Cyclic olefin copolymer for polarizer and preparation method thereof
By using cyclic olefin copolymers prepared using specific catalyst systems and reaction conditions in liquid crystal displays, the problem in the existing technology that it is difficult to simultaneously increase the glass transition temperature and reduce hygroscopicity is solved, achieving high heat resistance and waterproof performance , which improves the display effect.
Patent Information
- Application Number
- CN202410838863.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-26
AI Technical Summary
It is difficult to simultaneously increase the glass transition temperature and reduce hygroscopicity of cyclic olefin copolymers in liquid crystal displays with existing technology, and cannot meet the high requirements for heat resistance and waterproofness of LCD and OLED screens.
Using a specific catalyst system and reaction conditions, the cyclic olefin copolymer obtained by the diene reaction is introduced, norbornene and ethylene gas are introduced to enhance the catalyst activity and stability, adjust the reaction rate and selectivity, and prepare a high glass transition temperature and low hygroscopicity cyclic olefin copolymers.
It significantly improves the glass transition temperature and waterproof performance of the cyclic olefin copolymer, improves the stability and durability of the display in humid environments, optimizes the optical properties of the polarizer, and improves the display effect.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polarizing elements, and in particular to a cycloolefin copolymer used in polarizers and a preparation method thereof. Background Art
[0002] With the advancement of science and technology, display technology has developed from the initial cathode ray tube display (CRT) to flat panel display technology (FPD), then to plasma display (PDP), liquid crystal display (LCD), and finally to the increasingly mature organic light emitting diode (OLED). The mainstream display technologies are LCD and OLED technologies. Liquid crystal display technology (LCD) is a non-self-luminous technology. Its main working principle is to control the liquid crystal to transmit or shield the light source: the backlight module in the screen provides a uniform background light source, and the light enters the liquid crystal panel after passing through the polarizer. When the liquid crystal is affected by the external electric field, the liquid crystal molecules will rearrange to allow the light to selectively pass through, thereby producing a light and dark effect and displaying the image; one of the key components of the display screen is the polarizer. The light emitted by the backlight module is converted into polarized light after passing through the lower polarizer, and then reaches the upper polarizer through the liquid crystal layer. The upper polarizer analyzes the polarized light passing through the liquid crystal to produce a display screen; without a polarizer, the LCD screen cannot display any image.
[0003] Polarizer is a composite film composed of different optical films, including core polarizing element PVA film, TAC film, pressure-sensitive adhesive, protective film, and release film. The raw material of PVA film, the core polarizing element in polarizer, is polyvinyl alcohol with high transparency and high ductility. After the PVC film absorbs the two-dimensional absorption molecules of iodine and undergoes stretching and alignment, it can polarize light. The PVA film is covered by two layers of TAC film, so the TAC film is considered to be the most important protective layer in the polarizer. On the one hand, it supports the PVA film, and on the other hand, it protects the PVA from damage by water vapor and the like. TAC film, or triacetate cellulose film, has good support, transparency, UV resistance, and acid and alkali resistance. However, due to industry monopoly, the procurement cost of TAC film is high. In addition, the technical challenges and upgrades faced by LCD and OLED screens have also led to the gradual replacement of TAC film: for LCD screens, the shrinkage of the polarizer caused by the uneven heat of the backlight module and the high durability requirements of materials for long-distance transportation have caused the industry to begin to introduce other materials to replace TAC film; for OLED screens, since OLED will gradually be used in high-power electronic components such as 5G mobile phones, this development prospect has put forward new requirements for the heat resistance and waterproofness of the screen, and the high heat resistance and low moisture absorption of cycloolefin copolymer film make it the best substitute for TAC material.
[0004] CN116396430A discloses a cycloolefin copolymer, a preparation method and application thereof. The cycloolefin copolymer is a non-crystalline polymer with low hygroscopicity, high light transmittance, high refractive index, chemical resistance and mechanical strength. Compared with ordinary cycloolefin copolymers, the cycloolefin copolymer obtained in the preparation method of the invention can significantly improve heat resistance, and has high glass transition temperature and heat deformation temperature.
[0005] CN113354775A discloses a method for preparing a cycloolefin copolymer and its application in preparing heat-resistant optical materials. The preparation method comprises: a cycloolefin monomer and ethylene are subjected to an addition copolymerization reaction under the catalysis of a catalyst and a co-catalyst to obtain the cycloolefin copolymer; the catalytic system selected in the invention exhibits a higher catalytic activity and a higher conversion rate of the cycloolefin monomer.
[0006] The solutions reported in the above patent documents are all aimed at improving heat resistance, including glass transition temperature, but cannot solve the problem of reducing hygroscopicity at the same time. Summary of the invention
[0007] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to add cycloolefin copolymer to the cycloolefin copolymer film of the polarizer, so as to improve the glass transition temperature and waterproofness in screen applications.
[0008] To achieve the above object, the present invention provides a cycloolefin copolymer used in polarizer and a preparation method thereof.
[0009] A method for preparing a cyclic olefin copolymer for use in a polarizer comprises the following steps:
[0010] (1) Add 2,3-diaminotoluene, 1-cyclopentenecarboxaldehyde and titanocene dichloride to toluene, stir at 50-60° C. for 6-8 hours, cool to room temperature, filter through a silica gel pad 4-6 times to obtain the co-catalyst-toluene solution for later use;
[0011] (2) The reaction bottle is heated to 60-65° C., vacuumed at 0.1-0.5 MPa for 4-6 hours, replaced with nitrogen, and norbornene-toluene solution and triisobutylaluminum are added. The reaction bottle is replaced with nitrogen. Stirring is started at 60-65° C. and 200-300 r / min, and 0.5-1 atm ethylene gas is introduced. Vinylbisindenyl zirconium dichloride-toluene solution and co-catalyst-toluene solution are added, and stirred for 10-30 minutes. Stirring is stopped, and the solution is kept warm for 1-2 hours. Hydrogen chloride-ethanol solution is added dropwise to terminate the reaction and produce a precipitate. The precipitate is filtered, and the filter cake is washed with anhydrous ethanol for 2-4 times. The cycloolefin copolymer for polarizer is obtained.
[0012] The thickness of the silica gel pad in step (1) is 4-6 cm.
[0013] The silica gel pad in step (1) is 1000-2000 mesh silica gel powder.
[0014] In the step (1), the weight ratio of 2,3-diaminotoluene, 1-cyclopentenecarboxaldehyde, dichlorotitanocene and toluene is 0.02-0.04: 0.01-0.02: 0.004-0.008: 0.4-0.8.
[0015] In the step (2), the weight ratio of norbornene-toluene solution, triisobutylaluminum, vinylbisindenyl zirconium dichloride-toluene solution, co-catalyst-toluene solution, and hydrogen chloride-ethanol solution is 20-25: 0.01-0.02: 0.2-0.5: 0.5-1: 50-60.
[0016] The norbornene-toluene solution in step (2) is a 5-10 wt % norbornene-toluene solution.
[0017] The vinylbisindenyl zirconium dichloride-toluene solution in step (2) is a 6-12 wt % vinylbisindenyl zirconium dichloride-toluene solution.
[0018] The concentration of the hydrogen chloride-ethanol solution in step (2) is 10-20 wt %.
[0019] The catalyst of the diene reaction has a significant impact on the product, which not only determines the activity and selectivity of the polymerization reaction, but also directly affects the molecular weight, molecular weight distribution, microstructure of the copolymer and the physical and chemical properties of the final material, such as heat resistance, transparency and mechanical strength.
[0020] The cycloolefin copolymer prepared by the present invention introduces norbornene and ethylene gas as raw materials for diene reaction in the reaction system, and uses a specific catalyst to catalyze the polymerization reaction. The addition of only the vinyl bis-indenyl zirconium dichloride catalyst may have disadvantages such as low activity and limited catalytic efficiency. The added triisobutyl aluminum can be used as a Lewis acid to further activate and improve the activity of the catalyst with the vinyl bis-indenyl zirconium dichloride complex intermediate, and promote the diene reaction. 2,3-Diaminotoluene and 1-cyclopentene carboxaldehyde are used as ligands to react with dichlorodipentadienyl titanocene to form a co-catalyst, which enhances the activity and stability of the vinyl bis-indenyl zirconium dichloride catalyst and reduces the generation of side reactions. At the same time, the reaction rate and selectivity are adjusted through the synergistic effect of the catalyst, so that the copolymerization reaction is more active and selective, and the copolymerization reaction of norbornene and ethylene is promoted, so as to obtain a copolymer with specific properties for use in polarizers.
[0021] Beneficial effects of the present invention:
[0022] 1. Compared with the prior art, the cycloolefin copolymer prepared by the present invention has a higher glass transition temperature, lower hygroscopicity, better heat resistance, and can improve the waterproof performance in the application, which is of great significance in improving the stability and durability of the display screen in a humid environment;
[0023] 2. Compared with the prior art, the influence of the catalyst of the diene reaction on the product determines the activity and selectivity of the polymerization reaction. The cycloolefin copolymer prepared by the present invention introduces norbornene and ethylene gas into the reaction system as raw materials for the diene reaction, and adopts a specific catalyst to catalyze the polymerization reaction; by enhancing the activity and stability of the catalyst, the generation of side reactions is reduced, and at the same time, the reaction rate and selectivity are adjusted through the synergistic effect of the catalyst, so that the copolymerization reaction is more active and selective, and the copolymerization reaction of norbornene and ethylene is promoted, so as to obtain a copolymer with specific properties for use in polarizers.
[0024] 3. Compared with the prior art, the cycloolefin copolymer obtained by the preparation method of the present invention is applied to the cycloolefin copolymer film in the polarizer, which can optimize the optical properties of the polarizer, improve the display effect of the display screen, and make the image clearer and the color more vivid. DETAILED DESCRIPTION
[0025] The parameters of the specific chemical substances used in the examples are from the following sources:
[0026] Norbornene: The manufacturer is Wuhan KMK Biopharmaceutical Technology Co., Ltd., model number is KMK498-66-8.
[0027] 2,3-Diaminotoluene: The manufacturer is Hubei Qifei Pharmaceutical Chemical Co., Ltd., and the product number is QF5041.
[0028] 1-Cyclopentenecarboxaldehyde: The manufacturer is Hubei Weideli Chemical Technology Co., Ltd., and the product number is D18725.
[0029] Vinylbisindenylzirconium dichloride: The manufacturer is Guangdong Wengjiang Chemical Reagent Co., Ltd., and the product number is PA97774.
[0030] Zirconocene dichloride: The manufacturer is Wuxi Yaodesin Chemical Products Co., Ltd., and the product number is 1011.
[0031] Biscyclopentadienyl dimethyl titanium: The manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., and the product number is T23573.
[0032] The commercially available cyclic olefin copolymer in Example 3 has a brand of German TOPAS8007, a manufacturer of Guangzhou Hongcheng Plastic Chemical Co., Ltd., and a model of COC8007F-04. Embodiment 1:
[0033] A method for preparing a cyclic olefin copolymer for use in a polarizer comprises the following steps:
[0034] The reaction bottle was heated to 60°C, vacuumed at 0.1 MPa for 4 hours, replaced with nitrogen, 200 g of 6 wt% norbornene-toluene solution and 0.15 g of triisobutylaluminum were added, replaced with nitrogen, stirring was started at 60°C and 250 r / min, and 1 atm of ethylene gas was introduced, 4 g of 10 wt% vinyl bisindenyl zirconium dichloride-toluene solution was added, stirred for 15 minutes, stirring was stopped, and the mixture was kept warm for 1 hour, 500 g of 10 wt% hydrogen chloride-ethanol solution was added dropwise to terminate the reaction and produce a precipitate, which was filtered, the filter cake was washed twice with anhydrous ethanol, and dried in a vacuum oven at 65°C to obtain the cycloolefin copolymer used for the polarizer.
[0035] Comparative Example 1: A method for preparing a cyclic olefin copolymer for use in a polarizer, comprising the following steps:
[0036] The reaction bottle was heated to 60°C, vacuumed at 0.1 MPa for 4 hours, replaced with nitrogen, 200 g of 6 wt% norbornene-toluene solution and 0.15 g of triisobutylaluminum were added, replaced with nitrogen, stirring was started at 60°C and 250 r / min, and 1 atm of ethylene gas was introduced, 4 g of 10 wt% zirconocene dichloride-toluene solution was added, stirred for 15 minutes, stirring was stopped, and the mixture was kept warm for 1 hour, 500 g of 10 wt% hydrogen chloride-ethanol solution was added dropwise to terminate the reaction and produce a precipitate, which was filtered, the filter cake was washed twice with anhydrous ethanol, and dried in a vacuum oven at 65°C to obtain the cycloolefin copolymer used for the polarizer.
[0037] Comparative Example 2: A method for preparing a cyclic olefin copolymer for use in a polarizer, comprising the following steps:
[0038] The reaction bottle was heated to 60°C, vacuumed at 0.1 MPa for 4 hours, replaced with nitrogen, 200 g of 6 wt% norbornene-toluene solution and 0.15 g of triisobutylaluminum were added, replaced with nitrogen, stirring was started at 60°C and 250 r / min, and 1 atm ethylene gas was introduced, 4 g of 10 wt% biscyclopentadienyl dimethyltitanium-toluene solution was added, stirred for 15 minutes, stirring was stopped, and the mixture was kept warm for 1 hour, 500 g of 10 wt% hydrogen chloride-ethanol solution was added dropwise to terminate the reaction and produce a precipitate, which was filtered, the filter cake was washed twice with anhydrous ethanol, and dried in a vacuum oven at 65°C to obtain the cycloolefin copolymer used for the polarizer. Embodiment 2:
[0039] A method for preparing a cyclic olefin copolymer for use in a polarizer comprises the following steps:
[0040] (1) Add 0.2 g of 2,3-diaminotoluene, 0.13 g of 1-cyclopentenecarboxaldehyde, and 0.05 g of dichlorotitanocene to 6 g of toluene, stir at 55° C. for 8 hours, cool to room temperature, and filter through a 6 cm, 1800 mesh silica gel pad 4 times to obtain the co-catalyst-toluene solution for standby use;
[0041] (2) The reaction flask was heated to 60°C, vacuumed at 0.1 MPa for 4 hours, replaced with nitrogen, 200 g of 6 wt% norbornene-toluene solution and 0.15 g of triisobutylaluminum were added, the atmosphere was replaced with nitrogen, stirring was started at 60°C and 250 r / min, and 1 atm of ethylene gas was introduced, 4 g of 10 wt% vinylbisindenyl zirconium dichloride-toluene solution and 6 g of co-catalyst-toluene solution were added, stirred for 15 minutes, stirring was stopped, the temperature was kept for 1 hour, 500 g of 10 wt% hydrogen chloride-ethanol solution was added dropwise to terminate the reaction and produce a precipitate, which was filtered, the filter cake was washed twice with anhydrous ethanol, and dried in a vacuum oven at 65°C to obtain the cycloolefin copolymer used for polarizer.
[0042] Comparative Example 3 A method for preparing a cyclic olefin copolymer used in a polarizer comprises the following steps:
[0043] (1) Add 0.2 g of 2,3-diaminotoluene, 0.13 g of benzaldehyde, and 0.05 g of titanocene dichloride to 6 g of toluene, stir at 55° C. for 8 hours, cool to room temperature, and filter through a 6 cm, 1800 mesh silica gel pad 4 times to obtain the co-catalyst-toluene solution for later use;
[0044] (2) The reaction flask was heated to 60°C, vacuumed at 0.1 MPa for 4 hours, replaced with nitrogen, 200 g of 6 wt% norbornene-toluene solution and 0.15 g of triisobutylaluminum were added, the atmosphere was replaced with nitrogen, stirring was started at 60°C and 250 r / min, and 1 atm of ethylene gas was introduced, 4 g of 10 wt% vinylbisindenyl zirconium dichloride-toluene solution and 6 g of co-catalyst-toluene solution were added, stirred for 15 minutes, stirring was stopped, the temperature was kept for 1 hour, 500 g of 10 wt% hydrogen chloride-ethanol solution was added dropwise to terminate the reaction and produce a precipitate, which was filtered, the filter cake was washed twice with anhydrous ethanol, and dried in a vacuum oven at 65°C to obtain the cycloolefin copolymer used for polarizer.
[0045] Comparative Example 4 A method for preparing a cyclic olefin copolymer used in a polarizer comprises the following steps:
[0046] (1) Add 0.2 g of 3-chloro-2-methylaniline, 0.13 g of 1-cyclopentenecarboxaldehyde, and 0.05 g of titanocene dichloride to 6 g of toluene, stir at 55° C. for 8 hours, cool to room temperature, and filter through a 6 cm, 1800 mesh silica gel pad 4 times to obtain the co-catalyst-toluene solution for later use;
[0047] (2) The reaction flask was heated to 60°C, vacuumed at 0.1 MPa for 4 hours, replaced with nitrogen, 200 g of 6 wt% norbornene-toluene solution and 0.15 g of triisobutylaluminum were added, the atmosphere was replaced with nitrogen, stirring was started at 60°C and 250 r / min, and 1 atm of ethylene gas was introduced, 4 g of 10 wt% vinylbisindenyl zirconium dichloride-toluene solution and 6 g of co-catalyst-toluene solution were added, stirred for 15 minutes, stirring was stopped, the temperature was kept for 1 hour, 500 g of 10 wt% hydrogen chloride-ethanol solution was added dropwise to terminate the reaction and produce a precipitate, which was filtered, the filter cake was washed twice with anhydrous ethanol, and dried in a vacuum oven at 65°C to obtain the cycloolefin copolymer used for polarizer.
[0048] Comparative Example 5: A method for preparing a cyclic olefin copolymer for use in a polarizer, comprising the following steps:
[0049] (1) Add 0.2 g of 2-amino-4-methylphenol, 0.13 g of 1-cyclopentenecarboxaldehyde, and 0.05 g of titanocene dichloride to 6 g of toluene, stir at 55° C. for 8 hours, cool to room temperature, and filter through a 6 cm, 1800 mesh silica gel pad 4 times to obtain the co-catalyst-toluene solution for later use;
[0050] (2) The reaction flask was heated to 60°C, vacuumed at 0.1 MPa for 4 hours, replaced with nitrogen, 200 g of 6 wt% norbornene-toluene solution and 0.15 g of triisobutylaluminum were added, the atmosphere was replaced with nitrogen, stirring was started at 60°C and 250 r / min, and 1 atm of ethylene gas was introduced, 4 g of 10 wt% vinylbisindenyl zirconium dichloride-toluene solution and 6 g of co-catalyst-toluene solution were added, stirred for 15 minutes, stirring was stopped, the temperature was kept for 1 hour, 500 g of 10 wt% hydrogen chloride-ethanol solution was added dropwise to terminate the reaction and produce a precipitate, which was filtered, the filter cake was washed twice with anhydrous ethanol, and dried in a vacuum oven at 65°C to obtain the cycloolefin copolymer used for polarizer. Embodiment 3:
[0051] The cyclic olefin copolymers prepared by Examples 1-2, Comparative Examples 1-5, and commercially available cyclic olefin copolymers were applied to the preparation of cyclic olefin copolymer films in polarizers, and the specific method was as follows:
[0052] The cycloolefin copolymer was added to a twin-screw extruder for extrusion granulation. The temperature of the barrel of the twin-screw extruder from the feed zone to the conveying section, compression section, metering section and head was 150, 180, 200, 220 and 200°C, respectively. After extrusion, it was water-cooled and air-dried to obtain a masterbatch, which was melted at a high temperature of 160°C and injected into a mold. The cycloolefin copolymer films corresponding to Examples 1-2 and Comparative Examples 1-5 were obtained by hot pressing at 140°C and a pressure of 35 kPa, and the film thickness was 2 mm.
[0053] Test Example 1: The glass transition temperature test was performed on the cycloolefin copolymer films corresponding to Examples 1-2, Comparative Examples 1-5, and commercially available cycloolefin copolymers obtained by the method of Example 3, and the commercially available cycloolefin copolymer films were used as a comparative test. The sample size was 60 mm × 10 mm × 2 mm, and 3 parallel samples were prepared for each group; the test method was based on the national standard GB / T 40396-2021 "Test method for glass transition temperature of polymer-based composite materials - Dynamic mechanical analysis (DMA)".
[0054] The instrument uses a dynamic mechanical analyzer, the heating rate can reach 1℃ / min-10℃ / min, the loading frequency can reach 0.1Hz-10Hz, the equipment frequency can be controlled to ±0.05Hz, the furnace temperature can reach -100℃~500℃, and the temperature can be controlled to ±0.5℃.
[0055] The samples were placed in the laboratory standard environment conditions of 23°C and 50% relative humidity for 24 hours, then stored in sealed bags and tested within 30 minutes.
[0056] Select the specimen test mode, select the three-point bending mode. The prestress is 1.0N; input the span and the width and thickness of the specimen, set the heating rate to 5℃ / min, and the loading frequency to 1Hz; conduct the test in an air atmosphere, set the operating program temperature segment; start from room temperature and end when the modulus change tends to be flat.
[0057] After the test parameters are set, start the program to conduct the test, the equipment automatically collects data and forms a spectrum; use the instrument-specific software to analyze the spectrum, mark the intersection of the two tangents when the storage modulus drops sharply, and use the corresponding temperature as the glass transition temperature. The test results take the arithmetic mean of the test results, and the results are retained to one decimal place; each sample is tested 3 times, and the average value is taken as the test result, which is summarized as described in Table 1.
[0058] Table 1 Glass transition temperature test
[0059] / Commercially available Example 1 Comparative Example 1 Comparative Example 2 Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Glass transition temperature / Tg 78℃ 158℃ 150℃ 155℃ 172℃ 164℃ 169℃ 166℃
[0060] As can be seen from Table 1, the glass transition temperatures of the cycloolefin polymers of Example 2 and Comparative Examples 3-5 are significantly higher than those of Example 1 and Comparative Examples 1-2, indicating that the co-catalyst plays a key role in improving the heat resistance of the copolymer. Comparative Examples 1-2 screened the main catalyst on the basis of Example 1, and the effect was slightly lower than the data of Example 1. The difference between Example 2 and Comparative Examples 3-5 lies in the difference in the co-catalysts, among which the Tg values of Comparative Examples 3-5 are relatively close, ranging between 164-169°C, which may reflect the similarity of the catalyst composition or preparation stability. The glass transition temperature of Example 2 is the highest, reflecting the controllability and consistency of the cycloolefin copolymer film, which may have potential advantages in heat resistance and stability. The glass transition temperatures of the cycloolefin polymers of Examples 1-2 and Comparative Examples 1-5 are both higher than those of commercially available cycloolefin copolymer films. A higher Tg value means that the copolymer can still maintain its mechanical properties and chemical stability at higher temperatures, which can meet the demand for improved heat resistance in applications. The cycloolefin copolymer obtained by the preparation method of Example 2 is applied to the cycloolefin copolymer film in the polarizer, and can have good heat resistance.
[0061] Test Example 2: The moisture absorption performance of the cycloolefin copolymer films corresponding to Examples 1-2, Comparative Examples 1-5, and commercially available cycloolefin copolymers obtained by the method of Example 3 was tested, and the commercially available cycloolefin copolymer film was used as a comparative test. Prepare a sample size of 30mm×30mm×2mm, and prepare 3 parallel samples in each group; weigh the initial weight before the test begins, and then naturally hang the cycloolefin copolymer film sample in the standard atmosphere, and weigh it after 48 hours until the continuous weighing mass difference does not exceed 1%, that is, the actual weight; and calculate the moisture absorption rate: (actual weight-initial weight) / initial weight×100%. The waterproof performance is judged by the water absorption rate. The summary is described in Table 2.
[0062] Table 2 Summary of moisture absorption rate
[0063] / Commercially available Example 1 Comparative Example 1 Comparative Example 2 Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Moisture absorption rate (%) 0.0070 0.0072 0.0075 0.0081 0.0058 0.0070 0.0068 0.0069
[0064] It can be seen from Table 2 that the moisture absorption performance of the commercially available cycloolefin copolymer films, the examples and the comparative examples are different. Overall, the moisture absorption rate of Example 2 is the best, indicating that the addition of a co-catalyst can improve the performance of the copolymer material. Applying the cycloolefin copolymer of Example 2 to the cycloolefin copolymer film in the polarizer can enhance its waterproof performance.
[0065] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for preparing a cyclic olefin copolymer for use in a polarizer, characterized in that: The following steps are involved: (1) Add 2,3-diaminotoluene, 1-cyclopentenecarboxaldehyde and dichlorotitanocene to toluene, stir at 50-60°C for 6-8 hours, cool to room temperature, filter through a silica gel pad 4-6 times to obtain a co-catalyst-toluene solution for later use; (2) The reaction bottle is heated to 60-65° C., vacuumed at 0.1-0.5 MPa for 4-6 hours, replaced with nitrogen, and norbornene-toluene solution and triisobutylaluminum are added. The reaction bottle is replaced with nitrogen. Stirring is started at 60-65° C. and 200-300 r / min, and 0.5-1 atm ethylene gas is introduced. Vinylbisindenyl zirconium dichloride-toluene solution and co-catalyst-toluene solution are added, and stirred for 10-30 minutes. Stirring is stopped, and the solution is kept warm for 1-2 hours. Hydrogen chloride-ethanol solution is added dropwise to terminate the reaction and produce a precipitate. The precipitate is filtered, and the filter cake is washed with anhydrous ethanol for 2-4 times. The cycloolefin copolymer for polarizer is obtained.
2. The method for preparing a cyclic olefin copolymer for use in a polarizer according to claim 1, wherein: The thickness of the silica gel pad in step (1) is 4-6 cm.
3. The method for preparing a cyclic olefin copolymer for use in a polarizer according to claim 1, wherein: In the step (1), the weight ratio of 2,3-diaminotoluene, 1-cyclopentenecarboxaldehyde, dichlorotitanocene and toluene is 0.02-0.04: 0.01-0.02: 0.004-0.008: 0.4-0.
8.
4. The method for preparing a cyclic olefin copolymer for use in a polarizer according to claim 3, wherein: The norbornene-toluene solution in step (2) is a 5-10 wt % norbornene-toluene solution.
5. The method for preparing a cyclic olefin copolymer for use in a polarizer according to claim 4, wherein: The vinylbisindenyl zirconium dichloride-toluene solution in step (2) is a 6-12 wt % vinylbisindenyl zirconium dichloride-toluene solution.
6. The method for preparing a cyclic olefin copolymer for use in a polarizer according to claim 5, wherein: The concentration of the hydrogen chloride-ethanol solution in step (2) is 10-20 wt %.
7. The method for preparing a cyclic olefin copolymer for use in a polarizer according to claim 6, wherein: In the step (2), the weight ratio of norbornene-toluene solution, triisobutylaluminum, vinylbisindenyl zirconium dichloride-toluene solution, co-catalyst-toluene solution, and hydrogen chloride-ethanol solution is 20-25: 0.01-0.02: 0.2-0.5: 0.5-1: 50-60.
Citation Information
Patent Citations
Preparation method of cycloolefin copolymer and application of cycloolefin copolymer in preparation of heat-resistant optical material
CN113354775A
Cycloolefin copolymer as well as preparation method and application thereof
CN116396430A
Double-active center composite catalyst and cycloolefin copolymer prepared from same
CN106674428A
Synthesis method of polylactic acid grafted cycloolefin copolymer
CN116589664A
Cycloolefin copolymer and its production
JP1993320268A