Composite resin cross-linking agent for oil field and preparation method thereof

By adding polyhydroxy resin and other raw materials to the phenolic resin cross-linking agent, a composite resin cross-linking agent with high gelling strength and temperature resistance is prepared, which solves the problem of poor stability of phenolic resin in high-temperature oil fields and achieves a better Efficient oilfield profile control and flooding effect.

CN118420854BActive Publication Date: 2024-10-22SHENGLI OILFIELD SHENGJIA CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410895189.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-22
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

Existing phenolic resin cross-linking agents are difficult to apply in high-temperature oil fields and suffer from problems such as dehydration and aging, rapid reaction, degradation, and gel breakage. Moreover, the gel formed has poor stability at high temperatures, affecting the oilfield profile control and flooding effect.

Method used

Using a composite resin cross-linking agent, adding polyhydroxy resin, phenol, formaldehyde aqueous solution and catalyst, through specific reaction steps and proportions, a plugging regulator with high gelling strength, temperature resistance and plugging rate is prepared for use in oil fields. application.

Benefits of technology

It significantly improves the gelling strength, plugging rate and temperature resistance of the plugging control agent formed by the composite resin cross-linking agent and polyacrylamide used in oil fields, meets the applicable needs of high-temperature oil fields, and extends the effective service life of the cross-linking agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of oil field technology, and in particular to a composite resin crosslinking agent for oil field and a preparation method thereof. The composite resin crosslinking agent for oil field comprises the following raw materials: phenol, formaldehyde aqueous solution, catalyst and polyhydroxy resin; the amount of the polyhydroxy resin added to the raw materials is 5-10% of the weight of phenol; the polyhydroxy resin is prepared from 4,4′-dihydroxydiphenyl ether, phloroglucinol and diepoxy monomer. The plugging agent prepared by the composite resin crosslinking agent for oil field and polyacrylamide provided by the present invention has excellent gelling strength, plugging rate and temperature resistance, and can meet the applicable requirements of high temperature oil fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil fields, in particular to a composite resin cross-linking agent for oil fields and a preparation method thereof. Background Art

[0002] The formation temperature of high-temperature oil fields is as high as 150℃, and the formation physical properties vary greatly, with permeability ranging from 50mD to 2000mD. Due to the heterogeneity of the formation itself, the water content of some oil wells has exceeded 90%, and the oil wells with lower water content are in the stage of rapid water content increase. Effective water control and oil increase measures (such as the most commonly used profile control and drive control technology) can effectively improve the water drive effect and achieve the purpose of improving the recovery rate.

[0003] Most of the plugging agents currently used are cross-linked polyacrylamide and metal ions or phenolic liquid prepolymers to form gels. However, there are some disadvantages. Metal ion gels have dehydration and aging phenomena, and the validity period is not long, and the effect is not ideal. The use of phenolic prepolymer solution is inconvenient for long-distance transportation and storage due to the short validity period of the liquid prepolymer crosslinking agent. At the same time, a certain amount of free formaldehyde remains in the prepolymer solution, which pollutes the environment and causes harm to construction workers when used. In addition, the long-term stability of the gel system formed by it is poor at high temperatures, and the rapid gelation speed at high temperatures causes blockage in the near-well area.

[0004] Patent technology document CN202110576061.2 discloses a long-storage phenolic resin cross-linker and a high-temperature, high-salt gel prepared using the same. The long-storage phenolic resin cross-linker has a storage time of more than 6 months, which meets the requirements of oilfield profile adjustment and flooding operations. The high-temperature, high-salt gel prepared using the long-storage phenolic resin cross-linker has good gelling properties. It can gel in high-mineralized water, that is, water hardness ≤3000mg / L, water mineralization ≤150000mg / L and temperature 70-120°C. The gelling time is controllable from 12h to 240h. However, the phenolic resin cross-linker contains a large amount of active low-order hydroxyphenols, which react rapidly at high temperatures and easily lead to premature degradation and gel breakage. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a composite resin cross-linking agent for oil fields and a preparation method thereof, so as to solve the problem that phenolic resin cross-linking agents are difficult to be applied to high-temperature oil fields.

[0006] Based on the above purpose, the present invention provides a composite resin cross-linking agent for oil fields, comprising the following raw materials: phenol, formaldehyde aqueous solution, catalyst and polyhydroxy resin;

[0007] Furthermore, the amount of the polyhydroxy resin added to the raw material is 5-10% by weight of phenol;

[0008] The dosage ratio of the phenol and formaldehyde aqueous solution is 235-282g:440ml;

[0009] The catalyst is sodium hydroxide;

[0010] The catalyst is added in an amount of 5-8% by weight of phenol;

[0011] Furthermore, the preparation method of the polyhydroxy resin is as follows: under a nitrogen atmosphere, adding a reaction monomer and tetrabutylammonium bromide to N,N-dimethylformamide, then heating to 150° C., stirring for reaction for 10-14 hours, rotary evaporation, washing, and vacuum drying to obtain a polyhydroxy resin;

[0012] Further, the reactive monomer is a mixture of a hydroxyl monomer and a diepoxy monomer in a molar ratio of 1.1:0.5;

[0013] Further, the hydroxy monomer is a mixture of 4,4′-dihydroxydiphenyl ether and phloroglucinol in a molar ratio of 1:0.1;

[0014] The diepoxy monomer is one or a mixture of diglycidyl ether, glycerol diglycidyl ether, 1,4-butanediol diglycidyl ether, bisphenol A diglycidyl ether and resorcinol diglycidyl ether.

[0015] Preferably, the mass concentration of the formaldehyde aqueous solution is 37%.

[0016] Preferably, the amount of tetrabutylammonium bromide added is 0.5-1% by weight of the reaction monomers.

[0017] Preferably, the amount of N,N-dimethylformamide added is 300-500% of the weight of the reaction monomers.

[0018] Furthermore, the present invention also provides a method for preparing a composite resin cross-linking agent for oil fields, characterized in that the specific steps are as follows:

[0019] (1) Add phenol to the reaction kettle, stir at 50°C for 10-20 minutes, then add the catalyst, heat to 60°C, and stir for 20-30 minutes to obtain the initial reactant;

[0020] (2) Add the formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 40-50 minutes, then add the catalyst and polyhydroxy resin, continue stirring at 60°C for 20-30 minutes, then raise the temperature to 90°C, continue stirring for 20 minutes, and finally dry to obtain a composite resin crosslinking agent for oil fields.

[0021] Preferably, the amount of catalyst added in step (1) is 4-6% by weight of phenol.

[0022] Preferably, the amount of catalyst added in step (2) is 1-2% by weight of phenol.

[0023] Furthermore, the composite resin cross-linking agent for oil fields is used to prepare a plugging control agent.

[0024] Preferably, the plugging control agent is prepared by mixing polyacrylamide, a composite resin cross-linking agent for oil fields and water in a weight ratio of 0.2:0.5:100.

[0025] Preferably, the relative molecular mass of the polyacrylamide is 15 million to 20 million, and the degree of hydrolysis is 15-20%.

[0026] Beneficial effects of the present invention:

[0027] The present invention adds polyhydroxy resin to the synthetic raw material of phenolic resin. The three-dimensional structure and abundant reaction sites of the polyhydroxy resin significantly improve the gel strength, plugging rate and temperature resistance of the plugging agent formed by the composite resin cross-linking agent and polyacrylamide for oil fields, and can meet the application requirements of high-temperature oil fields.

[0028] The present invention adopts 4,4'-dihydroxydiphenyl ether as the main hydroxyl monomer and diepoxy monomer to synthesize polyhydroxy resin for preparing composite resin crosslinking agent for oil field. 4,4'-dihydroxydiphenyl ether gives polyhydroxy resin a large number of ether bonds and benzene rings, thereby improving the gelling strength, plugging rate and temperature resistance of the plugging agent formed by the composite resin crosslinking agent for oil field and polyacrylamide.

[0029] The present invention further adds phloroglucinol having three reaction sites in the synthesis of the polyhydroxy resin, thereby giving the polyhydroxy resin a three-dimensional structure. When the phloroglucinol is added to a composite resin crosslinking agent for oil fields, it can be crosslinked with phenol and formaldehyde, thereby improving the gelling strength, plugging rate and temperature resistance of the plugging agent formed by the composite resin crosslinking agent for oil fields and polyacrylamide. DETAILED DESCRIPTION

[0030] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0031] The relative molecular mass of the polyacrylamide used in the specific implementation manner of the present invention is 18 million, and the degree of hydrolysis is 18%.

[0032] Example 1: A method for preparing a composite resin cross-linking agent for oil fields, the specific preparation steps are as follows:

[0033] S1: Under a nitrogen atmosphere, 20.2 g of 4,4′-dihydroxydiphenyl ether, 1.26 g of phloroglucinol, 6.5 g of diglycidyl ether and 0.15 g of tetrabutylammonium bromide were added to 92.1 g of N,N-dimethylformamide, and then the temperature was raised to 150° C., stirred for reaction for 10 h, rotary evaporated, washed, and vacuum dried to obtain a polyhydroxy resin;

[0034] S2: Add 235 g of phenol into a reaction kettle, stir at 50° C. for 10 min, then add 9.4 g of sodium hydroxide, heat to 60° C., and stir for 20 min to obtain a preliminary reactant;

[0035] S3: Add 440 ml of 37% formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 40 minutes, then add 2.4 g of sodium hydroxide and 11.8 g of polyhydroxy resin, continue stirring at 60°C for 20 minutes, then heat to 90°C, continue stirring for 20 minutes, and finally dry to obtain a composite resin cross-linking agent for oil fields.

[0036] Example 2: A method for preparing a composite resin cross-linking agent for oil fields, the specific preparation steps are as follows:

[0037] S1: Under a nitrogen atmosphere, 20.2 g of 4,4′-dihydroxydiphenyl ether, 1.26 g of phloroglucinol, 10.1 g of 1,4-butanediol diglycidyl ether and 0.17 g of tetrabutylammonium bromide were added to 137.2 g of N,N-dimethylformamide, and then the temperature was raised to 150° C., stirred for reaction for 12 h, rotary evaporated, washed and vacuum dried to obtain a polyhydroxy resin;

[0038] S2: Add 254 g of phenol into a reaction kettle, stir at 50° C. for 15 min, then add 12.7 g of sodium hydroxide, raise the temperature to 60° C., and stir for 25 min to obtain a preliminary reactant;

[0039] S3: Add 440 ml of 37% formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 45 minutes, then add 3.8 g of sodium hydroxide and 17.8 g of polyhydroxy resin, continue stirring at 60°C for 25 minutes, then heat to 90°C, continue stirring for 20 minutes, and finally dry to obtain a composite resin cross-linking agent for oil fields.

[0040] Example 3: A method for preparing a composite resin cross-linking agent for oil fields, the specific preparation steps are as follows:

[0041] S1: Under a nitrogen atmosphere, 20.2 g of 4,4′-dihydroxydiphenyl ether, 1.26 g of phloroglucinol, 17 g of bisphenol A diglycidyl ether and 0.41 g of tetrabutylammonium bromide were added to 206 g of N,N-dimethylformamide, and then the temperature was raised to 150° C., stirred for reaction for 14 h, rotary evaporated, washed and vacuum dried to obtain a polyhydroxy resin;

[0042] S2: Add 282 g of phenol into a reaction kettle, stir at 50°C for 20 min, then add 16.9 g of sodium hydroxide, raise the temperature to 60°C, and stir for 30 min to obtain a preliminary reactant;

[0043] S3: Add 440 ml of 37% formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 50 minutes, then add 5.6 g of sodium hydroxide and 28.2 g of polyhydroxy resin, continue stirring at 60°C for 30 minutes, then heat to 90°C, continue stirring for 20 minutes, and finally dry to obtain a composite resin cross-linking agent for oil fields.

[0044] Example 4: A method for preparing a composite resin cross-linking agent for oil fields, the specific preparation steps are as follows:

[0045] S1: Under nitrogen atmosphere, 20.2 g of 4,4′-dihydroxydiphenyl ether, 1.26 g of phloroglucinol, 11.1 g of resorcinol diglycidyl ether and 0.28 g of tetrabutylammonium bromide were added to 141.2 g of N,N-dimethylformamide, and then the temperature was raised to 150° C., stirred for reaction for 14 h, rotary evaporated, washed and vacuum dried to obtain a polyhydroxy resin;

[0046] S2: Add 260 g of phenol into the reaction kettle, stir at 50°C for 20 min, then add 13 g of sodium hydroxide, heat to 60°C, and stir for 30 min to obtain a preliminary reactant;

[0047] S3: Add 440 ml of 37% formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 50 minutes, then add 3.9 g of sodium hydroxide and 20.8 g of polyhydroxy resin, continue stirring at 60°C for 30 minutes, then heat to 90°C, continue stirring for 20 minutes, and finally dry to obtain a composite resin cross-linking agent for oil fields.

[0048] Example 5: A plugging agent, the specific preparation method is as follows:

[0049] 2 g of polyacrylamide, 5 g of the composite resin cross-linking agent for oil fields prepared in Example 1 and 1000 g of mineralized water with a mineralization degree of 30000 ppm were mixed evenly to obtain a plugging control agent.

[0050] Example 6: A plugging agent, the specific preparation method is as follows:

[0051] 2 g of polyacrylamide, 5 g of the composite resin cross-linking agent for oil fields prepared in Example 2, and 1000 g of mineralized water with a mineralization degree of 30000 ppm were mixed evenly to obtain a plugging agent.

[0052] Example 7: A plugging agent, the specific preparation method is as follows:

[0053] 2 g of polyacrylamide, 5 g of the composite resin cross-linking agent for oil fields prepared in Example 3 and 1000 g of mineralized water with a mineralization degree of 30000 ppm were mixed evenly to obtain a plugging agent.

[0054] Example 8: A plugging agent, the specific preparation method is as follows:

[0055] 2 g of polyacrylamide, 5 g of the composite resin cross-linking agent for oil fields prepared in Example 4 and 1000 g of mineralized water with a mineralization degree of 30000 ppm were mixed evenly to obtain a plugging agent.

[0056] Comparative Example 1:

[0057] S1: Add 254 g of phenol into a reaction kettle, stir at 50°C for 15 min, then add 12.7 g of sodium hydroxide, heat to 60°C, and stir for 25 min to obtain a preliminary reactant;

[0058] S2: Add 440 ml of 37% formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 45 minutes, then add 3.8 g of sodium hydroxide, continue stirring at 60°C for 25 minutes, then heat to 90°C, continue stirring for 20 minutes, and finally dry to obtain a cross-linking agent.

[0059] 2 g of polyacrylamide, 5 g of the cross-linking agent prepared in Comparative Example 1 and 1000 g of mineralized water with a mineralization degree of 30000 ppm were mixed evenly to obtain a plugging agent.

[0060] Comparative Example 2:

[0061] S1: Under a nitrogen atmosphere, 22.2 g of 4,4′-dihydroxydiphenyl ether, 10.1 g of 1,4-butanediol diglycidyl ether and 0.17 g of tetrabutylammonium bromide were added to 137.2 g of N,N-dimethylformamide, and then the temperature was raised to 150° C., stirred for reaction for 12 h, rotary evaporated, washed and vacuum dried to obtain a polyhydroxy resin;

[0062] S2: Add 254 g of phenol into a reaction kettle, stir at 50° C. for 15 min, then add 12.7 g of sodium hydroxide, raise the temperature to 60° C., and stir for 25 min to obtain a preliminary reactant;

[0063] S3: Add 440 ml of 37% formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 45 minutes, then add 3.8 g of sodium hydroxide and 17.8 g of polyhydroxy resin, continue stirring at 60°C for 25 minutes, then heat to 90°C, continue stirring for 20 minutes, and finally dry to obtain a cross-linking agent.

[0064] 2 g of polyacrylamide, 5 g of the cross-linking agent prepared in Comparative Example 2 and 1000 g of mineralized water with a mineralization degree of 30000 ppm were mixed evenly to obtain a plugging agent.

[0065] Comparative Example 3:

[0066] S1: Under a nitrogen atmosphere, 12.1 g of hydroquinone, 10.1 g of 1,4-butanediol diglycidyl ether and 0.17 g of tetrabutylammonium bromide were added to 137.2 g of N,N-dimethylformamide, and then the temperature was raised to 150°C, stirred for reaction for 12 h, rotary evaporated, washed and vacuum dried to obtain a polyhydroxy resin;

[0067] S2: Add 254 g of phenol into a reaction kettle, stir at 50° C. for 15 min, then add 12.7 g of sodium hydroxide, raise the temperature to 60° C., and stir for 25 min to obtain a preliminary reactant;

[0068] S3: Add 440 ml of 37% formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 45 min, then add 3.8 g of sodium hydroxide and 17.8 g of polyhydroxy resin, continue stirring at 60°C for 25 min, then heat to 90°C, continue stirring for 20 min, and finally dry to obtain a crosslinking agent;

[0069] 2 g of polyacrylamide, 5 g of the cross-linking agent prepared in Comparative Example 3 and 1000 g of mineralized water with a mineralization degree of 30000 ppm were mixed evenly to obtain a plugging agent.

[0070] Performance Testing:

[0071] Determination of gelation time and gelation strength: The gelation strength of the plugging agent prepared in Examples 5-8 was determined by the gelation plate method. The time when the gel reaches the maximum strength is the gelation time. The gelation strength is determined by a viscometer, and the viscosity value when the gel reaches the maximum strength is selected. The experimental temperature is 150°C. The results are shown in Table 1.

[0072] Temperature resistance: The plugging agents prepared in Examples 5-8 were aged at 150°C for 180 days, the viscosity of the jelly was measured, and the dehydration rate of the jelly (the ratio of the dehydration amount of the jelly to the total mass of the jelly) was calculated. The results are shown in Table 1.

[0073] Plugging performance: 0.3 times the pore volume of the plugging agent prepared in Example 5-8 was injected into the core (diameter 25 mm, length 600 mm) at a rate of 1 mL / min. The experimental temperature was set at 150 °C. After aging for 3 days, subsequent water flooding was carried out to test the plugging rate. The results are shown in Table 1.

[0074] Table 1 Performance test results

[0075]

[0076] Data Analysis:

[0077] It can be seen from Examples 5-8 that the composite resin cross-linking agent for oil fields prepared by the present invention can be cross-linked with polyacrylamide to form a three-dimensional network structure, can gel in a short time at 150°C, has high gel strength and high plugging rate, can meet the applicable requirements of oil fields, and with the increase of the amount of polyhydroxy resin added, the gel time decreases, which is mainly because the increase of polyhydroxy resin can increase the cross-linking sites and opportunities per unit volume, thereby accelerating the cross-linking, and it has high long-term thermal stability, which can meet the applicable requirements of high-temperature oil fields.

[0078] It can be seen from Example 2 and Comparative Example 1 that the polyhydroxy resin prepared by the present invention can significantly improve the gelling strength, plugging rate and temperature resistance of the plugging agent.

[0079] It can be seen from Example 2 and Comparative Examples 2 and 3 that the use of 4,4′-dihydroxydiphenyl ether and phloroglucinol in the polyhydroxy resin can further improve the gel strength, plugging rate and temperature resistance of the plugging agent. This is mainly because phloroglucinol provides more cross-linking sites to improve the gel strength and plugging rate, and the ether bond in 4,4′-dihydroxydiphenyl ether can rotate, thereby consuming energy through the adjustment of the intramolecular structure and increasing the temperature resistance.

[0080] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A composite resin crosslinking agent for oil fields, characterized in that: The method comprises the following raw materials: phenol, formaldehyde aqueous solution, catalyst and polyhydroxy resin; The amount of the polyhydroxy resin added to the raw material is 5-10% of the weight of phenol; The dosage ratio of the phenol and formaldehyde aqueous solution is 235-282g:440ml; The catalyst is sodium hydroxide; The catalyst is added in an amount of 5-8% by weight of phenol; The preparation method of the polyhydroxy resin is as follows: under a nitrogen atmosphere, adding a reaction monomer and tetrabutylammonium bromide to N,N-dimethylformamide, then heating to 150° C., stirring for reaction for 10-14 hours, rotary evaporation, washing, and vacuum drying to obtain the polyhydroxy resin; The reactive monomer is a mixture of a hydroxyl monomer and a diepoxy monomer in a molar ratio of 1.1:0.5; The hydroxy monomer is a mixture of 4,4′-dihydroxydiphenyl ether and phloroglucinol in a molar ratio of 1:0.1; The diepoxy monomer is one or a mixture of diglycidyl ether, glycerol diglycidyl ether, 1,4-butanediol diglycidyl ether, bisphenol A diglycidyl ether and resorcinol diglycidyl ether; The preparation steps of the composite resin cross-linking agent for oil fields are as follows: (1) Add phenol to the reaction kettle, stir at 50°C for 10-20 minutes, then add the catalyst, heat to 60°C, and stir for 20-30 minutes to obtain the initial reactant; (2) Add the formaldehyde aqueous solution to the preliminary reactants, stir at 60°C for 40-50 minutes, then add the catalyst and polyhydroxy resin, continue stirring at 60°C for 20-30 minutes, then raise the temperature to 90°C, continue stirring for 20 minutes, and finally dry to obtain a composite resin crosslinking agent for oil fields.

2. The composite resin cross-linking agent for oil fields according to claim 1, characterized in that: The mass concentration of the formaldehyde aqueous solution is 37%.

3. The composite resin cross-linking agent for oil fields according to claim 1, characterized in that: The added amount of the tetrabutylammonium bromide is 0.5-1% of the weight of the reaction monomer; the added amount of the N,N-dimethylformamide is 300-500% of the weight of the reaction monomer.

4. The composite resin cross-linking agent for oil fields according to claim 1, characterized in that: The amount of catalyst added in step (1) is 4-6% of the weight of phenol; and the amount of catalyst added in step (2) is 1-2% of the weight of phenol.

5. An application of the composite resin crosslinking agent for oil fields according to any one of claims 1 to 4, characterized in that: The composite resin cross-linking agent for oil fields is used to prepare a plugging control agent; the plugging control agent is prepared by mixing polyacrylamide, the composite resin cross-linking agent for oil fields and water in a weight ratio of 0.2:0.5:

100.

6. The use of the composite resin cross-linking agent for oil fields according to claim 5, characterized in that: The relative molecular mass of the polyacrylamide is 15 million to 20 million, and the hydrolysis degree is 15 to 20%.