Environmentally friendly sound insulation coating and preparation method thereof

By using a core-shell structure and modified Cu-Fe layered double metal hydroxide in acrylic emulsion, the problem of insufficient research on the impact of layered double metal hydroxide on damping performance is solved, and the damping performance and performance of the coating are achieved. The improvement of sound insulation effect broadens the effective damping temperature range, and improves adhesion and environmental protection.

CN118406418BActive Publication Date: 2024-10-18GUANGDONG HUAZHU NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410635836.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-21
Publication Date
2024-10-18
Estimated Expiration
2044-05-21

AI Technical Summary

Technical Problem

In the existing technology, there are few studies on the effect of layered double metal hydroxides on damping performance. Especially in acrylic emulsions, there are challenges in broadening the damping performance and improving the sound insulation effect.

Method used

The core-shell acrylate emulsion structure is adopted, and modified Cu-Fe layered double metal hydroxide is added during the synthesis process. By changing the monomer ratio and interlayer structure of the core layer and the shell layer, the paint's properties are enhanced. Damping performance and sound insulation effect.

Benefits of technology

It significantly improves the damping performance and sound insulation effect of the coating, broadens the effective damping temperature range, improves adhesion, and achieves good room temperature sound insulation performance and environmental protection and low VOC characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004851661070000111
    Figure BDA0004851661070000111
Patent Text Reader

Abstract

The present invention relates to the field of coatings, and specifically to an environmentally friendly sound-insulating coating and a preparation method thereof. The present invention uses butyl acrylate to modify layered double metal hydroxides, and applies them to the synthesis of core-shell acrylic emulsions, thereby enhancing their damping properties. Furthermore, the present invention prepares the prepared core-shell acrylic emulsion into a sound-insulating coating, which has good room temperature sound-insulating properties, is environmentally friendly, and has low VOC. The present invention expands the application of layered double metal hydroxides in sound-insulating coatings, and provides a new idea for the development of new environmentally friendly sound-insulating coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of coatings, in particular to an environmentally friendly sound insulation coating and a preparation method thereof. Background Art

[0002] With the development of industrialization in today's society, the application of large machines has become increasingly widespread. As a result, the noise generated by the operation of the machines and the vibration of the parts is becoming more and more serious. These noises not only harm the environment, but also are a great hazard to the health of the workers. Therefore, damping coatings with anti-vibration and noise reduction properties have been developed. Damping coatings have the advantages of simple and convenient use and excellent damping effect, and are widely used in vehicle parts. When damping coatings are used on the surface of the engine, they can suppress the vibration generated by the engine and achieve the purpose of reducing noise. When used on the surface sheet metal of the car, it can reduce the noise generated by the friction between the vehicle sheet metal and the air when the vehicle is driving at high speed, thereby improving the comfort of the driver and passengers.

[0003] Damping refers to the gradual reduction of vibration amplitude caused by external forces (such as fluid resistance, friction, etc.) and inherent reasons of the domain system itself in any vibration system, as well as the quantitative characterization of this characteristic. From the perspective of vibration reduction, the energy of mechanical vibration is converted into heat energy or other energy that may be lost, so as to achieve the purpose of vibration reduction. Damping technology is to make full use of the general law of damping consumption, and give full play to the potential of damping in vibration reduction from technical issues such as materials, processes, and design, so as to improve the vibration resistance of mechanical structures, reduce the vibration of mechanical products, and enhance the dynamic stability of machinery and mechanical systems. With the rapid development of materials science and process technology, the family of damping materials is growing day by day. Damping materials can be divided into viscoelastic damping materials, composite damping materials, high damping alloy materials, ceramic high temperature resistant damping materials and intelligent damping materials.

[0004] Water-based damping coating is an environmentally friendly polymer-based damping coating with vibration and noise reduction effects. Damping coating is mainly composed of water-based emulsion, functional filler, flame retardant and additives. The matrix is ​​based on water-based emulsion. The water-based emulsion can be selected according to functional needs, such as styrene-acrylic emulsion, water-acrylic emulsion, silicone-acrylic emulsion, styrene-butadiene emulsion, etc. Compared with oil-based emulsion, water-based emulsion is widely used as a coating matrix because of its advantages such as environmental protection and low VOC. In addition, water-based damping coating has many advantages: first, it can be better applied to surfaces with complex structures to solve the problem of difficult construction of damping materials in complex structures; second, it has good anti-corrosion properties, safe and environmentally friendly; third, water-based coating has a good flame retardant effect, and also has vibration and noise reduction effects; fourth, for places with special purposes, damping coating can be selectively used: wide temperature range, corrosion resistance, wear resistance and other properties.

[0005] Filler is also an important component of water-based damping coatings. The inorganic filler of the lamellar layer will produce relative sliding with the base material due to its special structure, thereby increasing the loss of mechanical energy due to friction and realizing the dissipation of mechanical energy by frictional heat generation. Several commonly used inorganic fillers with lamellar structures include mica powder, graphite, talcum powder, and hollow glass microspheres. Among them, mica powder as a filler has a relatively good gain in the damping performance of damping coatings. By controlling the mesh size and dosage of mica powder, the loss factor and effective damping temperature range of damping coatings can be adjusted. Layered double hydroxides have a typical lamellar structure, with small interlayer forces and easy relative sliding. Therefore, they are more suitable for use as damping coatings. However, at present, there are more studies on the regulation of acrylic emulsions in China, and fewer studies on the influence of fillers on damping performance, especially the influence of layered double hydroxides on the damping performance of coatings is rarely reported. Therefore, it is very necessary to try layered double hydroxides to improve the damping performance of coatings.

[0006] CN 109337550 B discloses an aerogel water-based two-component transparent sound-insulating coating and a preparation and use method thereof. The coating applies silica aerogel particles to the glass sound-insulating coating, utilizes the low acoustic impedance characteristic of the silica aerogel to achieve the sound-insulating effect of the coating, and after being coated on the glass, the sound-insulating performance of the glass window can be improved, thereby effectively solving the problem of urban noise pollution. Summary of the invention

[0007] In view of the defects of the prior art, the present invention provides an environmentally friendly sound insulation coating and a preparation method thereof.

[0008] The environmentally friendly sound insulation coating comprises the following raw materials, calculated by weight: 70-75 parts of core-shell acrylic emulsion, 1-5 parts of hydroxyethyl cellulose, 0.2-0.5 parts of leveling agent, 0.4-0.8 parts of wetting agent, 0.3-0.5 parts of defoaming agent, 5-6 parts of film-forming agent and 70-75 parts of water.

[0009] The leveling agent is at least one of carboxymethyl cellulose, silicone oil, and polydimethylsiloxane; preferably, the leveling agent is silicone oil.

[0010] The wetting agent is at least one of propylene glycol, glycerin, Span-80 and Tween-60; preferably, the wetting agent is Span-80.

[0011] The defoamer is at least one of BYK-A555 defoamer and defoamer GP330; preferably, the defoamer is BYK-A555 defoamer.

[0012] The film-forming agent is at least one of dodecyl alcohol ester and hexylene glycol butyl ether acetate; preferably, the film-forming agent is dodecyl alcohol ester.

[0013] The preparation method of the core-shell type acrylic emulsion comprises the following steps:

[0014] N1: 13-15 parts of methyl methacrylate, 12-13 parts of styrene, 1-2 parts of divinylbenzene and 90-120 parts of water are mixed by mass, and then 1-2 parts of emulsifier and 1-2 parts of Cu-Fe layered double metal hydroxide modified by butyl acrylate are added thereto, and stirred at 200-400r / min in a nitrogen atmosphere at 70-80°C for 20-40min, and finally 0.01-0.05 parts of initiator and 0.2-0.4 parts of sodium bicarbonate are added, and the reaction is continued at a constant temperature for 120-180min to obtain a core emulsion;

[0015] N2: Mix 18-20 parts of butyl acrylate, 15-16 parts of isooctyl acrylate and 0.01-0.05 parts of initiator by mass to obtain a shell monomer emulsion; add the shell monomer emulsion dropwise to the core emulsion obtained in step N1 at a rate of 1-2 mL / min in a nitrogen atmosphere at 70-80°C, and continue the reaction for 120-180 min after the addition is completed to obtain a core-shell type acrylate emulsion.

[0016] The emulsifier is one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and polyvinyl alcohol; preferably, the emulsifier is sodium dodecylbenzene sulfonate.

[0017] The initiator is one of sodium persulfate and azobisisobutyronitrile; preferably, the initiator is sodium persulfate.

[0018] The preparation method of the butyl acrylate modified Cu-Fe layered double metal hydroxide comprises the following steps:

[0019] S1: adding 18-19 parts of copper nitrate and 24-25 parts of ferric nitrate to 300-400 parts of water by mass, stirring at 200-400 r / min for 5-10 min to obtain a metal salt solution, adding 10-20 parts of sodium citrate and 5-10 parts of urea to the metal salt solution, continuing to stir for 1-2 h, then adjusting the pH of the solution to 10-11 with a 12-16wt% sodium hydroxide aqueous solution, placing at 90-100°C, stirring at 200-400 r / min for reflux reaction for 6-8 h, centrifuging to obtain a precipitate, washing and drying to obtain a Cu-Fe layered double metal hydroxide;

[0020] S2: adding the Cu-Fe layered double metal hydroxide prepared in step S1 to 180-260 parts of anhydrous ethanol, stirring at 200-400 r / min for 24-48 hours in a nitrogen atmosphere, centrifuging at 4000-6000 r / min for 6-10 minutes, taking the supernatant, and obtaining a colloidal solution;

[0021] S3: adding 5-10 parts by mass of butyl acrylate to the colloidal solution prepared in step S2, and then reacting at 90-110° C. for 8-12 hours, cooling to room temperature, and centrifuging at a speed of 10000-12000 r / min for 6-10 minutes, centrifuging to obtain a precipitate, washing, and drying to obtain a Cu-Fe layered double metal hydroxide modified with butyl acrylate.

[0022] The invention also discloses a method for preparing the environmentally friendly sound insulation coating.

[0023] A method for preparing an environmentally friendly sound-insulating coating comprises the following steps: by weight, 70-75 parts of a core-shell acrylic emulsion, 1-5 parts of hydroxyethyl cellulose, 0.2-0.5 parts of a leveling agent, 0.4-0.8 parts of a wetting agent, 0.3-0.5 parts of a defoaming agent, 5-6 parts of a film-forming agent, and 70-75 parts of water are mixed, and stirred at a speed of 80-120 r / min for 5-15 min to obtain the environmentally friendly sound-insulating coating.

[0024] The present invention firstly adopts methyl methacrylate and styrene to polymerize to prepare acrylic emulsion, which has poor damping effect and does not have good sound insulation performance at room temperature. Furthermore, the present invention uses methyl methacrylate-styrene polymer as the core, and polymerizes butyl acrylate and isooctyl acrylate into the shell to obtain a core-shell acrylic emulsion, whose Tanδ value increases, indicating that its ability to consume sound wave energy is enhanced, and it also has excellent damping performance at room temperature. This is because the modification of the core-shell structure can achieve the purpose of widening the effective damping temperature range by increasing the number of shell layers. The monomer composition of the core layer and the shell layer is different. By changing the ratio of soft and hard monomers in the core layer and the shell layer, the core-shell structure can be designed as a hard core soft shell structure or a soft core hard shell structure. It is precisely because the glass transition temperature of the core layer and the shell layer is different, which effectively makes up for the problem that the effective damping temperature range of a single copolymer is too narrow. Furthermore, in the synthesis process of the core-shell structure acrylic emulsion, the present invention mixes the Cu-Fe layered double metal hydroxide and the core material, and polymerizes them together, and its Tanδ value is further increased, and the effective damping temperature range is further widened to the high temperature zone. This is because there are a large number of hydroxyl groups on the surface of the Cu-Fe layered double metal hydroxide, which can form a good connection with the methyl methacrylate-styrene copolymer. Due to the weak van der Waals force between its layers, when the vibration is transmitted, it can consume energy through plane sliding and weaken the transmission of sound waves. Further, the present invention modifies the added Cu-Fe layered double metal hydroxide, and replaces the nitrate ions between its layers with butyl acrylate, and its Tanδ value is increased again, and the effective damping temperature range is widened again, and its sound insulation effect is further enhanced. This is because the interlayer ions of the original Cu-Fe layered double metal hydroxide are nitrate ions, and the Cu-Fe layered double metal hydroxide is connected to the methyl methacrylate-styrene copolymer through the surface hydroxyl groups, and its translation energy consumption is low. After replacing nitrate ions with butyl acrylate, butyl acrylate can also participate in the polymerization of the core emulsion, thereby better transmitting vibration waves. In addition, butyl acrylate is larger than nitrate ions, which further reduces the interlayer force. When the vibration wave is transmitted, it may also move up and down, increase the interlayer distance, and recover under the action of the interlayer force, effectively losing energy. This shows that Cu-Fe layered double hydroxide does have the effect of improving damping performance, but the effect is not obvious. After a series of modifications, it significantly improves the damping performance of the coating.

[0025] Beneficial effects of the present invention: The present invention uses butyl acrylate to modify the layered double metal hydroxide, and applies it to the synthesis of the core-shell structure acrylic emulsion, thereby enhancing its damping performance. Furthermore, the present invention prepares the prepared core-shell acrylic emulsion into a sound insulation coating, which has good room temperature sound insulation performance, is environmentally friendly, and has low VOC. The present invention expands the application of layered double metal hydroxide in sound insulation coatings, and provides a new idea for the development of new environmentally friendly sound insulation coatings. DETAILED DESCRIPTION

[0026] Hydroxyethyl cellulose, CAS: 9004-62-0.

[0027] Dodecanol ester, CAS: 25265-77-4.

[0028] Example 1

[0029] A method for preparing an environmentally friendly sound-insulating coating comprises the following steps: by weight, 72 parts of acrylic emulsion, 4 parts of hydroxyethyl cellulose, 0.4 parts of a leveling agent, 0.6 parts of a wetting agent, 0.4 parts of a defoaming agent, 5.6 parts of a film-forming agent, and 72 parts of water are mixed, and stirred at a speed of 100 r / min for 10 minutes to obtain the environmentally friendly sound-insulating coating.

[0030] The leveling agent is silicone oil.

[0031] The wetting agent is Span-80.

[0032] The defoamer is BYK-A555 defoamer.

[0033] The film former is dodecyl alcohol ester.

[0034] The preparation method of the acrylic emulsion comprises the following steps: by weight, 14 parts of methyl methacrylate, 12.3 parts of styrene, 1.4 parts of divinylbenzene and 100 parts of water are mixed, and then 1.5 parts of an emulsifier is added thereto, and the mixture is stirred at a speed of 300 r / min for 30 minutes in a nitrogen atmosphere at 75° C., and finally 0.03 parts of an initiator and 0.3 parts of sodium bicarbonate are added, and the reaction is continued at a constant temperature for 150 minutes to obtain the acrylic emulsion.

[0035] The emulsifier is sodium dodecylbenzene sulfonate.

[0036] The initiator is sodium persulfate.

[0037] Example 2

[0038] A method for preparing an environmentally friendly sound-insulating coating comprises the following steps: by weight, 72 parts of a core-shell acrylic emulsion, 4 parts of hydroxyethyl cellulose, 0.4 parts of a leveling agent, 0.6 parts of a wetting agent, 0.4 parts of a defoaming agent, 5.6 parts of a film-forming agent, and 72 parts of water are mixed, and stirred at a speed of 100 r / min for 10 minutes to obtain the environmentally friendly sound-insulating coating.

[0039] The leveling agent is silicone oil.

[0040] The wetting agent is Span-80.

[0041] The defoamer is BYK-A555 defoamer.

[0042] The film former is dodecyl alcohol ester.

[0043] The preparation method of the core-shell type acrylic emulsion comprises the following steps:

[0044] N1: 14 parts of methyl methacrylate, 12.3 parts of styrene, 1.4 parts of divinylbenzene and 100 parts of water were mixed by weight, and then 1.5 parts of emulsifier were added thereto, and stirred at 300 r / min for 30 minutes in a nitrogen atmosphere at 75°C, and finally 0.03 parts of initiator and 0.3 parts of sodium bicarbonate were added, and the reaction was continued at a constant temperature for 150 minutes to obtain a core emulsion;

[0045] N2: Mix 19 parts of butyl acrylate, 15.5 parts of isooctyl acrylate and 0.03 parts of initiator by mass to obtain a shell monomer emulsion; add the shell monomer emulsion dropwise to the core emulsion obtained in step N1 at a rate of 2 mL / min in a nitrogen atmosphere at 75°C, and continue the reaction for 150 minutes after the addition is completed to obtain a core-shell type acrylate emulsion.

[0046] The emulsifier is sodium dodecylbenzene sulfonate.

[0047] The initiator is sodium persulfate.

[0048] Example 3

[0049] A method for preparing an environmentally friendly sound-insulating coating comprises the following steps: by weight, 72 parts of a core-shell acrylic emulsion, 4 parts of hydroxyethyl cellulose, 0.4 parts of a leveling agent, 0.6 parts of a wetting agent, 0.4 parts of a defoaming agent, 5.6 parts of a film-forming agent, and 72 parts of water are mixed, and stirred at a speed of 100 r / min for 10 minutes to obtain the environmentally friendly sound-insulating coating.

[0050] The leveling agent is silicone oil.

[0051] The wetting agent is Span-80.

[0052] The defoamer is BYK-A555 defoamer.

[0053] The film former is dodecyl alcohol ester.

[0054] The preparation method of the core-shell type acrylic emulsion comprises the following steps:

[0055] N1: 14 parts of methyl methacrylate, 12.3 parts of styrene, 1.4 parts of divinylbenzene and 100 parts of water were mixed by mass, and then 1.5 parts of emulsifier and 1.6 parts of Cu-Fe layered double metal hydroxide were added thereto, and stirred at 300 r / min for 30 minutes in a nitrogen atmosphere at 75°C, and finally 0.03 parts of initiator and 0.3 parts of sodium bicarbonate were added, and the reaction was continued at a constant temperature for 150 minutes to obtain a core emulsion;

[0056] N2: Mix 19 parts of butyl acrylate, 15.5 parts of isooctyl acrylate and 0.03 parts of initiator by mass to obtain a shell monomer emulsion; add the shell monomer emulsion dropwise to the core emulsion obtained in step N1 at a rate of 2 mL / min in a nitrogen atmosphere at 75°C, and continue the reaction for 150 minutes after the addition is completed to obtain a core-shell type acrylate emulsion.

[0057] The emulsifier is sodium dodecylbenzene sulfonate.

[0058] The initiator is sodium persulfate.

[0059] The preparation method of the Cu-Fe layered double metal hydroxide comprises the following steps: adding 18.7 parts of copper nitrate and 24.1 parts of ferric nitrate to 300 parts of water by mass, stirring at 300 r / min for 10 minutes to obtain a metal salt solution, adding 15 parts of sodium citrate and 8 parts of urea to the metal salt solution, continuing to stir for 2 hours, then adjusting the pH value of the solution to 10.5 with a sodium hydroxide aqueous solution with a concentration of 14wt%, placing the solution at 95°C, stirring and refluxing at a speed of 300 r / min for 8 hours, taking out a precipitate by centrifugation, washing and drying, and obtaining the Cu-Fe layered double metal hydroxide.

[0060] Example 4

[0061] A method for preparing an environmentally friendly sound-insulating coating comprises the following steps: by weight, 72 parts of a core-shell acrylic emulsion, 4 parts of hydroxyethyl cellulose, 0.4 parts of a leveling agent, 0.6 parts of a wetting agent, 0.4 parts of a defoaming agent, 5.6 parts of a film-forming agent, and 72 parts of water are mixed, and stirred at a speed of 100 r / min for 10 minutes to obtain the environmentally friendly sound-insulating coating.

[0062] The leveling agent is silicone oil.

[0063] The wetting agent is Span-80.

[0064] The defoamer is BYK-A555 defoamer.

[0065] The film former is dodecyl alcohol ester.

[0066] The preparation method of the core-shell type acrylic emulsion comprises the following steps:

[0067] N1: 14 parts of methyl methacrylate, 12.3 parts of styrene, 1.4 parts of divinylbenzene and 100 parts of water were mixed by mass, and then 1.5 parts of emulsifier and 1.6 parts of Cu-Fe layered double metal hydroxide modified by butyl acrylate were added thereto, and stirred at 300 r / min for 30 minutes in a nitrogen atmosphere at 75°C, and finally 0.03 parts of initiator and 0.3 parts of sodium bicarbonate were added, and the reaction was continued at a constant temperature for 150 minutes to obtain a core emulsion;

[0068] N2: Mix 19 parts of butyl acrylate, 15.5 parts of isooctyl acrylate and 0.03 parts of initiator by mass to obtain a shell monomer emulsion; add the shell monomer emulsion dropwise to the core emulsion obtained in step N1 at a rate of 2 mL / min in a nitrogen atmosphere at 75°C, and continue the reaction for 150 minutes after the addition is completed to obtain a core-shell type acrylate emulsion.

[0069] The emulsifier is sodium dodecylbenzene sulfonate.

[0070] The initiator is sodium persulfate.

[0071] The preparation method of the butyl acrylate modified Cu-Fe layered double metal hydroxide comprises the following steps:

[0072] S1: 18.7 parts of copper nitrate and 24.1 parts of ferric nitrate were added to 300 parts of water by mass, and stirred at 300 r / min for 10 min to obtain a metal salt solution. 15 parts of sodium citrate and 8 parts of urea were added to the metal salt solution, and stirring was continued for 2 h. Then, the pH of the solution was adjusted to 10.5 with a 14 wt% sodium hydroxide aqueous solution, and the solution was placed at 95°C and stirred at 300 r / min for 8 h. The precipitate was centrifuged, washed and dried to obtain a Cu-Fe layered double metal hydroxide.

[0073] S2: adding the Cu-Fe layered double metal hydroxide prepared in step S1 to 200 parts of anhydrous ethanol, stirring at 300 r / min for 24 h in a nitrogen atmosphere, centrifuging at 4000 r / min for 10 min, taking the supernatant, and obtaining a colloidal solution;

[0074] S3: adding 7 parts by mass of butyl acrylate to the colloidal solution prepared in step S2, and then reacting at 100° C. for 10 hours, cooling to room temperature, and centrifuging at a speed of 12000 r / min for 6 minutes, centrifuging and collecting the precipitate, washing and drying to obtain a Cu-Fe layered double metal hydroxide modified with butyl acrylate.

[0075] Example 5

[0076] A method for preparing an environmentally friendly sound-insulating coating comprises the following steps: by weight, 72 parts of a core-shell acrylic emulsion, 4 parts of hydroxyethyl cellulose, 0.4 parts of a leveling agent, 0.6 parts of a wetting agent, 0.4 parts of a defoaming agent, 5.6 parts of a film-forming agent, and 72 parts of water are mixed, and stirred at a speed of 100 r / min for 10 minutes to obtain the environmentally friendly sound-insulating coating.

[0077] The leveling agent is silicone oil.

[0078] The wetting agent is Span-80.

[0079] The defoamer is BYK-A555 defoamer.

[0080] The film former is dodecyl alcohol ester.

[0081] The preparation method of the core-shell type acrylic emulsion comprises the following steps:

[0082] N1: 14 parts of methyl methacrylate, 12.3 parts of styrene, 1.4 parts of divinylbenzene and 100 parts of water were mixed by weight, and then 1.5 parts of emulsifier were added thereto, and stirred at 300 r / min for 30 minutes in a nitrogen atmosphere at 75°C, and finally 0.03 parts of initiator and 0.3 parts of sodium bicarbonate were added, and the reaction was continued at a constant temperature for 150 minutes to obtain a core emulsion;

[0083] N2: Mix 19 parts of butyl acrylate, 15.5 parts of isooctyl acrylate, 1.6 parts of butyl acrylate-modified Cu-Fe layered double metal hydroxide, and 0.03 parts of initiator, by mass, to obtain a shell monomer emulsion; add the shell monomer emulsion dropwise to the core emulsion obtained in step N1 at a rate of 2 mL / min in a nitrogen atmosphere at 75°C, and continue the reaction for 150 min after the addition is completed to obtain a core-shell type acrylate emulsion.

[0084] The emulsifier is sodium dodecylbenzene sulfonate.

[0085] The initiator is sodium persulfate.

[0086] The preparation method of the butyl acrylate modified Cu-Fe layered double metal hydroxide comprises the following steps:

[0087] S1: 18.7 parts of copper nitrate and 24.1 parts of ferric nitrate were added to 300 parts of water by mass, and stirred at 300 r / min for 10 min to obtain a metal salt solution. 15 parts of sodium citrate and 8 parts of urea were added to the metal salt solution, and stirring was continued for 2 h. Then, the pH of the solution was adjusted to 10.5 with a 14 wt% sodium hydroxide aqueous solution, and the solution was placed at 95°C and stirred at 300 r / min for 8 h. The precipitate was centrifuged, washed and dried to obtain a Cu-Fe layered double metal hydroxide.

[0088] S2: adding the Cu-Fe layered double metal hydroxide prepared in step S1 to 200 parts of anhydrous ethanol, stirring at 300 r / min for 24 h in a nitrogen atmosphere, centrifuging at 4000 r / min for 10 min, taking the supernatant, and obtaining a colloidal solution;

[0089] S3: adding 7 parts by mass of butyl acrylate to the colloidal solution prepared in step S2, and then reacting at 100° C. for 10 hours, cooling to room temperature, and centrifuging at a speed of 12000 r / min for 6 minutes, centrifuging and collecting the precipitate, washing and drying to obtain a Cu-Fe layered double metal hydroxide modified with butyl acrylate.

[0090] Example 6

[0091] A method for preparing an environmentally friendly sound-insulating coating comprises the following steps: by weight, 70.4 parts of a core-shell acrylic emulsion, 1.6 parts of a Cu-Fe layered double metal hydroxide modified by butyl acrylate, 4 parts of hydroxyethyl cellulose, 0.4 parts of a leveling agent, 0.6 parts of a wetting agent, 0.4 parts of a defoaming agent, 5.6 parts of a film-forming agent, and 72 parts of water are mixed, and the mixture is stirred at a speed of 100 r / min for 10 minutes to obtain the environmentally friendly sound-insulating coating.

[0092] The leveling agent is silicone oil.

[0093] The wetting agent is Span-80.

[0094] The defoamer is BYK-A555 defoamer.

[0095] The film former is dodecyl alcohol ester.

[0096] The preparation method of the core-shell type acrylic emulsion comprises the following steps:

[0097] N1: 14 parts of methyl methacrylate, 12.3 parts of styrene, 1.4 parts of divinylbenzene and 100 parts of water were mixed by weight, and then 1.5 parts of emulsifier were added thereto, and stirred at 300 r / min for 30 minutes in a nitrogen atmosphere at 75°C, and finally 0.03 parts of initiator and 0.3 parts of sodium bicarbonate were added, and the reaction was continued at a constant temperature for 150 minutes to obtain a core emulsion;

[0098] N2: Mix 19 parts of butyl acrylate, 15.5 parts of isooctyl acrylate and 0.03 parts of initiator by mass to obtain a shell monomer emulsion; add the shell monomer emulsion dropwise to the core emulsion obtained in step N1 at a rate of 2 mL / min in a nitrogen atmosphere at 75°C, and continue the reaction for 150 minutes after the addition is completed to obtain a core-shell type acrylate emulsion.

[0099] The emulsifier is sodium dodecylbenzene sulfonate.

[0100] The initiator is sodium persulfate.

[0101] The preparation method of the butyl acrylate modified Cu-Fe layered double metal hydroxide comprises the following steps:

[0102] S1: 18.7 parts of copper nitrate and 24.1 parts of ferric nitrate were added to 300 parts of water by mass, and stirred at 300 r / min for 10 min to obtain a metal salt solution. 15 parts of sodium citrate and 8 parts of urea were added to the metal salt solution, and stirring was continued for 2 h. Then, the pH of the solution was adjusted to 10.5 with a 14 wt% sodium hydroxide aqueous solution, and the solution was placed at 95°C and stirred at 300 r / min for 8 h. The precipitate was centrifuged, washed and dried to obtain a Cu-Fe layered double metal hydroxide.

[0103] S2: adding the Cu-Fe layered double metal hydroxide prepared in step S1 to 200 parts of anhydrous ethanol, stirring at 300 r / min for 24 h in a nitrogen atmosphere, centrifuging at 4000 r / min for 10 min, taking the supernatant, and obtaining a colloidal solution;

[0104] S3: adding 7 parts by mass of butyl acrylate to the colloidal solution prepared in step S2, and then reacting at 100° C. for 10 hours, cooling to room temperature, and centrifuging at a speed of 12000 r / min for 6 minutes, centrifuging and collecting the precipitate, washing and drying to obtain a Cu-Fe layered double metal hydroxide modified with butyl acrylate.

[0105] Example 7

[0106] A method for preparing an environmentally friendly sound-insulating coating comprises the following steps: by weight, 70.4 parts of a core-shell acrylic emulsion, 1.6 parts of a Cu-Fe layered double metal hydroxide, 4 parts of hydroxyethyl cellulose, 0.4 parts of a leveling agent, 0.6 parts of a wetting agent, 0.4 parts of a defoaming agent, 5.6 parts of a film-forming agent, and 72 parts of water are mixed, and the mixture is stirred at a speed of 100 r / min for 10 minutes to obtain the environmentally friendly sound-insulating coating.

[0107] The leveling agent is silicone oil.

[0108] The wetting agent is Span-80.

[0109] The defoamer is BYK-A555 defoamer.

[0110] The film former is dodecyl alcohol ester.

[0111] The preparation method of the core-shell type acrylic emulsion comprises the following steps:

[0112] N1: 14 parts of methyl methacrylate, 12.3 parts of styrene, 1.4 parts of divinylbenzene and 100 parts of water were mixed by weight, and then 1.5 parts of emulsifier were added thereto, and stirred at 300 r / min for 30 minutes in a nitrogen atmosphere at 75°C, and finally 0.03 parts of initiator and 0.3 parts of sodium bicarbonate were added, and the reaction was continued at a constant temperature for 150 minutes to obtain a core emulsion;

[0113] N2: Mix 19 parts of butyl acrylate, 15.5 parts of isooctyl acrylate and 0.03 parts of initiator by mass to obtain a shell monomer emulsion; add the shell monomer emulsion dropwise to the core emulsion obtained in step N1 at a rate of 2 mL / min, and continue the reaction for 150 min after the addition is completed to obtain a core-shell type acrylate emulsion.

[0114] The emulsifier is sodium dodecylbenzene sulfonate.

[0115] The initiator is sodium persulfate.

[0116] The preparation method of the Cu-Fe layered double metal hydroxide comprises the following steps:

[0117] By mass, 18.7 parts of copper nitrate and 24.1 parts of ferric nitrate were added to 300 parts of water, and stirred at 300 r / min for 10 min to obtain a metal salt solution. 15 parts of sodium citrate and 8 parts of urea were added to the metal salt solution, and stirring was continued for 2 h. Then, the pH of the solution was adjusted to 10.5 with a 14 wt% sodium hydroxide aqueous solution, and the solution was placed at 95°C and stirred at 300 r / min for reflux reaction for 8 h. The precipitate was taken out by centrifugation, washed and dried to obtain a Cu-Fe layered double metal hydroxide.

[0118] Test Example 1

[0119] The environmentally friendly sound insulation coating prepared in each embodiment was poured into a template, dried naturally at room temperature for 48 hours, and then placed in an oven at 60° C. for 24 hours to prepare a 20 mm×6.50 mm×1.50 mm sample.

[0120] The damping performance of the environmentally friendly sound insulation coating prepared in the embodiment is tested using a DMTA Q800 dynamic mechanical performance instrument. During the test, the following settings are set: the tensile mode is selected, the strain condition is 1% strain, the test frequency is 1 Hz, the temperature range is set at -100-60°C during the test, and the temperature increase rate is 3°C per minute.

[0121] Table 1: DMA test data

[0122]

[0123] The loss factor (Tanδ) is usually used to represent the damping performance of a material. The larger the Tanδ value, the better the damping performance of the material. Correspondingly, the greater the material's ability to absorb and consume sound vibration energy. Materials with Tanδ≥0.3 are all effective damping materials.

[0124] As shown in Table 1, Example 1 uses core materials to directly make acrylic emulsion, and its Tanδ value is the smallest, and its effective damping temperature range is between -46.8 and 13.4, which shows that its damping effect is the worst and it does not have good sound insulation performance at room temperature. Example 2 makes the acrylic emulsion into a core-shell structure, and its Tanδ value increases, and its effective damping temperature range is between -47.8 and 35.2, which shows that its ability to consume sound wave energy is enhanced, and it also has excellent damping performance at room temperature. This is because the modification of the core-shell structure can achieve the purpose of widening the effective damping temperature range by increasing the number of shell layers. The monomer composition of the core layer and the shell layer is different. By changing the ratio of soft and hard monomers in the core layer and the shell layer, the core-shell structure can be designed as a hard core soft shell structure or a soft core hard shell structure. It is precisely because the glass transition temperature of the core layer and the shell layer is different, which effectively compensates for the problem that the effective damping temperature range of a single copolymer is too narrow. Example 3 In the synthesis process of the core-shell structure acrylic emulsion, the Cu-Fe layered double metal hydroxide and the core material are mixed and co-polymerized, and the Tanδ value is further increased, and the effective damping temperature range is -46.6-38.3. This is because there are a large number of hydroxyl groups on the surface of the Cu-Fe layered double metal hydroxide, which can form a good connection with the methyl methacrylate-styrene copolymer. Due to the weak van der Waals force between its layers, when the vibration is transmitted, it can consume energy through plane sliding and weaken the transmission of sound waves. Example 4 further modifies the added Cu-Fe layered double metal hydroxide, and replaces the nitrate ions between its layers with butyl acrylate. Its Tanδ value increases again, and the effective damping temperature range is -48.1-42.7, and its sound insulation effect is further enhanced. This is because the interlayer ions of the original Cu-Fe layered double metal hydroxide are nitrate ions, and the Cu-Fe layered double metal hydroxide is connected to the methyl methacrylate-styrene copolymer through the surface hydroxyl groups, and its translation energy consumption is low. After replacing the nitrate ions with butyl acrylate, butyl acrylate can also participate in the polymerization of the core emulsion, thereby better transmitting the vibration wave, and butyl acrylate is larger than the nitrate ion, which further reduces the interlayer force. When the vibration wave is transmitted, it may also move up and down, increase the interlayer distance, and recover under the action of the interlayer force, effectively losing energy. Example 5 attempts to add butyl acrylate-modified Cu-Fe layered double metal hydroxide to the shell raw material, and finds that its performance is slightly lower than that added to the core. The present invention believes that this is due to the larger volume of the Cu-Fe layered double metal hydroxide, which destroys the formation of the core-shell structure, thereby causing its damping performance to decrease. Example 6 and Example 7 attempt to directly add Cu-Fe layered double metal hydroxide and butyl acrylate-modified Cu-Fe layered double metal hydroxide to the environmentally friendly sound insulation coating, and find that its damping performance is slightly improved compared to Example 2 without addition, but significantly lower than Example 4.This shows that Cu-Fe layered double hydroxide does have the effect of improving damping performance, but the effect is not obvious. After a series of modifications, the damping performance of the coating is significantly improved.

[0125] Test Example 2

[0126] The environmentally friendly sound insulation coating is applied on the tinplate. After it dries, a layer of adhesive is applied on the coating surface. The circular forging die of the adhesion tester is connected to the coating surface through the adhesive. After the adhesive dries for 24 hours, the excess coating is scraped off along the periphery of the circular forging die. The adhesion tester is used to give the circular forging die a lifting force. When the circular forging die pulls the coating away from the tinplate surface, the displayed value is F. max , the area of ​​the circular forging die is S, the final result is measured three times and the average value is taken. The adhesion calculation formula is as follows:

[0127] Adhesion (MPa) = F max / S

[0128] Table 2: Paint adhesion test results

[0129] Adhesion(MPa) Example 1 0.56 Example 2 0.75 Example 3 0.81 Example 4 1.01 Example 5 1.05 Example 6 0.79 Example 7 0.76

[0130] It can be seen from Table 2 that the changes in adhesion and Tanδ values ​​of the environmentally friendly coatings obtained in Examples 1 to 7 are basically consistent. This shows that the Cu-Fe layered double metal hydroxide also has the effect of improving the adhesion of the coating. This is because there are a large number of hydroxyl groups on the surface of the Cu-Fe layered double metal hydroxide, which can form a good connection with the methyl methacrylate-styrene copolymer, and the copper ions and iron ions on its layer have a strong chelating effect, which can chelate with the groups on the surface of the tinplate, thereby enhancing the force between the coating and the metal surface. Therefore, Example 5 adds butyl acrylate-modified Cu-Fe layered double metal hydroxide to the shell raw material, and its adhesion is slightly higher than that of Example 4, which adds butyl acrylate-modified Cu-Fe layered double metal hydroxide to the core, but the damping performance of Example 5 is significantly lower than that of Example 4.

Claims

1. A method for preparing an environmentally friendly sound insulation coating, characterized in that: The following steps are involved: The core-shell acrylic emulsion, hydroxyethyl cellulose, a leveling agent, a wetting agent, a defoaming agent, a film-forming agent and water are mixed and stirred to obtain the environmentally friendly sound insulation coating; The preparation method of the core-shell type acrylic emulsion comprises the following steps: N1: Methyl methacrylate, styrene, divinylbenzene and water are mixed, and then an emulsifier and Cu-Fe layered double metal hydroxide modified by butyl acrylate are added thereto, heated and stirred in a nitrogen atmosphere, and finally an initiator and sodium bicarbonate are added, and the reaction is continued at a constant temperature to obtain a core emulsion; N2: mixing butyl acrylate, isooctyl acrylate and an initiator to obtain a shell monomer emulsion; dropping the shell monomer emulsion into the core emulsion obtained in step N1, and continuing the reaction after the dropwise addition is completed to obtain a core-shell type acrylate emulsion; The preparation method of the butyl acrylate modified Cu-Fe layered double metal hydroxide comprises the following steps: S1: adding copper nitrate and iron nitrate to water and stirring to obtain a metal salt solution, adding sodium citrate and urea to the metal salt solution, continuing to stir, then adjusting the pH of the solution with sodium hydroxide, placing the solution at a certain temperature and stirring under reflux reaction, centrifuging to obtain a precipitate, washing and drying to obtain a Cu-Fe layered double metal hydroxide; S2: adding the Cu-Fe layered double metal hydroxide prepared in step S1 into ethanol, stirring in a nitrogen atmosphere, centrifuging, and taking the supernatant to obtain a colloidal solution; S3: adding butyl acrylate to the colloidal solution prepared in step S2, then heating for reaction, cooling to room temperature, centrifuging, taking out the precipitate by centrifugation, washing and drying, and obtaining a Cu-Fe layered double metal hydroxide modified by butyl acrylate.

2. The method for preparing the environmentally friendly sound insulation coating according to claim 1, characterized in that: The leveling agent is at least one of carboxymethyl cellulose, silicone oil and polydimethylsiloxane.

3. The method for preparing the environmentally friendly sound insulation coating according to claim 1, characterized in that: The wetting agent is at least one of propylene glycol, glycerin, Span-80 and Tween-60.

4. The method for preparing the environmentally friendly sound insulation coating according to claim 1, characterized in that: The defoamer is at least one of BYK-A555 defoamer and defoamer GP330.

5. The method for preparing the environmentally friendly sound insulation coating according to claim 1, characterized in that: The film-forming agent is at least one of lauryl alcohol ester and hexanediol butyl ether acetate.

6. The method for preparing the environmentally friendly sound insulation coating according to claim 1, characterized in that: The emulsifier is one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and polyvinyl alcohol.

7. The method for preparing the environmentally friendly sound insulation coating according to claim 1, characterized in that: The initiator is one of sodium persulfate and azobisisobutyronitrile.

8. Environmentally friendly sound insulation coating, characterized in that: The environmentally friendly sound insulation coating is prepared by the preparation method of any one of claims 1 to 7.

Citation Information

Patent Citations

  • A two-component, aerogel-based transparent sound-insulating coating and its preparation and application method

    CN109337550B

  • Low-temperature water-based damping coating for extreme environment and preparation method of low-temperature water-based damping coating

    CN113698836A