Electrolyte, lithium-ion battery and electrical equipment

By using organic phosphine-based and/or organic amine-based additives with specific structures in the lithium-ion battery electrolyte to neutralize HF and prevent iron ion deposition, the problem of performance attenuation caused by iron dissolution reaction in lithium-ion batteries is solved, and the battery performance is significantly improved. Electrochemical and safety properties.

CN118412539BActive Publication Date: 2024-10-29SHENZHEN BYD LITHIUM BATTERY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410853003.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

The iron dissolution reaction of the LiFePO4 cathode material in lithium-ion batteries in a specific lithium salt electrolyte leads to the attenuation of battery rate performance and cycle performance, and poses a threat to safety performance. The existing solutions are not effective.

Method used

Additives containing organic phosphine groups and/or organic amine groups with specific structures are used as Lewis alkaline electron sources to neutralize HF in the electrolyte, inhibit the iron dissolution reaction, and prevent the deposition of iron ions on the negative electrode through bidentate coordination.

Benefits of technology

It significantly inhibits iron dissolution of the positive electrode material and iron deposition on the negative electrode, improves the electrochemical performance and safety performance of lithium-ion batteries, and maintains stable cycle performance and high energy density especially under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

The present disclosure relates to an electrolyte, a lithium ion battery and an electrical device, wherein the electrolyte comprises a lithium salt, an additive and an organic carbonate solvent. The electrolyte of the present disclosure contains a special additive, which can neutralize HF in the electrolyte to inhibit the iron dissolution reaction of the positive electrode material, and prevent iron deposition on the negative electrode by forming a complex with the iron ions dissolved in the electrolyte; the electrolyte used in the lithium ion battery can effectively improve the electrochemical performance and safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrolyte, a lithium-ion battery and an electrical device. Background Art

[0002] Lithium-ion batteries are composed of positive electrodes, negative electrodes, separators, and electrolytes. Compared with traditional LiMn2O4, LiCoO2, and ternary materials, lithium iron phosphate LiFePO4 (LFP) positive electrode materials with an olivine structure have high theoretical specific capacity, abundant resources, longer cycle life, and high safety, and are promising positive electrode materials for lithium-ion batteries. However, LiFePO4 will undergo a more obvious iron dissolution reaction in the electrolyte system of specific lithium salts (such as LiPF6). The iron ions dissolved from the positive electrode migrate through the electrolyte to the negative electrode (such as graphite), and will be reduced and deposited on the surface and inside of the negative electrode. The iron deposited at the negative electrode will: (1) occupy the ion transmission channel, hinder the intercalation and deintercalation of lithium ions in graphite, and lead to the attenuation of battery rate performance and cycle performance; (2) thicken the SEI film, increase the interfacial impedance, and also cause the loss of active lithium; (3) catalyze the decomposition of the electrolyte, produce gases such as CO2 and CH4; (4) induce uneven deposition of metallic lithium, pierce the diaphragm, cause internal short circuit, and have a serious impact on battery safety performance. HF produced by side reactions such as hydrolysis in the electrolyte is an important cause of iron dissolution in LiFePO4 positive electrode materials. Under high temperature conditions, the dissolution of iron is particularly obvious. The operating temperature range of large lithium-ion batteries in practical applications is -20℃ to 80℃. Therefore, in the field of energy storage, studying the mechanism and improvement measures of positive electrode iron dissolution is of great practical significance.

[0003] In order to reduce the impact of iron ion negative electrode deposition on the electrochemical performance and safety of the battery, common solutions include: (1) coating the surface of the positive electrode material with a carbon layer to prevent the contact between HF and the positive electrode LiFePO4; (2) adding film-forming additives (vinyl carbonate, fluoroethylene carbonate) to the electrolyte to form a passivation film to prevent the deposition of iron ions at the negative electrode; (3) adding water-removing additives (silane, organic amine) to the electrolyte to prevent the generation of HF; (4) adding acid-removing additives (alumina, magnesium oxide) to the electrolyte to neutralize the produced HF and reduce the corrosion of HF to the positive electrode. However, the above solutions have little inhibitory effect on iron dissolution and deposition, and new strategies need to be further explored to inhibit iron deposition and improve the cycle performance and safety of the battery. Summary of the invention

[0004] The purpose of the present disclosure is to provide an electrolyte, a lithium-ion battery and an electrical device to improve the electrochemical performance and safety performance of the lithium-ion battery.

[0005] In order to achieve the above-mentioned object, the present disclosure provides, in a first aspect, an electrolyte, comprising a lithium salt, an additive and a solvent, wherein the additive comprises at least one compound having a structure as shown in formula (1):

[0006] Formula (1);

[0007] Wherein, X1 and X2 are the same and are selected from P or N;

[0008] R1 and R2 are each independently selected from a substituted or unsubstituted aryl group having 6 to 14 carbon atoms;

[0009] R3 and R4 are each independently selected from an alkyl group having 1 to 4 carbon atoms, and a substituted or unsubstituted aryl group having 6 to 14 carbon atoms;

[0010] L is selected from an alkylene group having 1 to 12 carbon atoms, an alkynylene group having 2 to 12 carbon atoms, and an arylene group having 6 to 14 carbon atoms;

[0011] The substituents in R1, R2, R3, and R4 are each independently selected from an alkyl group having 1 to 4 carbon atoms and an alkenyl group having 2 to 4 carbon atoms.

[0012] Optionally, R1 and R2 are each independently selected from substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl;

[0013] R3 and R4 are each independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl;

[0014] L is selected from the group consisting of methylene, ethylene, propylene, butylene, pentylene, hexylene, ethynylene, phenylene, and biphenylene;

[0015] The substituents in R1, R2, R3 and R4 are independently selected from methyl and vinyl.

[0016] Optionally, the additive is selected from the group consisting of the following compounds:

[0017] .

[0018] Optionally, the weight ratio of the lithium salt, the additive and the solvent is 1:(0.01-0.2):(8-10).

[0019] Optionally, the weight ratio of the lithium salt, the additive and the solvent is 1: (0.05-0.15): (8.5-9.5).

[0020] Optionally, the solvent is at least one selected from carbonate solvents, carboxylate solvents and ether solvents.

[0021] Optionally, the solvent is a mixture of ethylene carbonate, dimethyl carbonate and diethyl carbonate, and the weight ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate is 1:(0.3~1):(0.3~1).

[0022] Optionally, the lithium salt is at least one selected from LiPF6, LiFSI and LiBOB.

[0023] In a second aspect of the present disclosure, a lithium-ion battery is provided, comprising a negative electrode, a positive electrode and the electrolyte according to the first aspect of the present disclosure, wherein the positive electrode comprises lithium iron phosphate and / or lithium iron manganese phosphate.

[0024] A third aspect of the present disclosure provides an electrical device comprising the lithium-ion battery described in the second aspect of the present disclosure.

[0025] Through the above technical scheme, the electrolyte disclosed in the present invention contains a special additive, which can neutralize HF in the electrolyte and inhibit the iron dissolution reaction of the positive electrode material on the one hand, and prevent iron deposition on the negative electrode by forming a complex with the iron ions dissolved in the electrolyte on the other hand; using the electrolyte in a lithium-ion battery can effectively improve the electrochemical performance and safety performance of the battery.

[0026] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0027] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.

[0028] In a first aspect of the present disclosure, an electrolyte is provided, the electrolyte comprising a lithium salt, an additive and a solvent, wherein the additive comprises at least one compound having a structure as shown in formula (1):

[0029] Formula (1);

[0030] In formula (1), X1 and X2 are the same and are selected from P or N;

[0031] R1 and R2 are each independently selected from a substituted or unsubstituted aryl group having 6 to 14 carbon atoms;

[0032] R3 and R4 are each independently selected from an alkyl group having 1 to 4 carbon atoms, and a substituted or unsubstituted aryl group having 6 to 14 carbon atoms;

[0033] L is selected from an alkylene group having 1 to 12 carbon atoms, an alkynylene group having 2 to 12 carbon atoms, and an arylene group having 6 to 14 carbon atoms;

[0034] The substituents in R1, R2, R3, and R4 are each independently selected from an alkyl group having 1 to 4 carbon atoms and an alkenyl group having 2 to 4 carbon atoms.

[0035] The electrolyte disclosed in the present invention contains a special additive, which contains an organic phosphine group and / or an organic amine group, which has Lewis alkalinity as an electron-donating group and can neutralize HF in the electrolyte, thereby reducing the corrosion of the electrolyte to the positive electrode material (such as LiFePO4) and inhibiting the iron dissolution reaction; at the same time, the organic phosphine group and / or the organic amine group can form a bidentate coordination with the transition metal ions (such as iron ions) in the electrolyte, so that the additive exhibits a strong transition metal ion chelating ability, and the diaryl group contained in the molecular structure of the additive greatly increases the molecular volume, which can hinder the migration of the organic phosphine and / or organic amine molecules after chelating the iron ions in the electrolyte, and effectively prevent the deposition of iron ions at the negative electrode.

[0036] In the present application, the description methods used "each independently is" and "respectively independently is" can be interchanged and should be understood in a broad sense. They can mean that in different groups, the specific options expressed by the same symbols do not affect each other, or that in the same group, the specific options expressed by the same symbols do not affect each other.

[0037] In the present application, the term "substituted or unsubstituted" means that the functional group recorded after the term may or may not have a substituent (hereinafter, for the convenience of description, the substituents are collectively referred to as Rc). For example, "substituted or unsubstituted aryl" refers to an aryl having a substituent Rc or an unsubstituted aryl. The above-mentioned substituent, i.e., Rc, can be, for example, an alkyl, a haloalkyl, an alkenyl, an aryl, etc. The number of substitutions can be 1 or more.

[0038] In the present application, the number of carbon atoms of a substituted or unsubstituted functional group refers to the total number of carbon atoms. For example, if R1 is a substituted aryl group with 12 carbon atoms, the total number of carbon atoms of the aryl group and the substituents thereon is 12.

[0039] In the present application, aryl refers to an optional functional group or substituent derived from an aromatic carbocyclic ring. The aryl group may be a monocyclic aryl group (e.g., phenyl) or a polycyclic aryl group. In other words, the aryl group may be a monocyclic aryl group, a condensed ring aryl group, two or more monocyclic aryl groups connected by carbon-carbon bond conjugation, a monocyclic aryl group and a condensed ring aryl group connected by carbon-carbon bond conjugation, and two or more condensed ring aryl groups connected by carbon-carbon bond conjugation. That is, unless otherwise specified, two or more aromatic groups connected by carbon-carbon bond conjugation may also be regarded as aryl groups of the present application. Among them, condensed ring aryl groups may include, for example, bicyclic condensed aryl groups (e.g., naphthyl), tricyclic condensed aryl groups (e.g., phenanthrenyl, fluorenyl, anthracenyl), etc. The aryl group does not contain heteroatoms such as B, N, O, S, P, Se, and Si. Examples of aryl groups may include, but are not limited to, phenyl, naphthyl, fluorenyl, anthracenyl, phenanthrenyl, biphenyl, terphenyl, etc. In the present application, the arylene group refers to a divalent group formed by further losing a hydrogen atom from an aryl group.

[0040] In the present application, the number of carbon atoms of a substituted aryl group refers to the total number of carbon atoms of the aryl group and the substituents on the aryl group. For example, a substituted aryl group with 14 carbon atoms refers to the total number of carbon atoms of the aryl group and the substituents is 14.

[0041] In the present application, the alkyl group having 1 to 4 carbon atoms may include a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms. Specific examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, and tert-butyl.

[0042] In the present application, the alkynylene group having 2 to 12 carbon atoms may include a straight chain alkynylene group having 2 to 12 carbon atoms and a branched chain alkynylene group having 3 to 12 carbon atoms. Specific examples of the alkynylene group include, but are not limited to, ethynylene, propynylene, butynylene, and the like.

[0043] In the present application, the alkenyl group having 2 to 4 carbon atoms may include a straight-chain alkenyl group having 2 to 4 carbon atoms and a branched-chain alkenyl group having 3 to 4 carbon atoms. Specific examples of the alkenyl group include ethenyl, propenyl, butenyl, and the like.

[0044] In some specific embodiments, the additive can be selected from the group consisting of the structures shown in formula (1-1) to (1-2):

[0045]

[0046] In some preferred embodiments, R1 and R2 are each independently selected from substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl; R3 and R4 are each independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl; L is selected from methylene, ethylene, propylene, butylene, pentylene, hexylene, ethynylene, phenylene, biphenylene; substituents in R1, R2, R3, and R4 are independently selected from methyl and vinyl. When the additive contains the above groups, it can form a favorable molecular volume and significantly inhibit the iron dissolution reaction and the deposition of iron ions.

[0047] Furthermore, when the additive is selected from the group consisting of the following compounds, it is beneficial to significantly improve the electrochemical performance and safety performance of the lithium iron phosphate battery:

[0048] .

[0049] The present disclosure has no particular limitation on the sources of the above-mentioned additives, which may be commercially available products or prepared according to methods disclosed in the prior art.

[0050] According to the present disclosure, the content of each component in the lithium iron phosphate battery electrolyte can be adjusted within a certain range. In a specific embodiment, the weight ratio of the lithium salt, the additive and the solvent can be 1: (0.01-0.2): (8-10), preferably 1: (0.05-0.15): (8.5-9.5). The electrolyte prepared using the preferred component ratio range is conducive to further improving the electrochemical performance and safety performance of the lithium iron phosphate battery.

[0051] According to the present disclosure, the solvent may be a common type in lithium-ion battery electrolytes, specifically, the solvent may be at least one selected from carbonate solvents, carboxylic acid ester solvents, and ether solvents. Among them, carbonate solvents may be ethylene carbonate (EC, molecular formula: C3H4O3), dimethyl carbonate (DMC, molecular formula: C3H6O3), diethyl carbonate (DEC, molecular formula: C5H 10 O3), etc.; the ether solvent may be dimethoxymethane, ethylene glycol dimethyl ether, tetrahydrofuran, etc.; the carboxylic acid ester solvent may be ethyl acetate, methyl propionate, ethyl propionate, etc. The above solvents have favorable conductivity, solubility, stability and safety, and are particularly suitable for the electrolyte disclosed in the present invention.

[0052] In a preferred embodiment, the organic carbonate solvent is a mixture of ethylene carbonate, dimethyl carbonate and diethyl carbonate, and the weight ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate can be 1: (0.3-1): (0.3-1), preferably 1: (0.5-0.8): (0.5-0.8). Using the above mixture as the organic carbonate solvent is conducive to the dissolution of lithium salts and the transmission of lithium ions.

[0053] According to the present disclosure, the lithium salt may be at least one selected from LiPF6, LiFSI and LiBOB. The above lithium salt has favorable conductivity, stability and safety, and is suitable for the electrolyte of the present disclosure. Preferably, the lithium salt is LiPF6, which has excellent comprehensive performance and is conducive to significantly improving the electrochemical performance and safety performance of lithium iron phosphate batteries.

[0054] According to the present disclosure, the electrolyte described in the present disclosure can be obtained by mixing the lithium salt, additive and solvent. In a specific embodiment, the preparation process of the electrolyte includes: mixing the solvent with the lithium salt at room temperature, stirring until the lithium salt is completely dissolved, and standing for 24 hours; then adding the additive in small amounts and stirring continuously until the additive is completely dissolved, and standing for 24 hours for standby use; to improve product quality, the above process can be operated in a glove box without water and oxygen (≤1 ppm).

[0055] The electrolyte disclosed in the present invention can effectively inhibit the dissolution of positive electrode iron and prevent the deposition of negative electrode iron. The use of the electrolyte in batteries containing lithium iron phosphate and / or lithium manganese iron phosphate can effectively improve the electrochemical performance and safety performance of the battery.

[0056] In a second aspect of the present disclosure, a lithium-ion battery is provided, the lithium-ion battery comprising a negative electrode, a positive electrode and the electrolyte described in the first aspect of the present disclosure. The present disclosure has no special restrictions on the specific structure of the lithium-ion battery, and the negative electrode material can be a common carbon material used for the negative electrode of a lithium-ion battery, such as graphite, amorphous carbon, silicon-based materials, etc.; the positive electrode material is at least one of lithium iron phosphate (LiFePO4) and lithium iron manganese phosphate (LiFeMnPO4).

[0057] The lithium-ion battery disclosed herein can maintain stable cycle performance in a high temperature environment, and can still maintain a high energy density and stability at high power output. At the same time, it can effectively avoid safety problems caused by puncturing the diaphragm and short circuits. It has excellent performance and is widely suitable for various application scenarios, such as energy storage in households and commercial fields, and some outdoor energy storage power stations under high temperature conditions.

[0058] A third aspect of the present disclosure provides an electrical device comprising the lithium-ion battery described in the second aspect of the present disclosure.

[0059] The present disclosure is further illustrated by the following examples, but is not intended to limit the present disclosure.

[0060] The raw materials and reagents used in the examples and comparative examples are all commercially available products.

[0061] Example 1

[0062] In the electrolyte of this embodiment, the lithium salt is LiPF6, and the additive structural formula is (purchased from Merck Reagent, CAS No. 6737-42-4), the solvent is a mixture of ethylene carbonate, dimethyl carbonate and diethyl carbonate (weight ratio is 1:0.5:0.5). The weight ratio of lithium salt, additive and solvent is 1:0.1:8.9.

[0063] The preparation process is carried out in a glove box without water and oxygen (≤1 ppm). Ethylene carbonate, dimethyl carbonate and diethyl carbonate with a water content of less than 20 ppm are fully stirred and mixed at room temperature; LiPF6 is added to the mixed solvent, stirred for about 30 minutes until completely dissolved, and allowed to stand for 24 hours; the additives are added to the mixed material in small amounts gradually and stirred continuously until the additives are completely dissolved, and then allowed to stand for 24 hours, and stored in a light-proof, water-free and oxygen-free environment below 40°C for future use.

[0064] Example 2

[0065] The electrolyte was prepared according to the steps described in Example 1, except that the additive had the structural formula: (purchased from Shanghai Aladdin, CAS No. 14118-16-2), the weight ratio of lithium salt, additive and solvent is 1:0.1:8.9, and the rest is the same as Example 1.

[0066] Example 3

[0067] The electrolyte was prepared according to the steps described in Example 1, except that the additive had the structural formula: (purchased from McLean, CAS No. 4129-44-6), the weight ratio of lithium salt, additive and solvent is 1:0.1:8.9, and the rest is the same as Example 1.

[0068] Example 4

[0069] The electrolyte was prepared according to the steps described in Example 1, except that the additive had the structural formula: (purchased from Merck reagent, CAS No. 6737-42-4), the weight ratio of lithium salt, additive and solvent is 1:0.05:8.95, and the rest is the same as Example 1.

[0070] Example 5

[0071] The electrolyte was prepared according to the steps described in Example 1, except that the additive had the structural formula: (purchased from Merck reagent, CAS No. 6737-42-4), the weight ratio of lithium salt, additive and solvent is 1:0.15:8.85, and the rest is the same as Example 1.

[0072] Example 6

[0073] The electrolyte was prepared according to the steps described in Example 1, except that the weight ratio of the lithium salt, the additive and the solvent was 1:0.01:8, and the rest was the same as Example 1.

[0074] Example 7

[0075] The electrolyte was prepared according to the steps described in Example 1, except that the weight ratio of the lithium salt, the additive and the solvent was 1:0.2:10, and the rest was the same as Example 1.

[0076] Example 8

[0077] The electrolyte was prepared according to the steps described in Example 1, except that the weight ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate in the organic carbonate solvent was 1:1:1, and the rest was the same as Example 1.

[0078] Example 9

[0079] The electrolyte was prepared according to the steps described in Example 1, except that the organic carbonate solvent was a mixture of ethylene carbonate and dimethyl carbonate (weight ratio of 1:1), and the rest was the same as Example 1.

[0080] Comparative Example 1

[0081] The electrolyte was prepared according to the steps described in Example 1, except that no additive was added, and the rest was the same as Example 1.

[0082] Comparative Example 2

[0083] The electrolyte was prepared according to the steps described in Example 1, except that the additive had the structural formula: (purchased from Shanghai Aladdin, CAS No. 23936-60-9), the rest is the same as Example 1.

[0084] Comparative Example 3

[0085] The lithium iron phosphate battery electrolyte was prepared according to the steps described in Example 1, except that the additive structural formula is (purchased from Shanghai Aladdin, CAS No. 829-85-6), the rest is the same as Example 1.

[0086] Test Example 1

[0087] The electrolytes prepared in Examples 1 to 9 and Comparative Examples 1 to 3 were respectively injected into square aluminum-shell LiFePO4 / C batteries with a capacity of 5 Ah, and the battery high-temperature cycle performance test was carried out.

[0088] Specifically, 19 g of electrolyte was injected into the battery cell by manual injection; the battery cell was then placed in a 25°C dew point space for aging for 4 days, and then the formation and capacity separation steps were performed; at 45°C, the battery cell after capacity separation was subjected to constant current charge and discharge tests in the voltage range of 2.5~3.6 V and a current density of 0.2 C, and the battery capacity was tested after 600 cycles. The capacity attenuation rate was calculated according to the following formula to obtain the high temperature cycle performance data of the battery cell. The results are shown in Table 1.

[0089] Capacity attenuation rate = (1-remaining capacity after 600 cycles / initial capacity) × 100%

[0090] Table 1

[0091]

[0092] As can be seen from Table 1, the electrolyte of the embodiment can be used in a lithium iron phosphate battery and has a higher capacity and a lower capacity attenuation rate after cycling 600 times at a high temperature of 45°C, showing a more excellent high-temperature cycle performance.

[0093] Test Example 2

[0094] The battery cells after 600 cycles in Test Example 1 were disassembled and tested for HF content and negative electrode iron deposition.

[0095] Specifically: using X-ray fluorescence spectrometer ( m XRF) was used to quantitatively analyze the iron deposited on the negative electrode. Specifically, a puncher was used to punch holes with an area of ​​1 cm at the edge and center of each group of negative electrode sheets. 2 The circular hole, with m XRF tests the weight of iron deposited on the two circular holes respectively, and then takes the average value of the mass. At the same time, liquid nuclear magnetic resonance (NMR) is used to quantitatively analyze the HF in the electrolyte after the reaction. Specifically, a certain amount of electrolyte is taken from each group into a nuclear magnetic resonance tube, and a calibration solution of known concentration is added. The results are shown in Table 2.

[0096] Table 2

[0097]

[0098] As can be seen from Table 2, after the electrolyte of the embodiment was used in the lithium iron phosphate battery for 600 cycles, the HF concentration in the electrolyte and the amount of iron deposited at the negative electrode were significantly lower, indicating that the electrolyte of the present invention has a significant effect of inhibiting the dissolution of positive electrode iron and preventing the deposition of negative electrode iron.

[0099] Test Example 3

[0100] The cells produced in Test Example 1 were subjected to charge and discharge performance tests at different rates.

[0101] Specifically, at 45°C, the cells were subjected to constant current charge and discharge tests at rates of 0.2 C, 1 C, 2 C, and 5 C in the voltage range of 2.5 to 3.6 V to obtain rate performance data at different current densities. The results are shown in Table 3.

[0102] Table 3

[0103]

[0104] As can be seen from Table 3, the electrolyte of the embodiment has higher capacity when used in lithium iron phosphate batteries at different rates, especially at a high rate of 5 C, the improvement effect is most obvious compared with the control example, showing a better battery rate performance.

[0105] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0106] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0107] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A lithium iron phosphate battery, characterized in that: The invention comprises a negative electrode, a positive electrode and an electrolyte, wherein the positive electrode comprises lithium iron phosphate, the electrolyte comprises a lithium salt, an additive and a solvent, and the weight ratio of the lithium salt, the additive and the solvent is 1: (0.05-0.15): (8.5-9.5), wherein the additive comprises at least one compound having a structure as shown in formula (1): Formula (1); Wherein, X1 and X2 are the same and are selected from P or N; R1 and R2 are each independently selected from a substituted or unsubstituted aryl group having 6 to 14 carbon atoms; R3 and R4 are each independently selected from an alkyl group having 1 to 4 carbon atoms, and a substituted or unsubstituted aryl group having 6 to 14 carbon atoms; L is selected from an alkylene group having 1 to 12 carbon atoms, an alkynylene group having 2 to 12 carbon atoms, and an arylene group having 6 to 14 carbon atoms; The substituents in R1, R2, R3, and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms and alkenyl groups having 2 to 4 carbon atoms; The solvent is a mixture of ethylene carbonate, dimethyl carbonate and diethyl carbonate, and the weight ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate is 1: (0.5-0.8): (0.5-0.8); The lithium salt is LiPF6, or the lithium salt is LiPF6 and LiFSI, or the lithium salt is LiPF6 and LiBOB, or the lithium salt is LiPF6, LiFSI and LiBOB.

2. The lithium iron phosphate battery according to claim 1, wherein: R1 and R2 are each independently selected from substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl; R3 and R4 are each independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl; L is selected from the group consisting of methylene, ethylene, propylene, butylene, pentylene, hexylene, ethynylene, phenylene, and biphenylene; The substituents in R1, R2, R3 and R4 are independently selected from methyl and vinyl.

3. The lithium iron phosphate battery according to claim 1 or 2, wherein: The additive is selected from the group consisting of the following compounds: 。 4. An electrical device, characterized in that: A lithium iron phosphate battery comprising any one of claims 1 to 3.

Citation Information

Patent Citations

  • Non-aqueous electrolyte and non-aqueous electrolyte secondary battery

    CN108346824A

  • Metal battery electrolyte and application thereof

    CN113725488A

  • Electrolyte suitable for manganese-containing positive electrode material battery and battery

    CN117352846A

  • Electrolyte for a lithium battery and lithium battery comprising the same

    CN1866605A

  • Nonaqueous electrolyte and lithium ion secondary battery

    JP2016018708A