not limited to nitrogen, argon or helium.
[0092] In the present application, the reducing gas includes but is not limited to hydrogen, carbon monoxide, olefins or alkynes, etc.
[0093] In some embodiments, the particle size D50 of the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor is 50-2000 nm. For example, the particle size D50 of the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor can be 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, 1200 nm, 1500 nm, etc., and is further preferably 300-1000 nm.
[0094] In the present application, the particle size D50 of the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor is controlled within the above range, the dispersion is relatively good, there are more oxygen vacancies per unit mass, and the reaction rate is high; if the particle size is too large, the specific surface area is low, the oxygen vacancies per unit mass are small, and the reaction efficiency is affected; if the particle size is too small, the dispersion is poor and the water content is high, which affects the cycle life of the battery.
[0095] In the present application, there is no limitation on the method for determining the particle size Dv50, which can be determined by conventional methods in the art, for example, by the following method:
[0096] The laser particle size analyzer tests the particle size Dv50 of the dispersion. The test solvent selected is deionized water. The powder to be tested is dispersed in the solvent by ultrasonic or mechanical stirring, and the sample is dripped into the test injector for testing. The test parameters are set as follows: material refractive index coating material setting, absorption rate 1.0, and light shielding degree 1-4%. The diameter of the particles that reach 50% of the volume in the sample is 30nm-2μm, which is the Dv50 value.
[0097] In some embodiments, the oxygen ion conductor is selected from at least one of a fluorite structure, a pyrochlore structure, a perovskite structure, an apatite structure, La2Mo2O9 and corresponding dopants; and / or
[0098] The variable valence metal oxide is MO y and corresponding dopants, wherein M is selected from metals, further selected from metal elements with an electronegativity greater than 1.5, preferably transition metal elements with multiple stable valences, further preferably selected from one or more of Ti, Mn, V, Co, W and Mo;
[0099] y = a / 2, where a is the highest stable valence state of M in the oxide.
[0100] In the present application, there is no limitation on the D50 of the oxygen ion conductor and the variable valence metal oxide, and any oxygen ion conductor and variable valence metal oxide with any D50 may be used. For example, for the variable valence metal oxide, its D50 may be 100-1000 nm, such as 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, etc.
[0101] In this application, D50 refers to Dv50.
[0102] In the present application, the dopant of the oxygen ion conductor refers to the dopant mentioned above.
[0103] The oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor prepared by the above method in the present application can effectively improve its chemical and electrochemical stability.
[0104] The present application provides an oxygen vacancy variable-valence metal oxide material coated with an oxygen ion conductor, which is prepared by any of the methods described above.
[0105] The present application provides the use of the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor described above or the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor prepared by the method described above in a lithium ion battery. In some embodiments, the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor is used for diaphragm coating, pole piece coating or pole piece surface coating.
[0106] The present application provides a diaphragm, which includes:
[0107] A diaphragm substrate and a coating comprising the oxygen vacancy valence-variable metal oxide material coated with the oxygen ion conductor described above or a coating comprising the oxygen vacancy valence-variable metal oxide material coated with the oxygen ion conductor prepared by the method described above.
[0108] In the present application, the preparation method of the diaphragm is not limited in any way, and the diaphragm can be prepared according to conventional methods in the art, for example, the following method can be used for preparation:
[0109] (1) mixing and stirring an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor, a dispersant and a solvent, and grinding and dispersing the mixture to obtain a dispersion;
[0110] (2) mixing and dispersing the dispersion liquid, thickener, binder and wetting agent to obtain a slurry;
[0111] (3) The slurry is coated on the surface of the diaphragm substrate and dried to obtain the diaphragm.
[0112] In the present application, the coating thickness is 0.1-10 μm.
[0113] In the present application, the dispersant, solvent, thickener, binder and wetting agent are not limited in any way, and they may be the commonly used dispersants, solvents, thickeners, binders and wetting agents in the art. For example, the dispersant may be at least one of sodium polyacrylate, polyacrylate ammonium salt copolymer, polyvinyl pyrrolidone, polyethylene glycol and sodium hexametaphosphate.
[0114] The solvent may include an aqueous or oily solvent, preferably at least one of water, ethanol, N-methylpyrrolidone, tetrahydrofuran, cyclohexane, petroleum ether, acetone, dimethylacetamide, and N,N-dimethylformamide;
[0115] The thickener may be at least one selected from sodium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate, polyvinylidene fluoride, polyacrylamide and polyvinyl alcohol;
[0116] The binder may be selected from at least one of polymethacrylic acid, methyl styrene-butadiene rubber, styrene-acrylic emulsion, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate, polyurethane, or a copolymer formed by methyl methacrylate and one or more monomers of methacrylic acid, ethacrylic acid, ethyl acrylate, ethyl methacrylate, propyl methacrylate, and butyl methacrylate;
[0117] The wetting agent may be selected from at least one of sodium perfluorooctanoate, nonylphenol, fluoroalkyl methoxy alcohol ether, polyoxyethylene alkylamine, sodium butylnaphthalene sulfonate, sodium arylnaphthalene sulfonate, sodium dodecylbenzene sulfonate or sodium alkyl sulfate.
[0118] In the present application, the membrane substrate may be a polymer porous membrane or a polymer porous membrane with a coating layer on the surface, and the polymer porous membrane may be one or more of polyethylene, polypropylene, polyimide, and polyethylene terephthalate. Optionally, the membrane substrate surface may be coated with high temperature resistant ceramic particles, such as alumina (Al2O3).
[0119] The present application provides a pole piece, which includes a current collector and an active material layer arranged on the current collector; the active material layer includes the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor described above or the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor prepared by the method described above.
[0120] In the present application, the present application does not impose any restrictions on the preparation method of the electrode sheet, and the electrode sheet can be prepared by conventional methods in the art, for example, the following method can be used for preparation:
[0121] (1) mixing and stirring an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor, a dispersant and a solvent, and grinding and dispersing the mixture to obtain a dispersion;
[0122] (2) mixing and dispersing the dispersion liquid, thickener, binder and wetting agent to obtain a slurry;
[0123] (3) The slurry is coated on the surface of the electrode and dried to obtain the electrode.
[0124] In the present application, the thickness of the coating is 0.1-10 μm.
[0125] In some embodiments, the electrode sheet is a positive electrode and / or a negative electrode sheet; in the present application, the active material in the positive electrode sheet may be selected from one or more of lithium cobalt oxide, lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA), lithium nickel manganese oxide and lithium-rich materials;
[0126] The active material in the negative electrode plate can be selected from one or more of graphite, hard carbon, silicon, molybdenum disulfide, lithium titanate, graphene, silicon carbon and silicon oxide.
[0127] In the present application, the coating method may be one or two of micro-gravure coating, dip coating, blade coating, spray coating, etc.
[0128] In some embodiments, the electrode sheet is a positive electrode and / or a negative electrode sheet.
[0129] The present application provides a lithium-ion battery, which comprises the above-mentioned diaphragm and / or the above-mentioned pole piece.
[0130] Example
[0131] The present application provides a general and / or specific description of the materials and test methods used in the experiments. In the following embodiments, unless otherwise specified, % means wt%, i.e., weight percentage. The reagents or instruments used without indicating the manufacturer are all conventional reagent products that can be purchased commercially, wherein LFP refers to lithium iron phosphate, LCO refers to lithium cobalt oxide, Ni83 refers to lithium nickel cobalt manganese oxide with a Ni content of 83%, Ni90 refers to lithium nickel cobalt manganese oxide with a Ni content of 90%, SiOC450 refers to silicon oxide doped graphite with a discharge capacity of 450 mAh / g, and SiOC650 refers to silicon oxide doped graphite with a discharge capacity of 650 mAh / g.
[0132] Example 1
[0133] (1) The valence metal oxide TiO2 with a particle size D50 of 400 nm and the oxygen ion conductor Ce with a particle size D50 of 50 nm are mixed. 0.5 Zr 0.5After adding O2 into a beaker at a coverage ratio of 80% by mass, anhydrous ethanol is used as a solvent and dispersed in an inert atmosphere in a heated constant temperature magnetic stirrer until it becomes a paste solid. The paste solid is sintered in an atmosphere of 95% hydrogen and 5% argon. The obtained material is ground and sieved to obtain the oxygen vacancy variable valence metal oxide material TiO2@Ce coated with an oxygen ion conductor. 0.5 Zr 0.5 O2, where TiO2 and Ce are calculated as follows 0.5 Zr 0.5 Mass ratio of O2:
[0134] The particle size R of the variable valence metal oxide TiO2 is 400nm and the density ρ1 is 4.26g / cm 3 , the particles are spherical, oxygen ion conductor Ce 0.5 Zr 0.5 The thickness H of the O2 coating layer is designed to be 80 nm and the density ρ2 is 7 g / cm 3 , the particle is spherical, the coverage is estimated to be 80%, and the mass ratio = (R / 2) 3 ×Π×ρ1:[(R / 2+H) 3 -(R / 2) 3 ]×Π×ρ2=5:6.
[0135] The coating thickness is measured as follows: an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor is cut into a sample for measurement using an ultrathin slicer with a diamond blade or laser cutting, and the cross-sectional structure is placed in a transmission electron microscope to take a picture. The magnification of the electron microscope is set so that the cross section of one particle enters the field of view. Figure 2 The diameters R in four directions are shown, and 10 particles of each type of sample are measured. The average particle size R1 of the core layer material before coating and the average particle size R2 of the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor are measured and calculated. The coating layer thickness H = (R1-R2) / 2, and the average result is 79nm.
[0136] The particle size of the material is determined according to the following method: a laser particle size analyzer is used to test the particle size D50 of the dispersion, deionized water is selected as the solvent, the powder to be tested is dispersed in the solvent by ultrasonic or mechanical stirring, and a sample is added dropwise to the test injector for testing. The test parameters are set as follows: the material refractive index coating material setting, the absorptivity is 1.0, the shading degree is 1-4%, and the result is 523nm.
[0137] The superoxide anion clearance rate (1 min clearance rate) was determined as follows:
[0138] ① Prepare the DMSO solution of nitro blue tetrazolium chloride (NBT) by drying and pyrogallol aqueous solution, and store in dark for later use;
[0139] ② Take pyrogallol solution, phosphate buffer and deionized water in a black cap bottle in a ratio of 1:3:6, mix them evenly, and directly shake them in the dark for 1 minute as a blank group. Add the oxygen vacancy variable valence metal oxide material coated with oxygen ion conductor, and shake them in the dark for 1 minute;
[0140] ③ Filter the suspension after the reaction, weigh the precipitate, divide the precipitate by the precipitate of the blank group, and evaluate the clearance rate. The result is 60.2%;
[0141] (2) Take the dispersant sodium polyacrylate and add it to the solvent water, stir it thoroughly, and then add 100g TiO2@Ce 0.5 Zr 0.5 O2, ball-milled evenly, then continued to add 1g of thickener sodium carboxymethyl cellulose, 5g of binder polyacrylate and 0.4g of wetting agent sodium perfluorooctanoate, so that the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor accounts for 94%, fully stirred to obtain a coating slurry;
[0142] (3) The coating slurry is coated on the diaphragm substrate by a micro-gravure coating machine, and baked at 40° C. for 2 minutes to form an oxygen vacancy variable valence metal oxide coating coated with an oxygen ion conductor, and rolled up to obtain the composite diaphragm, such as Figure 3 As shown, 11 is a polyethylene film, 21 and 22 are alumina coatings, and 31 is TiO2@Ce 0.5 Zr 0.5 O2 coating.
[0143] The lithium battery composite diaphragm prepared by the above method comprises a diaphragm substrate and an oxygen vacancy variable valence metal oxide coating coated with an oxygen ion conductor;
[0144] The diaphragm substrate is a polyethylene film with an aluminum oxide coating on both sides, where the thickness of the aluminum oxide coating is 2 μm and the thickness of the polyethylene film is 9 μm; TiO2@Ce 0.5 Zr 0.5 The thickness of the O2 coating is 2 μm;
[0145] The lithium battery composite separator prepared by the above method is used to test the electrochemical stability (CV), and the determination method is as follows:
[0146] The lithium battery composite separator was assembled into SS / / Li button cells with the coating facing the Li metal sheet. The voltage was increased from the open circuit voltage to 6V at a sweep rate of 1mV / s. The intersection of the horizontal line and the tangent of the inflection point of the current surge interval was taken as the electrochemical window, and the result was 5.5V.
[0147] The lithium battery composite diaphragm prepared by the above method is used to assemble a lithium battery. The battery structure is a Ni83||SiOC450 soft pack battery. The oxygen vacancy variable valence metal oxide material coating coated with the oxygen ion conductor faces the positive electrode side. The lithium battery prepared above is tested, and the results are shown in Table 1, wherein the overcharge pass rate is determined as follows:
[0148] The battery is discharged at a constant current to the discharge cut-off voltage, and then charged at a constant current of 3C rate or 3 times the manufacturer's recommended charging current, whichever is greater, to 160% SOC, and then left to stand for 1 hour. The battery has passed if it does not catch fire or explode.
[0149] The method for determining the hot box pass rate is as follows:
[0150] The battery is first discharged at a constant current to the discharge cut-off voltage, and then charged at a constant current to a fully charged state, and then placed in a test chamber. The test chamber is heated at a temperature rise rate of 5°C / min. When the temperature in the chamber reaches 140°C±2°C, it is kept constant for 1 hour. Then the temperature is raised at a temperature rise rate of 5°C / min. When the temperature in the chamber reaches 150°C±2°C, it is kept constant for 1 hour. Then the temperature is raised at a temperature rise rate of 5°C / min. When the temperature in the chamber reaches 1660°C±2°C, it is kept constant for 1 hour. During the whole process, the battery should not catch fire or explode, which means it has passed.
[0151] The room temperature cycle life is determined as follows:
[0152] a) Discharge at 1 C current to the material discharge termination voltage at 23℃±2℃, and let stand for 1 h;
[0153] b) Charge at 1 C current to the material charging termination voltage, then switch to constant voltage charging until the charging current rate drops to 0.05C, and let stand for 1 h;
[0154] c) The battery is discharged at a current of 1 C to the material discharge termination voltage, and the discharge specific capacity is recorded;
[0155] d) Repeat steps a and b three times, and select the average discharge capacity of the three tests as the initial capacity;
[0156] The battery is continuously charged and discharged at a current of 1 C. If the discharge capacity is lower than 80% of the initial capacity, the test is terminated and the total number of weeks during which the capacity is higher than the initial capacity is recorded.
[0157] The high temperature cycle life is determined as follows:
[0158] a) Discharge at 1 C current to the material discharge termination voltage at 23℃±2℃, and let stand for 1 h;
[0159] b) charging at 1 C at 45°C until the material charging termination voltage is reached, then switching to constant voltage charging until the charging current rate drops to 0.05 C;
[0160] c) After charging, the battery is left at 45°C for 5 hours.
[0161] d) At high temperature of 45°C, the battery is discharged at a current of 1 C to the material discharge termination voltage, and the discharge specific capacity is recorded;
[0162] e) Repeat steps b to d three times, and select the average discharge capacity of the three tests as the initial capacity;
[0163] The battery is continuously charged and discharged at a current of 1 C. If the discharge capacity is lower than 80% of the initial capacity, the test is terminated and the total number of weeks during which the capacity is higher than the initial capacity is recorded.
[0164] Example 2
[0165] The variable-valence metal oxide is TiO2 with a particle size D50 of 400 nm, and the oxygen ion conductor is La2Mo2O9 with a particle size D50 of 50 nm. The coating layer is added according to a designed thickness of 80 nm and a coverage degree of 80% by mass ratio. The other steps are the same as in Example 1. The thickness, particle size D50 and removal rate of the coating layer are measured according to the method described in Example 1. Among them, the particle size D50 of the oxygen vacancy variable-valence metal oxide coated with the oxygen ion conductor is 534 nm, the thickness of the coating layer is 81 nm, and the removal rate is 52.1%.
[0166] A lithium battery composite separator was prepared according to the method described in Example 1.
[0167] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, and the oxygen vacancy variable valence metal oxide material coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0168] Example 3
[0169] The variable valence metal oxide is WO3 with a particle size of D50 = 400nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 was added according to the designed coating thickness of 80nm and 80% coating mass ratio. The other steps were the same as those in Example 1. The thickness, particle size D50 and removal rate of the coating were determined according to the method described in Example 1. Among them, the particle size D50 of the oxygen vacancy variable valence metal oxide coated with the oxygen ion conductor was 552nm, the thickness of the coating was 83nm, and the removal rate was 46.9%.
[0170] A lithium battery composite separator was prepared according to the method described in Example 1.
[0171] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, and the oxygen vacancy variable valence metal oxide material coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0172] Example 4
[0173] The variable valence metal oxide is TiO2 with a particle size of D50 = 400nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 is added according to the designed coating thickness of 300nm and 80% coating degree by mass ratio. The other steps are the same as those in Example 1. The thickness and particle size D50 of the coating are determined according to the method described in Example 1, wherein the thickness of the coating is 267nm, and the particle size D50 of the oxygen vacancy variable valence metal oxide coated with the oxygen ion conductor is 893nm.
[0174] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, and the oxygen vacancy variable valence metal oxide material coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0175] Example 5
[0176] The variable valence metal oxide is TiO2 with a particle size of D50 = 400nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 was added according to the designed coating layer thickness of 30 nm and 80% coating degree by mass ratio. The other steps were the same as in Example 1. The thickness of the coating layer and the particle size D50 were determined according to the method described in Example 1, wherein the thickness of the coating layer was 32 nm and the particle size D50 was 486 nm.
[0177] A diaphragm was prepared according to the method described in Example 1 for assembling a lithium battery, the coating thickness was 2 μm, the battery structure was Ni83||SiOC450, the oxygen vacancy variable valence metal oxide coating coated with the oxygen ion conductor was facing the positive electrode side, and the overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0178] Example 6
[0179] The variable valence metal oxide is TiO2 with a particle size of D50 = 100nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 was added according to the designed coating layer thickness of 80nm and 80% coating degree by mass ratio. The other steps were the same as in Example 1. The thickness of the coating layer and the particle size D50 were determined according to the method described in Example 1, wherein the thickness of the coating layer was 78nm and the particle size D50 was 251nm.
[0180] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, and the oxygen vacancy variable valence metal oxide coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0181] Example 7
[0182] The variable valence metal oxide is TiO2 with a particle size of D50 = 1000nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 was added according to the designed coating layer thickness of 80nm and 80% coating degree by mass ratio. The other steps were the same as in Example 1. The thickness of the coating layer and the particle size D50 were determined according to the method described in Example 1, wherein the thickness of the coating layer was 80.5nm and the particle size D50 was 1226nm.
[0183] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, and the oxygen vacancy variable valence metal oxide coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0184] Example 8
[0185] The variable valence metal oxide is TiO2 with a particle size of D50 = 400nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 is added according to the designed coating thickness of 80nm and 50% coating mass ratio. The other steps are the same as those in Example 1. The thickness and particle size D50 of the coating layer are determined according to the method described in Example 1, wherein the particle size D50 of the oxygen vacancy variable valence metal oxide coated with the oxygen ion conductor is 513nm, and the thickness of the coating layer is 81nm.
[0186] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, the oxygen vacancy variable valence metal oxide coating coated with the oxygen ion conductor was facing the positive electrode side, and the oxygen vacancy variable valence metal oxide material coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0187] Example 9
[0188] The variable valence metal oxide is TiO2 with a particle size of D50 = 400nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 was added according to the designed coating thickness of 80nm and 95% coating degree by mass ratio. The other steps were the same as those in Example 1. The thickness and particle size D50 of the coating were determined according to the method described in Example 1. Among them, the particle size D50 of the oxygen vacancy variable valence metal oxide coated with the oxygen ion conductor was 547nm, and the thickness of the coating was 78.5nm.
[0189] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, the oxygen vacancy variable valence metal oxide coating coated with the oxygen ion conductor was facing the positive electrode side, and the oxygen vacancy variable valence metal oxide material coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0190] Example 10
[0191] The variable valence metal oxide is TiO2 with a particle size of D50 = 400nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 is added according to the designed coating thickness of 80nm and 80% coating degree by mass ratio. The other steps are the same as those in Example 1. The thickness and particle size D50 of the coating layer are determined according to the method described in Example 1, wherein the particle size D50 of the oxygen vacancy variable valence metal oxide coated with the oxygen ion conductor is 529nm, and the thickness of the coating layer is 79nm.
[0192] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, the oxygen vacancy variable valence metal oxide coating coated with the oxygen ion conductor was facing the negative electrode side, and the oxygen vacancy variable valence metal oxide material coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0193] Embodiment 11
[0194] (1) La 0.9 Sr 0.1 Ga 0.9 Mg 0.1 O 2.9 The acetate precursor salt compound of the metal element is dissolved in a citric acid aqueous solution according to the stoichiometric ratio of the metal element. The variable valence metal oxide TiO2 with a particle size D50 of 400nm is added according to the mass ratio of the coating layer design thickness of 80nm and 80% coverage, and stirred and dispersed evenly. An appropriate amount of ethylene glycol is added to promote complexation to form a milky white sol, and stirring is continued at 180°C until the water evaporates completely, so that the sol is converted into a gel. The obtained gel is sintered in a vacuum atmosphere, and the obtained material is ground and sieved to obtain the oxygen vacancy variable valence metal oxide material TiO2@La coated with an oxygen ion conductor. 0.9 Sr 0.1 Ga 0.9 Mg 0.1 O 2.9 The thickness and particle size D50 of the coating layer were measured according to the method described in Example 1, wherein the particle size D50 of the oxygen vacancy variable valence metal oxide coated with the oxygen ion conductor was 558 nm, and the thickness of the coating layer was 79.5 nm.
[0195] (2) Take the dispersant sodium polyacrylate and add it to the solvent water, stir it thoroughly, and then add 100g of oxygen vacancy variable valence metal oxide material TiO2@La coated with oxygen ion conductor 0.9 Sr 0.1 Ga 0.9 Mg 0.1 O 2.9 , ball-milled evenly, then continued to add 1g of thickener sodium carboxymethyl cellulose, 5g of binder polyacrylate and 0.4g of wetting agent sodium perfluorooctanoate, so that the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor accounts for 94%, and fully stirred to obtain a slurry;
[0196] (3) The slurry is coated on both sides of the diaphragm substrate by a micro-gravure coating machine, and baked at 40° C. for 2 minutes to form an oxygen vacancy variable valence metal oxide coating coated with an oxygen ion conductor, and then rolled up to obtain the diaphragm.
[0197] The lithium battery composite diaphragm prepared by the above method comprises a diaphragm substrate and an oxygen vacancy variable valence metal oxide coating coated with an oxygen ion conductor;
[0198] The diaphragm substrate is a polyethylene film with a thickness of 9 μm; the oxygen vacancy variable valence metal oxide material TiO2@La coated with an oxygen ion conductor 0.9 Sr 0.1 Ga 0.9Mg 0.1 O 2.9 The coating thickness is 2 μm;
[0199] The diaphragm prepared by the above method is used to assemble a lithium battery. The battery structure is LFP||graphite soft-pack battery. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life are measured according to the method described in Example 1. The results are shown in Table 1.
[0200] Comparative Example 1
[0201] (1) TiO2 with a particle size D50 of 400 nm was sintered in an atmosphere of 95% hydrogen and 5% argon. The obtained material was ground and sieved to obtain an oxygen vacancy variable valence metal oxide material. The removal rate was measured according to the method described in Example 1, and the removal rate was 6.8%.
[0202] (2) Add dispersant sodium polyacrylate to solvent water and stir thoroughly, then add 100g oxygen vacancy TiO2 and ball-mill evenly, then continue to add 1g thickener sodium carboxymethyl cellulose, 5g binder polyacrylate and 0.4g wetting agent sodium perfluorooctanoate, so that the oxygen vacancy variable valence metal oxide material accounts for 94%, stir thoroughly, and prepare slurry;
[0203] (3) The slurry is coated on a diaphragm substrate by a micro-gravure coating machine, baked at 40° C. for 2 minutes to form an oxygen vacancy variable valence metal oxide coating, and rolled up to obtain the diaphragm.
[0204] The lithium battery composite diaphragm prepared by the above method comprises a diaphragm substrate and an oxygen vacancy variable valence metal oxide coating;
[0205] The diaphragm substrate is a polyethylene film with aluminum oxide coating on both sides, wherein the thickness of the aluminum oxide coating is 2 μm, the thickness of the polyethylene film is 9 μm; the thickness of the oxygen vacancy TiO2 coating is 2 μm;
[0206] The electrochemical stability of the membrane was measured in the same manner as in Example 1, and the electrochemical window was 4.7V.
[0207] The diaphragm prepared by the above method is used to assemble a lithium battery. The battery structure is a Ni83||SiOC450 soft-pack battery, and the oxygen vacancy TiO2 coating faces the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life are determined according to the method described in Example 1. The results are shown in Table 1.
[0208] In addition, the electrochemical stability of the diaphragms obtained in Example 1 and Comparative Example 1 is compared. Figure 4 As shown. Figure 4 It can be seen that the electrochemical window of the membrane obtained in Example 1 is significantly improved.
[0209] Comparative Example 2
[0210] (1) Take the dispersant sodium polyacrylate and add it to the solvent water, stir it thoroughly, and then add 100g Ce 0.5 Zr 0.5 O2 (D50 is 50nm), ball-milled evenly, then continued to add 1g of thickener sodium carboxymethyl cellulose, 5g of binder polyacrylate and 0.4g of wetting agent sodium perfluorooctanoate, so that the oxygen ion conductor material accounts for 94%, fully stirred to obtain slurry;
[0211] (2) The slurry is coated on a diaphragm substrate by a micro-gravure coating machine, baked at 40° C. for 2 minutes to form an oxygen ion conductor coating, and rolled up to obtain the diaphragm.
[0212] Ce was measured in the same manner as in Example 1. 0.5 Zr 0.5 The removal rate of O2 is 2.6%.
[0213] The lithium battery composite diaphragm prepared by the above method includes a diaphragm substrate and an oxygen ion conductor coating; the diaphragm substrate is a polyethylene film with an aluminum oxide coating on both sides, wherein the aluminum oxide coating has a thickness of 2 μm and the polyethylene film has a thickness of 9 μm; Ce 0.5 Zr 0.5 The thickness of the O2 coating is 2 μm;
[0214] The diaphragm prepared by the above method is used to assemble a lithium battery. The battery structure is a Ni83||SiOC450 soft pack battery, Ce 0.5 Zr 0.5 The O2 coating was facing the positive electrode side, and the overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1. The results are shown in Table 1.
[0215] Comparative Example 3
[0216] (1) TiO2 with a particle size D50 of 400 nm was sintered in an atmosphere of 95% hydrogen and 5% argon. The obtained material was ground and sieved to obtain an oxygen vacancy variable valence metal oxide material. Then, the shell material Ce with a particle size D50 of 50 nm was sintered. 0.5 Zr 0.5 O2 is added into a beaker at a mass ratio of 5:6 with anhydrous ethanol as solvent and dispersed in a heated constant temperature magnetic stirrer until a paste-like solid is obtained, which is then ground, sieved and dried to obtain a mixture.
[0217] The clearance rate was determined according to the method described in Example 1 and was 12.4%.
[0218] (2) Add dispersant sodium polyacrylate to solvent water, stir thoroughly, then add 100 g of the mixture, ball mill evenly, then continue to add 1 g of thickener sodium carboxymethyl cellulose, 5 g of binder polyacrylate and 0.4 g of wetting agent sodium perfluorooctanoate, so that the mixture accounts for 94%, stir thoroughly, and prepare slurry;
[0219] (3) The slurry is coated on the diaphragm substrate by a micro-gravure coating machine, baked at 40° C. for 2 minutes to form a mixture coating, and rolled up to obtain the diaphragm.
[0220] The lithium battery composite diaphragm prepared by the above method comprises a diaphragm substrate and a mixture coating;
[0221] The diaphragm substrate is a polyethylene film with aluminum oxide coating on both sides, wherein the thickness of the aluminum oxide coating is 2 μm, the thickness of the polyethylene film is 9 μm, and the thickness of the mixture coating is 2 μm;
[0222] The electrochemical stability (CV) was tested in the same manner as in Example 1, and the electrochemical window was 4.9V.
[0223] The diaphragm prepared by the above method is used to assemble a lithium battery. The battery structure is a Ni83||SiOC450 soft-pack battery, and the mixture coating faces the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life are determined according to the method described in Example 1. The results are shown in Table 1.
[0224] Comparative Example 4
[0225] (1) Add dispersant sodium polyacrylate to solvent water and stir thoroughly, then add 100g TiO2 with a D50 of 400nm, ball mill evenly, then continue to add 1g thickener sodium carboxymethyl cellulose, 5g binder polyacrylate and 0.4g wetting agent sodium perfluorooctanoate, so that the metal oxide material accounts for 94%, stir thoroughly, and prepare slurry;
[0226] (2) The slurry is coated on a diaphragm substrate by a micro-gravure coating machine, baked at 40° C. for 2 minutes to form a metal oxide coating, and rolled up to obtain the diaphragm.
[0227] The lithium battery composite diaphragm prepared by the above method includes a diaphragm substrate and a metal oxide coating; the diaphragm substrate is a polyethylene film with aluminum oxide coating on both sides, wherein the aluminum oxide coating has a thickness of 2 μm and the polyethylene film has a thickness of 9 μm; the TiO2 coating has a thickness of 2 μm;
[0228] The diaphragm prepared by the above method is used to assemble a lithium battery. The battery structure is a Ni83||SiOC450 soft-pack battery with the TiO2 coating facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life are determined according to the method described in Example 1. The results are shown in Table 1.
[0229] Comparative Example 5
[0230] The variable valence metal oxide is TiO2 with a particle size of D50 = 400nm, and the oxygen ion conductor is Ce with a particle size of D50 = 50nm 0.5 Zr 0.5 O2 was added at a mass ratio of 80% coating degree, and the paste solid was sintered in an air atmosphere. The other steps were the same as in Example 1. The thickness and particle size D50 of the coating layer were determined according to the method described in Example 1, wherein the thickness of the coating layer was 77 nm.
[0231] The clearance rate was determined according to the method described in Example 1 and was 3.5%.
[0232] The membrane was prepared according to the method described in Example 1 for assembling lithium batteries, and the coating thickness was 2 μm. The battery structure was Ni83||SiOC450, and the variable valence metal oxide material coating coated with the oxygen ion conductor was facing the positive electrode side. The overcharge pass rate, hot box pass rate, room temperature cycle life and high temperature cycle life were measured according to the method described in Example 1, and the results are shown in Table 1.
[0233] Table 1 Performance of lithium batteries
[0234] .
[0235] It can be seen from the above table that the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor described in the present application has an excellent removal rate, and the high temperature cycle life, low temperature cycle life and safety of the prepared battery are all good, while the removal rate of the material described in the comparative example is low, and the high temperature cycle life, low temperature cycle life and safety of the prepared battery are also not good, indicating that the outer layer oxygen ion conductor of the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor can effectively prevent the inner layer of the highly active oxygen vacancy variable valence metal oxide from direct contact with the air, and improve its chemical and electrochemical stability without affecting the reaction activity of the oxygen vacancy variable valence metal oxide.
[0236] The above is only the preferred embodiment of the present application, and does not limit the present application in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present application without departing from the technical solution of the present application still falls within the protection scope of the technical solution of the present application.
Claims
1. An oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor, wherein: The coating layer is an oxygen ion conductor, and the inner layer is an oxygen vacancy variable valence metal oxide; The oxygen vacancy variable valence metal oxide is MO y-x , wherein M is selected from metal elements, y=a / 2, wherein a is the highest stable valence state of M in the oxide, 0<x<0.5; M is selected from one or more of Ti, Mn, V, Co, W and Mo; The oxygen ion conductor is selected from at least one of a fluorite structure, a pyrochlore structure, a perovskite structure, an apatite structure, La2Mo2O9 and their corresponding dopants; The fluorite structure is D 1 Doped zirconium oxide, ceria or thoria; or D 2 Doped bismuth oxide-based electrolyte; wherein D 1 At least one selected from alkaline earth metals and rare earth metals, D 2 At least one selected from the group consisting of metal cations Ni, V, and W; The molecular formula of the pyrochlore structure is A 1 2B 1 2O7, A 1 , B 1 are +3 and +4 cations, respectively, where A 1 is at least one of the rare earth metals, B 1 is at least one of Zr, Sn, Ti and Sn; The molecular formula of the perovskite structure is A 2 B 2 O3, where A 2 is at least one of the rare earth metals, B 2 is at least one of the transition metal ions that form hexa-coordination with oxygen ions; The molecular formula of the apatite structure is A 3 9.333+Z (B 3 O4)6O 2+1.5Z ,0≤Z<0.667, where A 3 is at least one of the rare earth metals, B 3 is Si and / or Ge.
2. The oxygen ion conductor-coated oxygen vacancy variable valence metal oxide material according to claim 1, wherein: A transition layer containing an oxygen ion conductor and an oxygen vacancy variable valence metal oxide is also included between the coating layer and the inner layer.
3. The oxygen ion conductor-coated oxygen vacancy variable valence metal oxide material according to claim 2, wherein: The transition layer is a doping layer, a solid solution layer or a mixed layer consisting of the doping layer and the solid solution layer.
4. The oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor according to any one of claims 1 to 3, wherein: The material particle size D50 is 50-2000nm.
5. The oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor according to any one of claims 1 to 3, wherein: The material particle size D50 is 300-1000nm.
6. The oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor according to any one of claims 1 to 3, wherein: The coverage degree of the oxygen ion conductor on the oxygen vacancy variable valence metal oxide is above 10%.
7. The oxygen ion conductor-coated oxygen vacancy variable valence metal oxide material according to claim 6, wherein: The coverage degree of the oxygen ion conductor on the oxygen vacancy variable valence metal oxide is above 30%.
8. The oxygen ion conductor-coated oxygen vacancy variable valence metal oxide material according to claim 7, wherein: The coverage degree of the oxygen ion conductor on the oxygen vacancy variable valence metal oxide is above 50%.
9. The oxygen ion conductor-coated oxygen vacancy variable valence metal oxide material according to claim 8, wherein: The coverage degree of the oxygen ion conductor on the oxygen vacancy variable valence metal oxide is above 80%.
10. A method for preparing the oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor according to any one of claims 1 to 9, comprising: The oxygen ion conductor and the variable valence metal oxide are mixed and sintered by a sol-gel method, a coprecipitation method or a high-temperature solid phase method to obtain the oxygen vacancy variable valence metal oxide material coated with the oxygen ion conductor.
11. The method according to claim 10, wherein: The oxygen ion conductor is selected from at least one of a fluorite structure, a pyrochlore structure, a perovskite structure, an apatite structure, La2Mo2O9 and their corresponding dopants; The fluorite structure is D 1 Doped zirconium oxide, ceria or thoria; or D 2 Doped bismuth oxide-based electrolyte; wherein D 1 At least one selected from alkaline earth metals and rare earth metals, D 2 At least one selected from the group consisting of metal cations Ni, V, and W; The molecular formula of the pyrochlore structure is A 1 2B 1 2O7, A 1 , B 1 are +3 and +4 cations, respectively, where A 1 is at least one of the rare earth metals, B 1 is at least one of Zr, Sn, Ti and Sn; The molecular formula of the perovskite structure is A 2 B 2 O3, where A 2 is at least one of the rare earth metals, B 2 is at least one of the transition metal ions that form hexa-coordination with oxygen ions; The molecular formula of the apatite structure is A 3 9.333+Z (B 3 O4)6O 2+1.5Z , 0≤Z<0.667, where A 3 is at least one of the rare earth metals, B 3 is Si and / or Ge; and / or The variable valence metal oxide is MO y And the corresponding dopant, wherein M is selected from a metal, y = a / 2, wherein a is the highest stable valence state of M in the oxide, 0 <x <0.5; M is one or more selected from the group consisting of Ti, Mn, V, Co, W and Mo.
12. A diaphragm comprising: Diaphragm substrate; and A coating comprising an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor according to any one of claims 1 to 9 or a coating comprising an oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor prepared by the method according to any one of claims 10 to 11.
13. A pole piece, comprising: A current collector, and an active material layer disposed on the current collector; The active material layer comprises the oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor according to any one of claims 1 to 9 or the oxygen vacancy variable valence metal oxide material coated with an oxygen ion conductor prepared by the method according to any one of claims 10 to 11.
14. The pole piece according to claim 13, wherein: The pole piece is a positive pole piece and / or a negative pole piece.
15. A lithium ion battery comprising the separator according to claim 12 and / or the pole piece according to any one of claims 13-14.
Citation Information
Patent Citations
Anode active material and lithium battery comprising anode active material
CN102376946A
Lithium ion battery anode composite material
CN103700850A
Lithium cobalt oxide cathode material with core-shell structure and preparation method thereof
CN111924886A
Sodium-ion battery positive electrode material with high ion mobility and preparation method thereof
CN117254016A
Perovskite and other solar cell materials
US20150144196A1