Ion-conducting film and its preparation method and application
By using a porous zwitterionic conductive membrane in the flow battery, the pore structure is adjusted through the covalent bonding of the matrix resin and the pore modifier, which solves the problem of difficulty in balancing ion selectivity and conductivity in the existing membrane, and improves the efficiency of the flow battery. Battery performance and stability, reducing production costs.
Patent Information
- Application Number
- CN202410781348.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-18
AI Technical Summary
Existing ion conductive membranes have problems in balancing ion selectivity and conductivity in flow batteries. Nafion membranes have high cost and vanadium ion permeability issues. In addition, existing modification solutions have limited scope of use and poor production convenience. full.
Using a porous zwitterionic conductive membrane, the pore structure is adjusted to improve ion conductivity and selectivity through the covalent bonding of the matrix resin composition and the pore modifier, using hydrophilic and hydrophobic polymers, inorganic fillers and ionic liquids , control the molecular weight and proportion of the pore modifier to form a membrane with a porosity of 30% to 75%.
It achieves the balance of ion conductivity and selectivity in the flow battery, improves the current efficiency and voltage efficiency, has good chemical stability and anti-oxidation properties, and reduces the swelling rate and production cost of the membrane.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of polymer materials, and specifically relates to an ion-conducting film and a preparation method and application thereof, and in particular to an amphoteric ion-conducting film for battery diaphragms and a preparation method and application thereof, and is particularly suitable for diaphragms used in liquid flow batteries. Background Art
[0002] With the increasing depletion of traditional fossil fuels and the environmental pollution they cause, there is an urgent need to develop environmentally friendly renewable energy. Renewable energy sources such as solar energy, hydropower, and wind power are intermittent and volatile, and require large-scale energy storage systems to achieve continuous and reliable power output. Liquid flow batteries are one of the most important large-scale energy storage systems, with the advantages of high energy efficiency, large storage capacity, no geographical restrictions, deep discharge depth, long working life, and environmental friendliness. Ion conduction membranes are the most core component materials in liquid flow batteries. First, it plays the role of transferring hydrogen ions in the electrolyte to complete the internal circuit of the battery; second, it separates the positive and negative electrolytes to prevent cross-mixing; third, it separates the positive and negative current collectors to prevent battery short circuits. The Nafion series of perfluorosulfonic acid membranes produced by DuPont in the United States are the most representative and commercially successful ion conduction membranes. However, the Nafion membrane has problems such as poor barrier capacity and high cost, which hinders its promotion and application in the further commercialization of liquid flow batteries.
[0003] In recent years, there have been many studies on ion conduction membranes for flow batteries. The existing technologies mainly adopt the technical routes of blending modification of Nafion resin with other organic and inorganic materials, sulfonation or quaternization modification of non-fluorine resins, hybrid modification of various resins and inorganic fillers, and multi-layer thin film composite modification. Among them, the physical morphology of the membrane is mainly classified into dense membrane and porous membrane, and it can be divided into perfluorinated membrane, partially fluorinated membrane, and non-fluorinated membrane according to whether it contains fluorine.
[0004] Reference 1 discloses a blended membrane for all-vanadium redox flow battery and a preparation method thereof. In order to solve the problems that the currently used Nafion membrane is very easy to swell in water, has poor dimensional stability, reduces mechanical strength, and has a high vanadium ion permeability, which limits the needs of large-scale commercial batteries, a perfluorosulfonic acid ion exchange resin (PFSA) and sulfonated polybenzimidazole (SPBI) blended ion exchange membrane with improved dimensional stability, mechanical strength, and reduced vanadium ion permeability is prepared, and the blended membrane is suitable for all-vanadium redox flow battery (VRB).
[0005] Reference 2 discloses an all-vanadium liquid flow battery membrane and a preparation method thereof. The main technical means is to perform polymer radiation grafting on PVDF and composite it with inorganic carbon materials, and then perform sulfonation and protonation, and then dry it to obtain a zwitterionic ion exchange membrane.
[0006] Reference 3 discloses a zwitterionic ion exchange membrane for an all-vanadium liquid flow battery. The zwitterionic membrane is made by solution casting and acidification. The solution casting is to pour a mixed solution containing a first polymer and a second polymer into a mold for solidification. The first polymer is a polymer containing a sulfonic acid group, and the second polymer is a polymer containing an N-heterocyclic cation or a quaternary ammonium cation.
[0007] Reference 4 discloses a cross-linked amphoteric ion exchange membrane and its preparation method and application. An ion exchange membrane having both cation and anion exchange capabilities is prepared by using sodium styrene sulfonate monomers with sulfonic acid groups and N-(4-vinylbenzyl)-N,N-dialkylamine monomers with tertiary amine groups for polymerization, and introducing a cross-linking agent divinylbenzene, which reduces the vanadium migration phenomenon to a certain extent. The addition of the cross-linking agent divinylbenzene polymerizes the linear molecules into a cross-linked spatial network structure.
[0008] Reference 5 discloses a polybenzimidazole type zwitterionic ion exchange membrane material and a preparation method and application thereof. The polybenzimidazole type zwitterionic ion exchange membrane material has good antioxidant properties, high chemical stability and thermal stability and a long service life.
[0009] Although the above existing technologies have conducted research on ion-conducting membranes to a certain extent, there is still a lot of room for discussion on comprehensively improving the performance of the membranes.
[0010] References:
[0011] Reference 1: CN102881853A
[0012] Reference 2: CN107658478A
[0013] Reference 3: CN109103483A
[0014] Reference 4: CN115160476A
[0015] Reference 5: CN114213688A Summary of the invention
[0016] Problem that the invention aims to solve
[0017] As mentioned above, although cation exchange membranes represented by Nafion membranes have high ion conductivity and chemical stability, they are highly permeable to metal ions, especially vanadium ions, so there is a phenomenon of cross contamination, poor ion selectivity, and high price. On the other hand, anion exchange membranes have good ion selectivity due to the Donnan exclusion effect, but low conductivity, which shows that it is difficult to achieve a balance between ion conductivity and selectivity.
[0018] On this basis, the use of amphoteric ion exchange membranes has been proposed to solve the contradiction between cation and anion exchange membranes. Such attempts, for example, are cited in references 1 to 5, which respectively prepare amphoteric ion exchange membranes for batteries, especially (all-vanadium) flow batteries, by using Nafion resins and other organic and inorganic materials for blending and modification, non-fluorine-based resins for sulfonation or quaternization, hybrid modification of multiple resins and inorganic fillers, and multi-layer film composite modification. However, it is also found that the scope of use of the diaphragms obtained by these schemes is relatively limited, and the specific implementation effect, product index performance, and convenience of continuous production are still insufficient.
[0019] Therefore, the primary purpose of the present invention is to provide a zwitterionic ion conductive film for batteries, especially liquid flow batteries. The zwitterionic ion conductive film is a composite porous ion conductive membrane of multiple materials, which is particularly suitable for use as an ion conductive diaphragm in liquid flow batteries (such as all-vanadium liquid flow batteries, iron-chromium liquid flow batteries, zinc-bromine liquid flow batteries, zinc-iron liquid flow batteries, all-iron liquid flow batteries, etc.), and not only has excellent ion conductivity and ion selectivity, but also has excellent chemical stability.
[0020] In addition, the present invention also provides a method for preparing a zwitterionic ion conductive film for a battery, especially a liquid flow battery. The preparation method is simple and easy to implement with low cost.
[0021] In addition, the present invention also provides a battery device, which comprises the above-mentioned zwitterionic ion conductive film. In particular, such a battery device is a liquid flow battery device.
[0022] Solutions for solving problems
[0023] [1] The present invention first proposes a zwitterionic conductive film, which is a porous membrane with a pore structure.
[0024] The porous membrane is formed from a matrix resin composition, and a pore modifier exists in the pore structure;
[0025] Wherein, the matrix resin composition comprises a hydrophilic polymer;
[0026] The pore modifier includes a polymer having a cationic functional group and an anionic functional group, and the pore modifier is bonded to the inner wall of the pore structure through a covalent bond;
[0027] The porosity of the zwitterionic conductive film is 30% to 75%.
[0028] [2] The zwitterionic ion conductive film according to [1], wherein the matrix resin composition comprises a hydrophilic polymer, a hydrophobic polymer and an inorganic filler, and optionally further comprises an ionic liquid.
[0029] [3] The zwitterion conductive film according to [1] or [2], wherein the content of the hydrophilic polymer in the matrix resin composition is 10% by mass to 50% by mass.
[0030] [4] The zwitterion conductive film according to any one of [1] to [3], wherein the hydrophilic polymer comprises a combination of one or more of cellulose and its derivatives, polyvinyl alcohol and its copolymers.
[0031] [5] The zwitterionic ion conductive film according to any one of [1] to [4], wherein the anionic functional group in the pore modifier comprises a sulfonic acid group; and the cationic functional group in the pore modifier comprises a quaternary ammonium group.
[0032] [6] The zwitterionic ion conductive film according to any one of [1] to [5], wherein the molar ratio of the cationic functional group to the anionic functional group in the pore modifier is 1:1 to 1:5.
[0033] [7] The zwitterion conductive film according to any one of [1] to [6], wherein the pore modifier is derived from a polyurethane polymer.
[0034] [8] The zwitterion conductive film according to any one of [1] to [7], wherein the zwitterion conductive film has a thickness of 10 μm to 500 μm.
[0035] [9]. Furthermore, the present invention also provides a method for preparing the zwitterionic ion conductive film according to any one of [1] to [8], comprising the following steps:
[0036] The step of preparing the porous membrane comprises mixing the raw materials for forming the matrix resin composition and obtaining the porous membrane having a porous channel structure through extrusion and coagulation bath treatment;
[0037] The step of modifying is to combine the porous membrane with a multi-porous structure through a pore modifier.
[0038]
[10] The method according to [9], wherein in the step of preparing the porous membrane, the coagulation bath is an aqueous solution containing an ionic liquid.
[0039]
[11] The method according to [9] or
[10] , wherein in the modification step, the pore modifier is covalently linked to the inner wall of the pore structure by in situ polymerization in the pore structure.
[0040]
[12] . In addition, the present invention also provides a battery device, wherein the battery device comprises the zwitterion conductive film according to any one of [1] to [8] or the zwitterion conductive film prepared by the method according to any one of [9] to
[11] .
[0041]
[13] The battery device according to
[12] , wherein the battery device is a liquid flow battery device.
[0042] Effects of the Invention
[0043] By implementing the above technical solution, the present invention can achieve the following technical effects:
[0044] 1) The zwitterionic conductive film of the present invention is a porous membrane with a pore structure. It uses a pore modifier containing a specific functional group to covalently modify the pore structure of the base resin. On the one hand, the polymer with zwitterionic conductivity is fixed to the surface of the pore, thereby regulating the transmission of anions and cations; on the other hand, the molecular weight of the pore modifier can be flexibly adjusted by controlling the raw materials and processes, thereby playing a role in modifying and regulating the pore size. The two aspects work together to balance the ion conductivity and selectivity, while improving the conductivity of the conductive ions and inhibiting the interpenetration of the redox couple ions, thereby improving the current efficiency and voltage efficiency of the flow battery, and having a higher energy efficiency.
[0045] 2) The zwitterionic ion conductive film of the present invention uses cationic functional groups and anionic functional groups as specific functional groups. By flexibly adjusting the ratio of the two, the balance of anion and cation transport can be adjusted respectively, thereby further improving ion conductivity and selectivity.
[0046] 3) The matrix resin composition in the zwitterionic ion conductive film of the present invention can have good acid and alkali resistance and antioxidant properties by selecting different resins, and the pore modification polymer used for zwitterionic ion conduction mainly exists on the surface of the pore structure, rather than in the molecular chain of the matrix resin, and will not affect the acid and alkali resistance and antioxidant properties of the matrix resin, thereby maintaining the acid and alkali resistance and antioxidant properties of the zwitterionic ion conductive film.
[0047] 4) In some preferred embodiments, the zwitterionic ion conductive film of the present invention also contains an ionic liquid, which has a strong affinity for protons and can effectively enhance the conductivity of protons, thereby improving the voltage efficiency of the liquid flow battery.
[0048] 5) Inorganic nanomaterials can also be used in the zwitterionic conductive film of the present invention for compounding, which can play a role in assisting pore formation and improving porosity, and can effectively reduce the swelling rate of the membrane on the other hand. DETAILED DESCRIPTION
[0049] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.
[0050] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.
[0051] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0052] In this specification, the numerical range expressed using "above" or "below" means a numerical range including the number.
[0053] In this specification, the word "may" means both performing a certain process and not performing a certain process.
[0054] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.
[0055] In this specification, the "normal temperature" or "room temperature" used means an indoor ambient temperature of "23±2°C".
[0056] In this specification, unless otherwise stated, "%" used means weight or mass percentage.
[0057] In this specification, the use of "substantially" means that the standard deviation from a theoretical model or theoretical data is within a numerical range of 5%, preferably 3%, and more preferably 1%.
[0058] In this specification, when the terms “include” and / or “comprise” are used, they indicate the existence of features, steps, operations, devices, components and / or their combinations.
[0059] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.
[0060] The present invention mainly provides a zwitterionic ion conductive film for batteries, especially for liquid flow batteries. The zwitterionic ion conductive film is a composite of multiple materials and has a porous ion conductive membrane with a pore structure. It is particularly suitable for use as an ion conductive diaphragm in various liquid flow batteries (such as all-vanadium liquid flow batteries, iron-chromium liquid flow batteries, zinc-bromine liquid flow batteries, zinc-iron liquid flow batteries, all-iron liquid flow batteries, etc.). It not only has excellent ion conductivity and ion selectivity, but also has excellent chemical stability.
[0061] The present invention is mainly obtained through the following insights:
[0062] Ion exchange membranes represented by Nafion membranes and their modified products still have the problem of the trade-off between ion permeability and ion selectivity. In addition, the usual modification involves the blending modification of the membrane itself. Therefore, there are also problems such as improved ion permeability and selectivity but reduced stability or strength.
[0063] After long-term research, the inventors of the present invention have found that by covalently bonding a polymer having a special group that can conduct anions and cations in the pore structure of the film, the conduction capacity of anions and cations can be adjusted, and the pore size of the pore can be controlled by controlling the molecular size of the polymer, thereby balancing the conductivity and selectivity of the ions. In addition, since the special group that can conduct anions and cations mainly exists in the pore structure, it will not affect the acid and alkali resistance and oxidation resistance of the base resin, thereby improving the chemical stability of the conductive film.
[0064] Furthermore, in some preferred processes, the special groups that can conduct anions and cations can be derived from sulfonic acid (salt) groups and quaternary ammonium (salt) groups. Through the coordination and adjustment of the two groups, the balance of anion and cation transport capabilities can be further improved.
[0065] <First aspect>
[0066] The present invention primarily provides a zwitterionic ion conductive membrane for batteries, especially suitable for various liquid flow batteries.
[0067] The zwitterionic ion conducting film of the present invention is a porous film having a pore structure, and such a pore structure may be a pore structure penetrating in the thickness direction of the film.
[0068] The porous membrane is formed from a matrix resin composition, and a pore modifier exists in the pore structure;
[0069] Wherein, the matrix resin composition comprises a hydrophilic polymer, which can be advantageously covalently bonded to the pore modification;
[0070] The pore modifier includes a polymer having a cationic functional group and an anionic functional group, and the pore modifier is bonded to the inner wall of the pore structure through a covalent bond;
[0071] By controlling the molecular weight of the pore modifier polymer, the porosity of the amphoteric ion conductive film can be adjusted to 30% to 75%, which ensures both the ion permeation efficiency and good ion permeation selectivity.
[0072] (Matrix resin composition)
[0073] The matrix resin composition of the present invention is mainly used to form the main body of the porous membrane.
[0074] The matrix resin composition of the present invention necessarily contains a hydrophilic polymer. The hydrophilic polymer of the present invention can effectively provide the pore modifier with the inner wall of the pore structure by providing a hydrophilic group.
[0075] In principle, there is no particular limitation on the type of the hydrophilic group. In some preferred embodiments, these groups may be one or more of hydroxyl, amino, thiol, etc. Preferably, the hydrophilic group is hydroxyl.
[0076] In a further preferred embodiment, the hydrophilic polymer of the present invention can be selected from organic polymers containing a polyhydroxy structure, such as a combination of one or more of cellulose and its derivatives, polyvinyl alcohol and its copolymers. The cellulose derivatives can include various cellulose ethers, cellulose esters, cellulose ether esters, etc.
[0077] Furthermore, the matrix resin composition of the present invention may include one or more components such as hydrophobic polymers, inorganic fillers, and additives in addition to the above-mentioned hydrophilic polymers in order to improve chemical resistance, stability, and mechanical strength.
[0078] The hydrophobic polymer may be selected from a combination of one or more of fluorine-containing or fluorine-free saturated polyolefins and fusible polymers. In some preferred embodiments, the fluorine-containing saturated polyolefin includes polyvinylidene fluoride or polytetrafluoroethylene, etc.; the fluorine-free saturated polyolefin includes polyethylene or polypropylene, etc.; the fusible polymer includes a fusible aromatic polymer or an aliphatic polymer, which may include fusible polyetheretherketone or polyetherimide, etc. The hydrophobic polymer is used to give the porous membrane of the present invention better chemical resistance and heat stability.
[0079] In addition, there is no particular limitation on the inorganic filler in principle, and various inorganic nano materials, such as nano silicon dioxide, nano titanium dioxide, nano aluminum oxide and nano carbon materials, can be used when necessary. The addition of inorganic nano materials can assist in pore formation and improve porosity. In addition, in the present invention, the use of inorganic nano materials can also effectively reduce the swelling rate of the membrane.
[0080] In addition, in a further preferred embodiment of the present invention, the resin composition may also contain an ionic liquid. Such an ionic liquid may act as a diluent to improve the ion conduction characteristics. For such an ionic liquid, from the perspective of solubility, the diluent may be selected from a combination of one or more of an imidazole ionic liquid, an ionic liquid containing a sulfonate structure, and an ionic liquid containing a phosphate structure. Preferably, the ionic liquid may be an imidazole ionic liquid. Ionic liquids have a strong affinity for protons and can effectively enhance the conductivity of protons, thereby improving the voltage efficiency of the flow battery.
[0081] Regarding the composition of the matrix resin composition for forming the porous membrane of the present invention, in some specific embodiments, based on the total mass of the composition:
[0082] The content of the hydrophilic polymer is 10 mass % or more, for example, 10 mass % to 50 mass %, preferably 20 mass % to 43 mass %, more preferably 22 mass % to 40 mass %, for example, 12 mass %, 16 mass %, 20 mass %, 24 mass %, 25 mass %, 28 mass %, 30 mass %, 32 mass %, 35 mass %, 38 mass %, etc.
[0083] The content of the hydrophobic polymer may be 80 mass % or less, preferably 45 mass % to 70 mass %, for example 35 mass %, 40 mass %, 44 mass %, 48 mass %, 52 mass %, 56 mass %, 60 mass %, 64 mass %, 68 mass %, 72 mass %, 76 mass %, etc.
[0084] The content of the inorganic filler may be 40 mass % or less, preferably 15 mass % to 30 mass %, for example 10 mass %, 12 mass %, 16 mass %, 20 mass %, 24 mass %, 28 mass %, 32 mass %, 36 mass %, etc.
[0085] The content of the ionic liquid may be 10% by mass or less, preferably 3% to 10% by mass, for example, 4%, 5%, 6%, 7%, 8%, 9% by mass, etc. When the content of the ionic liquid is 3% to 10% by mass of the total mass of the matrix resin, the conductivity of protons can be further effectively improved, thereby improving the voltage efficiency of the flow battery.
[0086] (pore modifier)
[0087] The present invention modifies the surface of the pore structure in the conductive film by using a pore modifier, introduces a polymer capable of transmitting anions and cations into the pore structure, and balances the selectivity while improving the ion conductivity.
[0088] For the above polymer, correspondingly, there are cationic functional groups and anionic functional groups for ion transport in its molecular structure. Considering the ion transport property, the cationic functional group can be selected from one or more of positively charged groups such as secondary amine groups, primary amine groups, tertiary amine groups and quaternary ammonium groups; the anionic functional group can be selected from one or more of negatively charged groups such as sulfonic acid groups and carboxyl groups. In some preferred embodiments of the present invention, the cationic functional group can be a quaternary amine group, and the anionic functional group can be a sulfonic acid group.
[0089] Furthermore, in principle, there is no particular limitation on the type of polymer having cationic and anionic functional groups. For example, it may be a polyurethane polymer, a polyolefin polymer, a polyacrylate polymer, a polyurethane polyacrylate polymer or a polyamide polymer, etc. Preferably, it may be a polyurethane polymer.
[0090] The pore modifier of the present invention is bonded to the inner wall of the pore structure of the porous membrane through a covalent bond. Therefore, in some preferred embodiments, the polymer structure having cationic functional groups and anionic functional groups contains an active terminal group structure that can react with a hydroxyl group, such as a hydroxyl group, a carboxyl group, an isocyanate group, etc. Preferably, it can be a hydroxyl group or an isocyanate group.
[0091] By controlling or adjusting the molecular weight of the pore modifier, the filling of the polymer in the pore structure can be regulated. At the same time, by controlling or adjusting the ratio of cationic functional groups to anionic functional groups in the pore modifier polymer, the ion transport properties can also be regulated.
[0092] In some specific embodiments of the present invention, the molecular weight of the pore modifier can be, for example, 10,000 to 50,000, such as 20,000, 25,000, 30,000, 35,000, 40,000, etc.; the molar ratio of the cationic functional group to the anionic functional group in the pore modifier polymer can be 1:1 to 1:5, for example, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, etc.
[0093] In addition, there is no particular limitation on the content of the pore modifier in principle, as long as the porosity of the final porous membrane specified in the present invention can be satisfied. In some specific embodiments, the content of the pore modifier is 3% to 10% by mass of the total mass of the final porous membrane, for example, 4%, 5%, 6%, 7%, 8%, 9% by mass, etc.
[0094] (Membrane properties of zwitterionic ion-conducting films)
[0095] The thickness of the zwitterionic conductive film is not particularly limited in the present invention and can be selected as needed, for example, 10 to 500 μm, preferably 20 to 200 μm, such as 30 μm, 50 μm, 80 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, etc.
[0096] The porosity of the zwitterion conductive film may be 30% to 75%, preferably 35% to 72%, for example, 35%, 40%, 42%, 47%, 50%, 52%, 55%, 58%, 60%, 63%, 65%, 68%, 71%, etc.
[0097] <Second Aspect>
[0098] In the second aspect of the present invention, a method for preparing a zwitterion conducting membrane is disclosed, in particular, the method for preparing the zwitterion conducting membrane described in the first aspect of the present invention.
[0099] The method mainly comprises the following steps:
[0100] The step of preparing the porous original membrane comprises mixing the raw materials for forming the matrix resin composition and obtaining the porous original membrane having a multi-porous structure through extrusion and coagulation bath treatment;
[0101] The step of modifying is to combine the porous original membrane with a multi-porous structure through a pore modifier to obtain the zwitterion conductive porous membrane of the present invention.
[0102] (Steps for preparing porous original membrane)
[0103] The preparation of the porous original membrane of the present invention mainly comprises extruding the mixed matrix resin composition into a membrane, and then curing the original membrane through treatment in a coagulation bath to form porous channels in the original membrane.
[0104] Extrusion film
[0105] In some specific embodiments, the extrusion film formation can be mainly carried out by melt extrusion and casting processing. For example, the resin composition raw material is meshed, melted, dissolved, degassed, etc. at high temperature through an extrusion casting device to obtain a resin solution, which is then cast into a film.
[0106] In principle, there is no particular limitation on the equipment used in the extrusion step, and conventional equipment in the art, such as a twin-screw or single-screw extruder, can be used.
[0107] The present invention does not particularly limit the temperature of the extruded drooling, and can be selected as needed. In some specific embodiments, the temperature of the extruded drooling is 150-350°C, for example, 170°C, 180°C, 190°C, 200°C, 250°C, 300°C, 330°C, etc.
[0108] Coagulation bath treatment
[0109] After the saliva is extruded, the obtained cast film is subjected to a physical coagulation treatment. In this treatment step, the cast film is immersed in a coagulation bath for physical coagulation treatment to obtain a porous original film with an initial microporous structure (pore structure).
[0110] In principle, there is no particular limitation on the coagulation bath. In some specific embodiments, the composition of the coagulation bath may be an aqueous solution of an ionic liquid. Typically, the concentration of the ionic liquid in the coagulation bath may be 30% to 70% by mass, for example, 35%, 40%, 45%, 50%, 55%, 60%, or 65% by mass. The range of optional types of the ionic liquid may be the same as the ionic liquid mentioned in the first aspect above.
[0111] In the coagulation bath treatment process, in addition to coagulating the salivating film, the ionic liquid in the salivating film also enters the coagulation bath at a certain diffusion rate, thereby forming an initial microporous structure in the film. In addition, there is no particular restriction on the temperature of the coagulation bath, preferably, it can be between 20 and 50° C.; there is no particular restriction on the temperature of the coagulation bath treatment, preferably, it can be 1 to 5 minutes.
[0112] (First post-processing)
[0113] After the coagulation bath treatment, in some preferred embodiments of the present invention, a first post-treatment may be performed, wherein the first post-treatment comprises water washing and a first heat treatment.
[0114] The water washing treatment includes washing the porous original membrane obtained from the coagulation bath with water to wash and replace the excess ionic liquid to obtain a wet membrane. In addition, there is no particular limitation on the water washing temperature, preferably, it can be 30-60°C; there is no particular limitation on the water washing time, preferably, it can be 5-10 minutes.
[0115] The first heat treatment step comprises heat treating the washed wet film at a certain temperature to obtain a dry porous original film. In some specific embodiments, the moisture content in the porous original film may be 0.5% by mass or less. In addition, there is no particular limitation on the temperature of the first heat treatment, and preferably, it may be 100-150°C.
[0116] In addition, optionally, after the heat treatment, the porous original membrane may be subjected to uniaxial or biaxial stretching treatment as required to obtain enhanced mechanical properties or appropriate porosity.
[0117] For the above-mentioned porous original membrane of the present invention, in some specific embodiments, the porosity can be 60~80%.
[0118] (Steps for pore modification)
[0119] The modification step of the present invention mainly comprises combining the porous membrane having a multi-porous structure with a pore modifier to obtain the zwitterion conductive porous membrane of the present invention.
[0120] In principle, there is no particular limitation on the method of combining. In some specific embodiments, the pore modifier can be infiltrated into the pore structure of the porous original membrane, and further chemically reacted to allow the pore modifier to be covalently bonded to the inside of the pore structure (Method 1). In other specific embodiments, the pore modifier precursor (such as a prepolymer) and the coupling agent / curing agent can be simultaneously infiltrated into the pore structure, and chemical reactions are carried out to complete the formation of the modifier and the covalent bonding of the modifier to the inside of the pore (Method 2).
[0121] From the perspective of processing convenience, the method 2 is preferred. Specifically, the prepolymer can be infiltrated into the pore structure by coating and impregnation. The prepolymer is further subjected to a secondary polymerization reaction in the pore structure, and the polymer with zwitterionic conductivity is fixed to the surface of the inner wall of the pore while forming the polymer to complete the modification.
[0122] In addition, the molecular weight of the prepolymer may be 1000 to 10000, for example, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, etc., in view of processability.
[0123] In some preferred embodiments, before the pore modifier dipping treatment is performed, the above-mentioned coupling agent or curing agent can be first given to the inside of the pore structure. Such a process can also be achieved by coating or dipping. Afterwards, the above-mentioned prepolymer entering the pore structure completes the secondary polymerization reaction under the action of the coupling agent or curing agent.
[0124] In a further preferred embodiment of the present invention, the prepolymer may be a polyol prepolymer having a cationic functional group and an anionic functional group in its molecular structure, such as a polyurethane polyol prepolymer, etc. In addition, the coupling agent or curing agent may be a polyisocyanate compound having an isocyanate group, such as diphenylmethane diisocyanate (MDI), etc.
[0125] (Second post-processing)
[0126] After the pore modification, the porous membrane after pore modification can be subjected to a second post-treatment, optionally. In some specific embodiments, the second post-treatment comprises a second heat treatment, winding and aging treatment.
[0127] The second heat treatment includes heat treating the pore-modified porous membrane at a certain temperature to obtain a dry membrane, and can also further improve the formation of the pore modifier and the combination with the inner wall of the pore, so as to further control the pore size and porosity. There is no particular limitation on the temperature of the second heat treatment, and it can preferably be 50-100°C; there is no particular limitation on the time of the second heat treatment, and it can preferably be 10-20 minutes.
[0128] The winding includes winding the dry film.
[0129] The aging treatment includes storing and aging the rolled dry film at a certain temperature for a certain period of time to obtain a zwitterionic conductive film with a final microporous structure. In some specific embodiments, the aging temperature is 50-100°C, for example, 60°C, 70°C, 80°C, 90°C, etc.; the aging time is 5-15h, for example, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, etc.
[0130] A typical preparation method of the present invention comprises the following steps:
[0131] (1) Mixing
[0132] A quantitative amount of hydrophobic polymer, hydrophilic polymer, ionic liquid, inorganic nano powder and thermal stabilizer are added into a mixer, and uniform mixing is completed after a certain temperature and time.
[0133] (2) Squeeze out drool
[0134] The mixed materials are quantitatively conveyed to a twin-screw or single-screw extruder through a feeder. The uniform resin solution is conveyed to a T-die head through meshing, melting, dissolving and exhausting at high temperature to flow onto a flat and smooth stainless steel belt for cooling and leveling. The end of the steel belt enters a coagulation bath for natural peeling of the wet film.
[0135] (3) Coagulation bath treatment
[0136] The peeled wet film is immersed in an ionic liquid aqueous solution containing a certain concentration and temperature for coagulation. The ionic liquid in the resin solution enters the coagulation bath at a certain diffusion rate to form an initial microporous morphology.
[0137] (4) Washing
[0138] After multiple water washings under certain conditions, the ionic liquid is cleaned and replaced to ensure that the residual amount is 3% to 10% by weight of the dry weight of the membrane, and most of the volume of the ionic liquid in the resin solution is occupied by water.
[0139] (5) Primary drying
[0140] The wet film after washing is dried under certain temperature conditions, and the moisture content is controlled to be less than 0.5%, thereby obtaining a film with a porous structure. At this time, it is an intermediate process microporous morphology, and the porosity is between 60% and 80%.
[0141] (6) Modification by modifier
[0142] The film after once drying is first dipped in a solution containing a certain concentration of coupling agent / curing agent, and connected by the reaction of the curing agent with the hydrophilic polymer containing multiple hydroxy groups in the membrane; then it is immersed in a prepolymer solution with zwitterionic conductive groups, and the prepolymer then reacts with the coupling agent / curing agent to form a pore-modifying polymer, and at the same time, the pore-modifying polymer is firmly bonded to the inner wall of the membrane pore.
[0143] (7) Secondary drying and winding
[0144] The film obtained above is subjected to secondary drying at a certain temperature and time, and then the dry film is rolled up.
[0145] (8) Post-ripening treatment
[0146] The rolled-up film is stored and aged at a certain temperature for a period of time to obtain a zwitterion conductive porous film with a final microporous morphology.
[0147] <Third Aspect>
[0148] The present invention further provides a battery device, which comprises the above-mentioned zwitterionic ion conductive film.
[0149] The battery device is preferably a liquid flow battery device. Such liquid flow batteries include all-vanadium liquid flow batteries, iron-chromium liquid flow batteries, zinc-bromine liquid flow batteries, zinc-iron liquid flow batteries, all-iron liquid flow batteries, etc. Preferably, the battery device of the present invention is an all-vanadium liquid flow battery device.
[0150] Example
[0151] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0152] Example 1
[0153] 100 g of vinylidene fluoride, 100 g of pulp, 50 g of fumed silica, 2.5 g of calcium stearate, and 747.5 g of imidazole-type ionic liquid were added to a mixer, the temperature was set to 50° C., and the mixture was stirred and mixed for 2 h. Afterwards, the uniformly mixed materials were conveyed to a feeder.
[0154] The feeder is turned on to quantitatively convey the material to the twin-screw extruder. The upper temperature limit of each zone of the twin-screw extruder is set to 260°C. The quantitative extrusion speed is set to stably extrude to the T-die head, and the thickness difference between the webs is adjusted. The wet film is evenly sprayed onto the steel belt and then enters the coagulation bath for coagulation.
[0155] The concentration of the coagulation bath ionic liquid aqueous solution was set to 40%, the coagulation bath temperature was set to 30°C, and the wet film residence time was set to 3 min according to the vehicle speed.
[0156] After exiting the coagulation bath, the film enters the water washing zone, the water washing temperature is 40°C, and the wet film residence time is 8 minutes. The residual amount of ionic liquid is tested to be 5%.
[0157] After washing, it enters the drying area. The drying temperature is set at 105°C. After drying, the moisture content is 0.2% and the porosity is 69.5%.
[0158] After primary drying, it enters the curing agent dipping area. The curing agent is mixed with MDI DMF solution in a certain amount, where the curing agent concentration is 5%, the dipping temperature is 30°C, and the residence time is set to 2 minutes.
[0159] The wet film after the curing agent is dipped into a waterborne polyurethane prepolymer, wherein the molecular weight of the waterborne polyurethane prepolymer is 3000, and the molar ratio of the sulfonic acid group, the quaternary ammonium group and the hydroxyl group is 3:3:1. The concentration of the waterborne polyurethane DMF solution is 30%, and the residence time is set to 5 minutes.
[0160] The secondary drying temperature was set at 80°C and the drying time was set at 15 minutes. After that, the film after secondary drying was rolled up and the rolled sample was placed in an environment of 80°C for aging for 6 hours to obtain a porous amphoteric ion conductive film with a final morphology. The porosity of the film was tested to be 65%, and the thickness of the ion conductive film was 50 μm.
[0161] Example 2
[0162] 150 g of vinylidene fluoride, 50 g of pulp, 100 g of fumed silica, 3 g of calcium stearate, and 697 g of imidazole-type ionic liquid were added to a mixer, the temperature was set to 60° C., and the mixture was stirred and mixed for 2 h. Afterwards, the uniformly mixed materials were conveyed to a feeder.
[0163] The feeder is turned on to quantitatively convey the material to the twin-screw extruder. The upper temperature limit of each zone of the twin-screw extruder is set to 250°C. The quantitative extrusion speed is set to stably extrude to the T-die head, and the thickness difference between the webs is adjusted. The wet film is evenly sprayed onto the steel belt and then enters the coagulation bath for coagulation.
[0164] The concentration of the coagulation bath ionic liquid aqueous solution was set to 50%, the coagulation bath temperature was set to 30°C, and the wet film residence time was set to 3 min according to the vehicle speed.
[0165] After exiting the coagulation bath, the film enters the water washing zone, the water washing temperature is 50°C, and the wet film residence time is 8 minutes. The residual amount of ionic liquid is 3% after testing.
[0166] After washing, it enters the drying area. The drying temperature is set at 110℃. After drying, the moisture content is 0.1% and the porosity is 65.5%.
[0167] After primary drying, it enters the curing agent dipping area. The curing agent is mixed with MDI DMF solution in a certain ratio, where the curing agent concentration is 7%, the dipping temperature is 30°C, and the residence time is set to 2 minutes.
[0168] The wet film after the curing agent is dipped into a waterborne polyurethane prepolymer, wherein the molecular weight of the waterborne polyurethane prepolymer is 5000, wherein the molar ratio of the sulfonic acid group, the quaternary ammonium group and the hydroxyl group is 3:1:1. The concentration of the waterborne polyurethane DMF solution is 30%, and the residence time is set to 5 minutes.
[0169] The secondary drying temperature was set at 85°C and the drying time was set at 15 minutes. After that, the film after secondary drying was rolled up and the rolled sample was placed in an environment of 85°C for aging for 6 hours to obtain a porous zwitterionic conductive film with the final morphology. The film was tested to have a porosity of 62%.
[0170] The thickness of the obtained ion conductive membrane was 75 μm.
[0171] Example 3
[0172] 150 g polyethylene, 100 g pulp, 50 g fumed silica, 3 g calcium stearate, and 697 g imidazole ionic liquid were added to a mixer, the temperature was set to 60° C., and the mixture was stirred and mixed for 2 h. Afterwards, the uniformly mixed materials were conveyed to a feeder.
[0173] The feeder is turned on to quantitatively convey the material to the twin-screw extruder. The upper temperature limit of each zone of the twin-screw extruder is set to 240°C. The quantitative extrusion speed is set to stably extrude to the T-die head, and the thickness difference between the webs is adjusted. The wet film is evenly sprayed onto the steel belt and then enters the coagulation bath for coagulation.
[0174] The concentration of the coagulation bath ionic liquid aqueous solution was set to 35%, the coagulation bath temperature was set to 30°C, and the wet film residence time was set to 3 min according to the vehicle speed.
[0175] After exiting the coagulation bath, the film enters the water washing zone, the water washing temperature is 50°C, and the wet film residence time is 8 minutes. The residual amount of ionic liquid is tested to be 3.2%.
[0176] After washing, it enters the drying area. The drying temperature is set at 110℃. After drying, the moisture content is 0.1% and the porosity is 66%.
[0177] After primary drying, it enters the curing agent dipping area. The curing agent is mixed with MDI DMF solution in a certain amount, where the curing agent concentration is 5%, the dipping temperature is 30°C, and the residence time is set to 2 minutes.
[0178] The wet film after the curing agent is dipped into a waterborne polyurethane prepolymer, wherein the molecular weight of the waterborne polyurethane prepolymer is 5000, wherein the molar ratio of the sulfonic acid group, the quaternary ammonium group and the hydroxyl group is 3:1:1. The concentration of the waterborne polyurethane DMF solution is 35%, and the residence time is set to 5 minutes.
[0179] The secondary drying temperature was set at 85°C and the drying time was set at 15 minutes. After that, the film after secondary drying was rolled up and the rolled sample was placed in an environment of 85°C for aging for 6 hours to obtain a porous amphoteric ion conductive film with a final morphology. The porosity of the film was tested to be 62.5%, and the thickness of the ion conductive membrane was 100 μm.
[0180] Example 4
[0181] 100 g of polyethylene, 50 g of polyvinyl alcohol copolymer, 50 g of fumed silica, 2 g of calcium stearate, and 798 g of imidazole-type ionic liquid were added to a mixer, the temperature was set to 60° C., and the mixture was stirred and mixed for 2 h. Afterwards, the uniformly mixed materials were conveyed to a feeder.
[0182] The feeder is turned on to quantitatively convey the material to the twin-screw extruder. The upper temperature limit of each zone of the twin-screw extruder is set to 235°C. The quantitative extrusion speed is set to stably extrude to the T-die head, and the thickness difference between the webs is adjusted. The wet film is evenly sprayed onto the steel belt and then enters the coagulation bath for coagulation.
[0183] The concentration of the coagulation bath ionic liquid aqueous solution was set to 35%, the coagulation bath temperature was set to 30°C, and the wet film residence time was set to 3 min according to the vehicle speed.
[0184] After exiting the coagulation bath, the film enters the water washing zone, the water washing temperature is 50°C, and the wet film residence time is 8 minutes. The residual amount of ionic liquid is tested to be 3.2%.
[0185] After washing, it enters the drying area. The drying temperature is set at 105°C. After drying, the moisture content is 0.1% and the porosity is 75.5%.
[0186] After primary drying, it enters the curing agent dipping area. The curing agent is mixed with MDI DMF solution in a certain amount, where the curing agent concentration is 5%, the dipping temperature is 30°C, and the residence time is set to 2 minutes.
[0187] The wet film after the curing agent is dipped into a waterborne polyurethane prepolymer, wherein the molecular weight of the waterborne polyurethane prepolymer is 10000, wherein the molar ratio of the sulfonic acid group, the quaternary ammonium group and the hydroxyl group is 5:1:1. The concentration of the waterborne polyurethane DMF solution is 35%, and the residence time is set to 5 minutes.
[0188] The secondary drying temperature was set at 80°C and the drying time was set at 15 minutes. After that, the film after secondary drying was rolled up and the rolled sample was placed in an environment of 80°C for aging for 12 hours to obtain a porous amphoteric ion conductive film with a final morphology. The porosity of the film was tested to be 70%, and the thickness of the ion conductive film was 200 μm.
[0189] Example 5
[0190] 200 g of polyetheretherketone, 50 g of pulp, 50 g of fumed silica, 3 g of calcium stearate, and 697 g of sulfonic acid ionic liquid were added to a mixer, the temperature was set to 60° C., and the mixture was stirred and mixed for 2 h. Afterwards, the uniformly mixed materials were conveyed to a feeder.
[0191] The feeder is turned on to quantitatively convey the material to the twin-screw extruder. The upper temperature limit of each zone of the twin-screw extruder is set to 350°C. The quantitative extrusion speed is set to stably extrude to the T-die head, and the thickness difference between the webs is adjusted. The wet film is evenly sprayed onto the steel belt and then enters the coagulation bath for coagulation.
[0192] The concentration of the coagulation bath ionic liquid aqueous solution was set to 35%, the coagulation bath temperature was set to 30°C, and the wet film residence time was set to 3 min according to the vehicle speed.
[0193] After exiting the coagulation bath, the film enters the water washing zone, the water washing temperature is 50°C, and the wet film residence time is 8 minutes. The residual amount of ionic liquid is tested to be 3.2%.
[0194] After washing, it enters the drying area. The drying temperature is set at 105°C. After drying, the moisture content is 0.1% and the porosity is 66.2%.
[0195] After primary drying, it enters the curing agent dipping area. The curing agent is mixed with MDI DMF solution in a certain amount, where the curing agent concentration is 5%, the dipping temperature is 30°C, and the residence time is set to 2 minutes.
[0196] The wet film after the curing agent is dipped into a waterborne polyurethane prepolymer, wherein the molecular weight of the waterborne polyurethane prepolymer is 10000, wherein the molar ratio of the sulfonic acid group, the quaternary ammonium group and the hydroxyl group is 5:1:1. The concentration of the waterborne polyurethane DMF solution is 35%, and the residence time is set to 5 minutes.
[0197] The secondary drying temperature was set at 80°C and the drying time was set at 15 minutes. After that, the film after secondary drying was rolled up and the rolled sample was placed in an environment of 80°C for aging for 12 hours to obtain a porous amphoteric ion conductive film with the final morphology. The porosity of the film was tested to be 60%, and the thickness of the ion conductive membrane was 150 μm.
[0198] Comparative Example 1
[0199] The currently commercially available perfluorosulfonic acid proton exchange membrane (DuPont Nafion NR-212) was used as comparative example 1, and its performance index data are shown in Table 2.
[0200] Comparative Example 2
[0201] The method is basically the same as Example 1, except that the curing agent is not dipped, but directly immersed in the polyurethane prepolymer.
[0202] Comparative Example 3:
[0203] It is basically the same as Example 1, except that the hydrophilic polymer cellulose pulp is not used.
[0204] Reference example:
[0205] It is basically the same as Example 1, except that the residual amount of the ionic liquid is less than 0.1%, close to 0.
[0206] Comparative Example 4:
[0207] It is basically the same as Example 1, except that no heating and aging treatment is performed, so the connection reaction between the pore modifier and the inner wall of the micropore is not sufficient.
[0208] Performance Testing
[0209] According to the energy industry standard NB / T42080-2016, the performance index of the ion conductive membrane prepared in Examples 1 to 5, Comparative Examples 2 to 4 and Reference Example was tested, wherein the test conditions for the charge and discharge performance were an ambient temperature of 30°C and a current density of 80 mA / cm 2 The test results are shown in Tables 1 and 2.
[0210] Table 1 Performance data of Examples 1 to 5 and Reference Examples
[0211]
[0212] Table 2 Performance data of comparative examples 1 to 4
[0213]
[0214] From the above test results, it can be seen that the ion conductive membranes prepared in Examples 1 to 5 have excellent performance. This type of ion conductive membrane has a good balance between ion conductivity and barrier properties, and its comprehensive performance is significantly better than the currently used perfluorosulfonic acid proton exchange membrane and various situations of the comparative examples, and is suitable for large-scale use in liquid flow batteries. Among them, the reference example also shows that the use or residue of ionic liquids also has a certain promoting effect on the conductivity and energy efficiency of the present invention.
[0215] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.
[0216] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A zwitterionic conductive film, characterized in that: It is a porous membrane with a pore structure. The porous membrane is formed from a matrix resin composition, and a pore modifier exists in the pore structure; Wherein, the matrix resin composition comprises a hydrophilic polymer, a hydrophobic polymer and an inorganic filler; The pore modifier includes a polymer having a cationic functional group and an anionic functional group, and the pore modifier is bonded to the inner wall of the pore structure through a covalent bond; the pore modifier is derived from a waterborne polyurethane compound; The porosity of the zwitterionic conductive film is 30% to 75%. The hydrophilic polymer can provide a pore modifier for bonding with the inner wall of the pore structure by providing a hydrophilic group, wherein the hydrophilic group is one or more of a hydroxyl group, an amino group, and a thiol group. The content of the pore modifier is 3% to 10% by mass of the mass of the zwitterion conductive film.
2. The zwitterion conductive film according to claim 1, characterized in that: The base resin composition further contains an ionic liquid.
3. The zwitterion conductive film according to claim 1 or 2, characterized in that: In the matrix resin composition, the content of the hydrophilic polymer is 10% to 50% by mass.
4. The zwitterion conductive film according to claim 1 or 2, characterized in that: The hydrophilic polymer includes one or more combinations of cellulose and its derivatives, wherein the derivative is selected from cellulose ether, cellulose ester or cellulose ether ester.
5. The zwitterion conductive film according to claim 1 or 2, characterized in that: The anionic functional group in the pore modifier includes a sulfonic acid group; and the cationic functional group in the pore modifier includes a quaternary ammonium group.
6. The zwitterion conductive film according to claim 1 or 2, characterized in that: The molar ratio of the cationic functional group to the anionic functional group in the pore modifier is 1:1 to 1:
5.
7. The zwitterion conductive film according to claim 1 or 2, characterized in that: The thickness of the zwitterionic ion conductive film is 10 μm-500 μm.
8. A method for preparing a zwitterionic conductive film according to any one of claims 1 to 7, characterized in that: The following steps are involved: The step of preparing the porous original membrane comprises mixing the raw materials for forming the matrix resin composition and obtaining the porous original membrane having a multi-porous structure through extrusion and coagulation bath treatment; The step of modifying is to combine the porous original membrane with a multi-pore structure with a pore modifier.
9. The method according to claim 8, characterized in that In the step of preparing the porous original membrane, the coagulation bath is an aqueous solution containing an ionic liquid.
10. The method according to claim 8 or 9, characterized in that: In the modification step, the pore modifier is covalently linked to the inner wall of the pore structure by in-situ polymerization in the pore structure.
11. A battery device, characterized in that: The battery device comprises the zwitterion conductive film according to any one of claims 1 to 7 or the zwitterion conductive film prepared by the method according to any one of claims 8 to 10.