Quartz glass cloth packaging method

By controlling the humidity inside the packaging and using low water vapor permeability membranes and desiccants, the problem of dielectric loss tangent deterioration caused by moisture adsorption on the surface of quartz glass cloth was solved, thus achieving a stable improvement in signal transmission performance.

CN118414286BActive Publication Date: 2024-11-08SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380012993.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-12-23
Filing Date
2023-11-28
Publication Date
2024-11-08
Estimated Expiration
2043-11-28

AI Technical Summary

Technical Problem

When quartz glass cloth absorbs moisture on its surface, the dielectric loss tangent deteriorates, affecting signal transmission performance.

Method used

By controlling the absolute humidity inside the packaging to below 10.0 g/m3, using packaging films and desiccants with low water vapor permeability, a dry atmosphere inside the packaging is ensured, inhibiting the adsorption of moisture by hydrogen bonds of Si-OH groups, and reducing the dielectric loss tangent.

Benefits of technology

It effectively suppressed the deterioration of the dielectric loss tangent of the quartz glass cloth, maintained stable signal transmission performance, and reduced the dielectric loss tangent to below 0.0005 at 10GHz.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005022077670000071
    Figure GDA0005022077670000071
  • Figure GDA0005022077670000151
    Figure GDA0005022077670000151
  • Figure GDA0005022077670000161
    Figure GDA0005022077670000161
Patent Text Reader

Abstract

The present invention is a packaging method for quartz glass cloth, which is a packaging method for packaging quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, wherein the volume absolute humidity in the package is 10.0 g / m 3 The following gases.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a packaging method for quartz glass cloth. Background Art

[0002] At present, with the high-speed communication of 5G, there is a strong desire for printed wiring substrates and antenna substrates with low transmission loss even when using high frequencies such as millimeter waves. In addition, in information terminals such as smart phones, high-density installation and ultra-thinning of printed wiring substrates are significantly carried out. As glass cloth for the printed wiring substrate, low-dielectric glass cloths such as D glass, NE glass, and L glass are proposed (Patent Documents 1 to 3). A laminated board is used in which prepregs obtained by impregnating low-dielectric glass cloth with thermoplastic resins such as fluororesins and polyphenylene ethers, and thermosetting resins such as low-dielectric epoxy resins and low-dielectric maleimide resins are stacked and heated and pressurized to cure.

[0003] The signal transmission loss is as Edward A.Wolff formula: Transmission loss As shown in the patent document 4, it is known that the smaller the dielectric constant (ε) and the dielectric loss tangent (tanδ), the better the material. Therefore, a low dielectric loss tangent is required in glass cloth, and quartz glass is proposed. In particular, a quartz glass cloth is proposed that satisfies the dielectric loss tangent of 0.0001 at 10 GHz by performing a high-temperature heating treatment and an etching treatment (Patent Document 4). However, there is no record of the packaging method in these documents.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 5-170483

[0007] Patent Document 2: Japanese Patent Application Publication No. 2009-263569

[0008] Patent Document 3: Japanese Patent Application Publication No. 2009-019150

[0009] Patent Document 4: Japanese Patent Application Publication No. 2021-195689 Summary of the invention

[0010] Problems to be solved by the invention

[0011] Quartz glass cloth is easy to adhere to and adsorb water on its surface due to its high purity. Therefore, due to the form of delivery to the user and the packaging method, the dielectric loss tangent may change over time and deteriorate. The purpose of the present invention is to provide a packaging method for suppressing the deterioration of the dielectric loss tangent of quartz glass cloth with low dielectric loss tangent.

[0012] Means for solving problems

[0013] For quartz glass cloth containing 99.5% or more SiO2, no matter how low the dielectric loss tangent is, a small amount of Si-OH groups will be generated on the surface. The Si-OH groups on the surface easily absorb moisture through hydrogen bonds. The inventors have found that the dielectric loss tangent of quartz glass cloth with low dielectric loss tangent is affected by the external atmosphere and packaging conditions when it is carried in, and the dielectric loss tangent is reduced. In order to solve this problem, the inventors have learned that in a packaging method for packaging quartz glass cloth containing 99.5% or more SiO2 with a packaging film, by controlling the absolute humidity in the package, the deterioration of the dielectric loss tangent of the quartz glass cloth with low dielectric loss tangent can be suppressed, and the present invention has been completed.

[0014] Therefore, the present invention provides a method for packaging quartz glass cloth.

[0015] 1. A method for packaging quartz glass cloth, comprising packaging quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, wherein the absolute humidity of the volume in the packaging is 10.0 g / m 3 the following.

[0016] 2. The method for packaging quartz glass cloth according to item 1, wherein the absolute humidity of the volume in the package is 5.0 g / m 3 the following.

[0017] 3. A packaging method for quartz glass cloth, comprising packaging quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, wherein the absolute humidity of the volume in the packaging within 5 minutes before the packaging is opened is 9.8 g / m 3 the following.

[0018] 4. The method for packaging a quartz glass cloth according to any one of 1 to 3, wherein the packaging film has a water vapor permeability of 20 g / (m 2 · days) or less packaging film.

[0019] 5. The method for packaging quartz glass cloth according to any one of 1 to 4, wherein the packaging film is a film selected from polyethylene, polypropylene, polyester, nylon (PA), ethylene-vinyl alcohol copolymer and vinylidene chloride, an organic resin composite film and a metal vapor-deposited film.

[0020] 6. The method for packaging a quartz glass cloth according to any one of 1 to 5, wherein a desiccant is packaged together in the packaging film.

[0021] 7. The method for packaging quartz glass cloth according to 6, wherein the desiccant has a maximum moisture absorption of 20% by mass or more at a relative humidity of 90%.

[0022] 8. The method for packaging quartz glass cloth according to 6 or 7, wherein the desiccant is a desiccant selected from silica gel, bentonite, zeolite, calcium chloride, calcium oxide and phosphorus pentoxide.

[0023] 9. The method for packaging quartz glass cloth according to any one of 1 to 8, wherein the volume absolute humidity in the packaging film at the initial stage of packaging is 10.0 g / m 3 the following.

[0024] 10. The method for packaging quartz glass cloth according to 9, wherein the absolute humidity of the volume in the packaging film at the initial stage of packaging is 5.0 g / m 3 the following.

[0025] 11. The method for packaging a quartz glass cloth according to any one of 1 to 10, wherein the gas in the package is dry air.

[0026] 12. The method for packaging a quartz glass cloth according to any one of 1 to 10, wherein the gas in the package is an inert gas.

[0027] 13. A method for packaging quartz glass cloth, comprising packaging quartz glass cloth containing 99.5 mass % or more of SiO2 with a packaging film, wherein the packaging film has a water vapor permeability of 20 g / (m 2 · days) or less, and pack the desiccant together in the packaging film.

[0028] 14. The method for packaging silica glass cloth according to any one of 1 to 13, wherein the dielectric loss tangent of the silica glass cloth taken out from the package at 10 GHz is 0.0005 or less after 1 day to 3 years of packaging.

[0029] 15. The method for packaging quartz glass cloth according to any one of 1 to 13, wherein the quartz glass cloth containing 99.5% by mass or more of SiO2 is a quartz glass cloth treated with a silane coupling agent. Effect of the Invention

[0030] According to the present invention, it is possible to provide a packaging method for suppressing deterioration in the dielectric loss tangent of a low-dielectric silica glass cloth. DETAILED DESCRIPTION

[0031] The packaging method of the quartz glass cloth of the present invention is a packaging method for packaging the quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, wherein the volume absolute humidity in the packaging is 10.0 g / m 3 The following gases.

[0032] In addition, the present invention relates to a packaging method for quartz glass cloth, which is a packaging method for packaging quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, wherein the packaging film has a water vapor permeability of 20 g / (m 2 · days) or less, and pack the desiccant together in the packaging film.

[0033] [Quartz glass cloth]

[0034] The SiO2 composition of the quartz glass cloth of the present invention is 99.5% by mass or more. From the perspective of electrical properties such as dielectric loss tangent and physical properties such as thermal expansion, quartz glass with a composition of 99.9% by mass or more is preferred. If the SiO2 composition is less than 99.5% by mass, the effect of the present invention cannot be exerted due to the deterioration of dielectric loss tangent.

[0035] As a method for manufacturing quartz glass cloth, for example, the following method can be cited. By melting quartz glass with a diameter of 50 to 500 mm at 1700 to 2300°C, the filamentary product is wound to obtain a quartz filament with a diameter of 200±100μm. If the melting temperature is within this range, stable stretching can be performed. Quartz filaments can be obtained by further stretching the quartz filaments to a diameter of 2 to 15μm at 1700 to 2300°C in a mixed flame of oxygen and hydrogen. Quartz filament bundles are manufactured by bundling 20 to 400 quartz filaments. In order to bundle the filament bundles, starch is used as the main raw material, and in order to impart functions, a bundling agent combined with a softener and a lubricant is used. Quartz yarn is obtained by twisting the filament bundles produced as described above. As the frequency of twisting, it is preferably 0.1 to 5.0 times per 25mm.

[0036] Quartz glass cloth is obtained by weaving quartz yarn. There is no particular limitation on the weaving method, and examples thereof include weaving methods using air jet looms, water jet looms, rapier looms, shuttle looms, and the like. When weaving using air jet looms, etc., in order to obtain further lubricity, polyvinyl alcohol (PVA) and starch can be attached as secondary sizing agents. For the obtained quartz glass cloth, a fiber opening treatment is performed to improve the impregnation of the resin in the subsequent process. There is no particular limitation on the fiber opening treatment method, and examples thereof include a fiber opening treatment method using ultrasound, a method using a high-pressure columnar water level flow, and a method using a gas-liquid mixed mist with an adjusted gas-water volume ratio. Depending on the type of quartz glass cloth, the methods are used as appropriate.

[0037] The sizing agent is attached to the surface of the quartz glass cloth obtained as above, and the sizing agent is removed by a degreasing process. The degreasing process includes washing with water or an organic solvent; and a heating cleaning process to burn and remove organic matter. From the perspective of being able to perform degreasing more reliably, a heating cleaning process is generally used. As for this treatment, there are methods using a fluidized or intermittent heating furnace. The fluidized method burns the sizing agent to ashes at high temperature all at once, so there are problems such as reduced strength of the quartz glass cloth and residual sizing agent after burning. Generally, the intermittent method burns and removes organic matter slowly at 300 to 700°C.

[0038] At this time, by heating the quartz glass cloth in dry air with a dew point of 15°C or less, the SiOH content of the quartz glass cloth is prevented from increasing, and a glass cloth with excellent dielectric loss tangent can be obtained. As a method of making the dew point of the quartz glass cloth into a gas below 15°C, there is a method of introducing dry air produced by a compressor, an air dryer, etc. into a heating furnace. The dew point of the introduced dry gas is preferably 15°C (volume absolute humidity: 12.8 g / m 3 ) or less, preferably 0°C (volume absolute humidity: 4.85 g / m 3 ) or less, preferably -20°C (volume absolute humidity: 1.07 g / m 3 ) or less, particularly preferably -60°C (volume absolute humidity: 0.0193 g / m 3 ) or less. In the heating process in the gas, As for the reaction, the lower the dew point, the more the balance tilts to the left, and the dielectric loss tangent of the quartz glass cloth decreases. There is no particular limitation on the amount of dry air introduced, but it is preferably 0.5 to 20 times the volume of the drying furnace per hour to sufficiently reduce the dew point in the furnace and maintain the temperature in the furnace within a certain range.

[0039] The quartz glass cloth may be in a deoiled state, but is more preferably treated with a silane coupling agent to obtain a silane coupling agent-treated quartz glass cloth in order to reduce the Si-OH groups on the surface of the glass cloth.

[0040] There is no particular limitation on the method of treating with the silane coupling agent. For cloth-like quartz glass cloth, wet treatment is preferred. As the silane coupling agent, known silane coupling agents can be used, and examples thereof include trimethylmethoxysilane, trimethylethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenylmethylvinylethoxysilane, naphthyltrimethoxysilane, naphthyltriethoxysilane, 1,4-bis(methoxydimethylsilyl)benzene, tetramethoxysilane, tetraethoxysilane, n-propyltrimethoxysilane, 1,4-bis(methoxydimethylsilyl)benzene ... Silane coupling agents containing unsaturated groups such as alkoxysilanes such as triethoxysilane, hexyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, and 1,6-bis(trimethoxysilyl)hexane, vinyltrimethoxysilane, vinyltriethoxysilane, p-phenylvinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyldimethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-methacryloxypropyldiethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropylmethyldimethoxysilane, 3-glycidyloxy Silane coupling agents containing epoxy groups such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-( Silane coupling agents containing amino groups such as N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane and its hydrochloride, N-(vinylbenzyl)-2-aminoethyl-3-aminopropylmethyldimethoxysilane and its hydrochloride, and alkoxysilane compounds such as 3-isocyanatepropyltriethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, and trifluoropropyltrimethoxysilane can be used alone or in combination. Among them, one or more selected from 3-aminopropyltrimethoxysilane, N-(2-(aminoethyl)-3-aminopropyltrimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane are more preferred.

[0041] The concentration of the silane coupling agent is generally used in a dilute aqueous solution of 0.1 to 5% by mass, and is effective when used in a concentration of 0.1 to 1% by mass. This allows the silane coupling agent to adhere evenly, providing a more uniform protective effect on the surface of the quartz glass cloth and making it easier to handle, and allows the resin used in the manufacture of substrates to be evenly and unevenly applied. In addition, the amount of silane coupling agent attached is preferably 0.01 to 0.3% by mass relative to the attached quartz glass cloth.

[0042] [Quartz glass cloth packaging method]

[0043] In the present invention, the volume absolute humidity in the package is 10.0g / m 3 The volume absolute humidity is preferably 7.5g / m 3 Below, more preferably 5.0g / m 3 There is no particular lower limit, but it can be 0 g / m 3 . As a method, for example, the above-mentioned range of dry gas can be achieved by sealing a desiccant together in the package or selecting a preferred packaging film. Furthermore, in the present invention, the measurement of the "volume absolute humidity in the package" is to introduce the measuring part of the thermometer and hygrometer into the packaging film just after opening the package, and after sealing it again, the value after 5 minutes is used as the volume absolute humidity regardless of the storage period. In the above measurement, the value measured without storage period, that is, the volume absolute humidity in the packaging film at the initial stage of packaging is preferably 10.0 g / m 3 Below, more preferably 5.0g / m 3 For the initial measurement of packaging, there is no particular lower limit, which can be 0 g / m 3 In addition, when a battery-type thermometer and hygrometer is packaged together with the packaging film for measurement, the volume absolute humidity in the package within 5 minutes just before opening the package (the volume absolute humidity in the package obtained by sealing the battery-type thermometer and hygrometer together) is preferably 9.8 g / m 3 Below, the volume absolute humidity is preferably 7.3g / m 3 Below, more preferably 4.9g / m 3 There is no particular lower limit, but it can be 0 g / m 3 .

[0044] The volume absolute humidity is measured by calculating the temperature (°C) and relative humidity (%) using the following formula.

[0045]

Number 1

[0046]

[0047] The thermohygrometer may be any measuring instrument as long as it can measure temperature and relative humidity, and the volume absolute humidity can be directly measured without using the above calculation formula.

[0048] [Packaging film]

[0049] The packaging film used for packaging the quartz glass cloth preferably has a water vapor permeability of 20 g / (m2) in a 40°C / 90% RH atmosphere in order to minimize the effect on the dielectric loss tangent. 2 The water vapor permeability is more preferably 10 g / (m 2 ·day) or less, more preferably 5g / (m 2 The lower limit is not particularly limited and can be 0 g / (m 2 · days). The water vapor transmission rate was measured by the method described in JIS Z0208-1976.

[0050] As the base material of the packaging film, there can be cited films composed of organic resins such as polyethylene (PE), polypropylene (PP), polyester (PET), nylon (PA), ethylene-vinyl alcohol copolymer (EVOH), and polyvinylidene chloride (PVDC), organic resin composite films coated with PVDC on PET and NA, and metal vapor-deposited films on PP and PET. Among them, the film selected from polyethylene film, polypropylene film, nylon film, ethylene-vinyl alcohol copolymer film, organic resin composite film, and metal vapor-deposited film is preferred. Compared with the organic resin single-layer film, the water vapor permeability of the organic resin composite film is low, and the water vapor permeability of the metal vapor-deposited film is the lowest. The best packaging film is selected according to the placement environment and time after packaging. In the present invention, since a desiccant is placed in the package, it can be an organic resin film.

[0051] [Desiccant]

[0052] There is no particular limitation on the desiccant that removes moisture from the air in contact with the packaged quartz glass cloth and prevents the deterioration of the dielectric loss tangent. One kind can be used alone or two or more kinds can be used in combination. For example, silica gel, bentonite, zeolite, calcium chloride, calcium oxide and phosphorus pentoxide, synthetic zeolite, clay, etc. can be listed. Among them, silica gel, bentonite, zeolite, calcium chloride, calcium oxide and phosphorus pentoxide are preferred, and silica gel, bentonite, zeolite and calcium chloride are more preferred. The desiccant preferably has a maximum moisture absorption of 20% by mass or more at a relative humidity of 90%, more preferably 50% by mass or more, and further preferably 100% by mass or more. The determination of hygroscopicity is determined by the method described in JISZ0701-1977. As for the amount of desiccant, as long as the absolute humidity in the package is 10.0g / m 3 The following methods are appropriately selected and may be any amount.

[0053] If the volume absolute humidity in the package is used, there is no particular limitation on the package. Examples of the gas in the package include air, nitrogen, argon and other inert gases. Among them, dry air is preferred in terms of production efficiency. Examples of devices for generating the dry air include compressors, air dryers and the like.

[0054] The packaging method of quartz glass cloth is a packaging method of packaging quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, and the volume absolute humidity in the package is 10.0g / m 3 The following gases are not particularly limited. Specifically, for example, preferably, 1000 m or 2000 m of quartz glass cloth is wound in a paper tube with a width of 1270 mm and the water vapor permeability is 20 g / (m 2 · days) or less, and contain a desiccant in the package to make the air in the package have a volume absolute humidity of 5.0g / m 3 The following dry air packaging and storage method is more preferably a packaging in which the package is sealed with dry air having a dew point of 0°C or less.

[0055] The above method can suppress the deterioration of the dielectric loss tangent of the quartz glass cloth. The width and length of the quartz glass cloth are not limited to 1300 mm wide, 1000 m long, or 2000 m long according to the subsequent process. For example, it can be appropriately selected from 400 to 650 mm wide, such as 800 to 1300 mm wide.

[0056] The packaging form is not particularly limited, but it is preferred to use a bag or film made of the above packaging film, and then heat-seal the two ends to form a sealed system. In addition, the environment and atmosphere during packaging is preferably a low humidity atmosphere, for example, the volume absolute humidity is preferably 10.0 g / m 3 Below, more preferably 7.5g / m 3 Below, more preferably 5.0g / m 3 In addition, during packaging, the air may be replaced with dry air from which moisture has been removed in advance using an air dryer or an inert gas such as nitrogen or argon with a very low absolute volume humidity.

[0057] The packaging (storage) period is not particularly limited, and can be appropriately selected from 1 day to 3 years, for example, 3 to 10 days, 1 month to 12 months, etc., depending on the purpose. The storage environment and atmosphere are not particularly limited to low humidity atmospheres, but from the viewpoint of keeping the volume absolute humidity in the package low, the dew point is preferably 25°C or less, more preferably 20°C or less, further preferably 15°C or less, and particularly preferably 10°C or less.

[0058] [Dielectric loss tangent of quartz glass cloth at 10 GHz]

[0059] The dielectric loss tangent of the quartz glass cloth packaged by the packaging method of the present invention is preferably 0.00050 or less at 10 GHz, more preferably 0.00035 or less. By adopting this packaging method, the dielectric loss tangent of the quartz glass cloth at 10 GHz can be made to be 0.00050 or less. If it is this packaging method, the dielectric loss tangent is basically the original dielectric loss tangent of the quartz glass cloth with adsorbed water removed, and the influence of the dielectric loss tangent caused by adsorbed water can be eliminated. The dielectric loss tangent of the quartz glass cloth at 10 GHz is measured using a resonator, such as a cavity resonator (TE011 mode) manufactured by AET.

[0060] The thickness of the glass cloth was measured using the theoretical film thickness. The theoretical film thickness of the glass cloth is given by the following equation: theoretical film thickness t (μm) = mass per unit area (g / m 2 ) / Specific gravity (g / cm 3 ) is calculated. The specific method is described in the examples.

[0061] [Dielectric loss tangent ratio before and after storage]

[0062] The ratio of the dielectric loss tangent at 10 GHz of the quartz glass cloth stored by the storage method of the present invention to the dielectric loss tangent before storage is preferably 1.5 times or less, more preferably 1.3 times or less, and further preferably 1.0 times or less.

[0063] The present invention is a method for packaging quartz glass cloth, which is a method for packaging quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, wherein the packaging film is 40°C·

[0064] The water vapor permeability in 90% RH atmosphere is 20g / (m 2 · days) or less, and the desiccant is packaged together in the packaging film. The preferred situation, amount, etc. are the same as above.

[0065] Example

[0066] The present invention will be specifically described below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0067] A quartz glass ingot containing 99.9% or more SiO2 was heated and stretched to produce a quartz glass fiber consisting of quartz glass filaments with a diameter of 5.3 μm. The quartz glass fiber was coated with the above-mentioned quartz glass fiber bundling agent (3.0% by mass of starch, 0.5% by mass of beef tallow, 0.1% by mass of emulsifier, and the balance of water) using a coater, and then bundled and wound using a bundling machine to produce a quartz glass bundle with 200 quartz glass filaments. The wound quartz glass bundle was twisted at 24 T / m to produce a quartz glass yarn.

[0068] After applying an aqueous solution consisting of 1.5% by mass of partially saponified polyvinyl acetate and 1.5% by mass of starch as a secondary sizing agent to the obtained quartz glass yarn, a jet loom was used to manufacture quartz glass cloth of IPC specification 1078, and a fiber opening treatment was performed using air-water mixed mist. Then, the sizing agent was removed by heating at 500°C for 36 hours using an electric furnace B80×85×200-3Z12-10 manufactured by Nemus Co., Ltd., and a quartz glass cloth with the sizing agent removed was obtained. At this time, dry air with a dew point of -70°C produced by a super non-heating dryer SHD3025 manufactured by CKD Co., Ltd. was fed in an amount 10 times the volume of the electric furnace per hour, and heated in a dry state. The obtained quartz glass cloth from which the sizing agent had been removed was surface treated with 3-methacryloxypropyltrimethoxysilane: KBM-503 (manufactured by Shin-Etsu Chemical Co., Ltd.) so that the adhesion rate became 0.05 mass %, thereby obtaining a silane-treated quartz glass cloth. The dielectric loss tangent (10 GHz) of the quartz glass cloth was 0.00035.

[0069] [Example 1]

[0070] A quartz glass cloth roll of 1000 m was prepared by winding the quartz glass cloth of 1270 mm width produced in the preparation example into a paper tube of 76.5 mm inner diameter, 182.6 mm outer diameter, and 1320 mm width. The roll was coated with high-density polyethylene (water vapor permeability at 40°C / 90%RH: 5.0 g / (m 2 ·day)) packaging bag (surface area: 2.8m 2 ) packaging, and put a bag of 100g type A silica gel made by Nippon Kagakukizai Co., Ltd., with a maximum moisture absorption of 30% by mass at a relative humidity of 90%, into the packaging. At this time (at the beginning of packaging), the volume absolute humidity in the packaging (film) measured by the temperature and humidity meter AD-5696 made by AND Co., Ltd. was 7.2g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. After storage, the packaging film was opened and placed in the temperature and humidity meter AD-5696 made by AND within 30 seconds, and then sealed again. The volume absolute humidity was 8.0g / m3 In addition, the dielectric loss tangent (10 GHz) is 0.00050.

[0071] [Example 2]

[0072] A quartz glass cloth roll of 1000 m was prepared by winding the quartz glass cloth of 1270 mm width produced in the preparation example into a paper tube of 76.5 mm inner diameter, 182.6 mm outer diameter, and 1320 mm width. The roll was coated with high-density polyethylene (water vapor permeability at 40°C / 90%RH: 5.0 g / (m 2 ·day)) packaging bag (surface area: 2.8m 2 ) packaging, put a bag of non-woven fabric packaging A-type silica gel 100g type made by Japan Chemical Machinery Co., Ltd. in the packaging, and package it. At this time (at the beginning of packaging), the volume absolute humidity in the packaging (film) is 7.2g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. At this time, an AD-5696 thermometer made by AND Co. was sealed together with the glass cloth. After 30 days, the thermometer records were checked and the absolute humidity in the package just before opening was 7.8 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00050.

[0073] [Example 3]

[0074] The quartz glass cloth roll prepared in the same manner as in Example 1 was coated with a high-density polyethylene (water vapor permeability at 40°C / 90%RH: 5.0 g / (m 2 ·day)) packaging bag (surface area: 2.8m 2 ) packaging, put 3 bags of non-woven fabric packaging A-type silica gel 200g type made by Japan Chemical Machinery Co., Ltd. in the packaging, and package. At this time, the volume absolute humidity in the packaging film is 7.2g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 4.8 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00040.

[0075] [Example 4]

[0076] The quartz glass cloth roll prepared in the same manner as in Example 1 was coated with an organic resin composite film (water vapor permeability at 40°C / 90%RH: 1.9 g / (m 2 ·day)) packaging bag (surface area: 2.8m 2) packaging, and in the same manner as in Example 1, three bags of non-woven fabric packaging A-type silica gel 200g type manufactured by Nippon Kagakukizai Co., Ltd. were placed in the packaging and packaged. At this time, the volume absolute humidity in the packaging film was 7.2g / m 3 .

[0077] The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 2.6 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00035.

[0078] [Example 5]

[0079] The quartz glass cloth roll prepared in the same manner as in Example 1 was coated with a vapor-deposited film (water vapor permeability at 40°C / 90%RH: 1.0 g / (m 2 ·day)) packaging bag (surface area: 2.8m 2 ) packaging, and in the same manner as in Example 1, three bags of non-woven fabric packaging A-type silica gel 200g type manufactured by Nippon Kagakukizai Co., Ltd. were placed in the packaging and packaged. At this time, the volume absolute humidity in the packaging film was 7.2g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The volume absolute humidity in the packaging film measured in the same manner as in Example 1 was 2.1 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00030.

[0080] [Example 6]

[0081] In the same quartz glass cloth roll package as in Example 5, 6 bags of non-woven fabric packaged clay-based desiccant DESICLAY 100g type manufactured by Tokai Chemical Industry Co., Ltd., with a maximum moisture absorption of 30% by mass at a relative humidity of 90%, were placed in the package. At this time, the volume absolute humidity in the packaging film was 7.2 g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 2.1 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00030.

[0082] [Example 7]

[0083] In the same quartz glass cloth roll package as in Example 5, one bag of calcium chloride-based Pavasso CE 100g type manufactured by Fuji Gel Industry Co., Ltd., with a maximum moisture absorption of 400 mass % at a relative humidity of 90%, was placed in the package and packaged. At this time, the volume absolute humidity in the packaging film was 7.2 g / m3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 1.8 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00030.

[0084] [Example 8]

[0085] In the same quartz glass cloth roll package as in Example 5, a bag of 200 g of non-woven fabric package A-type silica gel produced by Nippon Kagakukizai Co., Ltd. was placed in the package and packaged. At this time, the volume absolute humidity in the packaging film was 7.2 g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 2.4 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00040.

[0086] [Example 9]

[0087] The quartz glass cloth roll produced in the same manner as in Example 1 was packaged in high-density polyethylene in the same manner as in Example 1, and a bag of 200 g of non-woven fabric package A-type silica gel produced by Nippon Kagakukizai Co., Ltd. was placed in the package. At this time, the volume absolute humidity in the packaging film was 7.2 g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 7 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 3.2 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00050.

[0088] [Example 10]

[0089] In the same quartz glass cloth roll package as in Example 4, the air in the packaging film was replaced with dry air produced using Inverter Package Oil Free Babycon POD-15VNP manufactured by HITATHI. The volume absolute humidity in the packaging film was 1.2 g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 1.8 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00030.

[0090] [Example 11]

[0091] In the packaging of the same quartz glass cloth roll as in Example 4, the air in the packaging film was filled with nitrogen produced by Basho Kaisha (with a volume absolute humidity of less than 0.1 g / m 3 ) replacement. At this time, the absolute humidity of the volume in the packaging film is less than 0.1g / m 3 The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 1.5 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00030.

[0092] [Comparative Example 1]

[0093] The quartz glass cloth roll was prepared in the same manner as in Example 1 except that the high-density polyethylene in Example 1 was replaced with vinyl acetate (water vapor permeability at 40°C / 90%RH: 150 g / (m 2 ·days), the A-type silica gel was placed in the package, packaged and stored. The packaged quartz glass cloth was stored in a room with a dew point of 24°C for 30 days. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 12.3 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00070.

[0094] [Comparative Example 2]

[0095] The quartz glass cloth roll produced in the same manner as in Example 1 was packaged in high-density polyethylene in the same manner as in Example 1. However, the roll was stored in the same manner as in Example 1, except that the silica gel was not placed in the package. The absolute humidity in the packaging film measured in the same manner as in Example 1 was 21.8 g / m 3 In addition, the dielectric loss tangent (10 GHz) is 0.00110.

[0096] The packaging material composed of the low moisture permeability film of the present invention and the desiccant in the packaging can suppress the deterioration of the dielectric loss tangent of the low dielectric quartz glass cloth due to humidity.

[0097]

Table 1

[0098]

[0099]

Table 2

[0100]

[0101] The measurement method is as follows.

[0102] 1. The measurement of "volume absolute humidity in the package" is to insert the measuring part of the thermo-hygrometer into the packaging film within 30 seconds after opening the package, regardless of the storage time. After resealing, the value after 5 minutes is used as the volume absolute humidity.

[0103] In Example 2, when a battery-type thermometer and hygrometer are sealed together in the packaging film and continuously measured, the recording frequency is set to every 5 minutes, and the volume absolute humidity within 5 minutes just before the package is opened is taken as the "volume absolute humidity in the package sealed together with the battery-type thermometer and hygrometer". The measurement at the initial stage of packaging is the value measured without the storage period in the above measurement.

[0104] The volume absolute humidity was calculated using the following formula from the temperature (°C) and relative humidity (%) measured using a thermohygrometer.

[0105]

Number 2

[0106]

[0107] 2. The water vapor permeability in a 40°C / 90%RH atmosphere was measured by the method described in JIS Z0208-1976.

[0108] 3. Determination of the maximum moisture absorption capacity of desiccant

[0109] The measurement was performed under the condition of a relative humidity of 90% described in JIS Z 0701-1977.

[0110] 4. Dielectric loss tangent

[0111] The dielectric loss tangent of the glass cloth at 10 GHz and 40 GHz was measured using a cavity resonator (TE011 mode) manufactured by AET. The thickness of the glass cloth was measured using the theoretical film thickness. The theoretical film thickness of the glass cloth is given by

[0112] Theoretical film thickness t (μm) = mass per unit area (g / m 2 ) / Specific gravity (g / cm 3 )

[0113] Figure it out.

[0114] 5. Changes in dielectric loss tangent

[0115] Dielectric loss tangent ratio = dielectric loss tangent of quartz glass cloth after storage / dielectric loss tangent of quartz glass cloth before storage

Claims

1. A method for packaging quartz glass cloth, comprising packaging quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, wherein the absolute humidity of the volume in the packaging is 10.0 g / m 3 the following.

2. The method for packaging quartz glass cloth according to claim 1, wherein: The absolute humidity of the volume inside the package is 5.0g / m 3 the following.

3. A packaging method for quartz glass cloth, comprising packaging quartz glass cloth containing 99.5% by mass or more of SiO2 with a packaging film, wherein the absolute humidity of the volume in the package within 5 minutes before the package is opened is 9.8 g / m 3 the following.

4. The method for packaging quartz glass cloth according to any one of claims 1 to 3, wherein: The packaging film has a water vapor permeability of 20 g / (m 2 · days) or less packaging film.

5. The method for packaging quartz glass cloth according to any one of claims 1 to 3, wherein: The packaging film is a film selected from polyethylene, polypropylene, polyester, nylon (PA), ethylene-vinyl alcohol copolymer and vinylidene chloride, organic resin composite film and metal vapor-deposited film.

6. The method for packaging quartz glass cloth according to any one of claims 1 to 3, wherein: Package the desiccant together in the packaging film.

7. The method for packaging quartz glass cloth according to claim 6, wherein: The desiccant has a maximum moisture absorption of 20% by mass or more at a relative humidity of 90%.

8. The method for packaging quartz glass cloth according to claim 6, wherein: The desiccant is selected from silica gel, bentonite, zeolite, calcium chloride, calcium oxide and phosphorus pentoxide.

9. The method for packaging quartz glass cloth according to any one of claims 1 to 3, wherein: The absolute humidity of the packaging film at the initial stage of packaging is 10.0g / m 3 the following.

10. The method for packaging quartz glass cloth according to claim 9, wherein: The absolute humidity of the packaging film at the initial stage of packaging is 5.0g / m 3 the following.

11. The method for packaging quartz glass cloth according to any one of claims 1 to 3, wherein: The gas in the package is dry air.

12. The method for packaging quartz glass cloth according to any one of claims 1 to 3, wherein: The gas in the package is inert gas.

13. A method for packaging quartz glass cloth, comprising packaging quartz glass cloth containing 99.5 mass % or more of SiO2 with a packaging film, wherein the packaging film has a water vapor permeability of 20 g / (m 2 · days) or less, and pack the desiccant together in the packaging film.

14. The method for packaging quartz glass cloth according to any one of claims 1, 3 and 13, wherein: After 1 day to 3 years from packaging, the dielectric loss tangent of the quartz glass cloth taken out from the packaging at 10 GHz was 0.0005 or less.

15. The method for packaging quartz glass cloth according to any one of claims 1, 3 and 13, wherein the quartz glass cloth containing 99.5% by mass or more of SiO2 is a quartz glass cloth treated with a silane coupling agent wherein the quartz glass cloth containing 99.5% by mass or more of SiO2 is treated with a silane coupling agent.