Modified high-strength flame-retardant cable protection material and preparation method

Through the combination of surface-modified magnesium hydroxide whiskers and boron nitride microtube-coated flame retardants, the problem of insufficient strength and flame retardant properties of high-strength flame-retardant cable materials is solved, and excellent mechanical and flame retardant properties are achieved. Improved to ensure safety and stability in extreme environments.

CN118420996BActive Publication Date: 2024-10-18JIANGSU TONGSHANG NEW MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410463763.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-10-18
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

Existing high-strength flame-retardant cable materials have deficiencies in strength and flame-retardant properties, making it difficult to meet the needs of special working conditions. Moreover, the large amount of hydroxide added to traditional flame-retardant materials leads to a decrease in mechanical properties, low flame-retardant efficiency, and cannot effectively prevent The fire spreads.

Method used

Surface-modified magnesium hydroxide whiskers and boron nitride micron tubes are used to coat the flame retardant. Magnesium hydroxide is modified by silane coupling agent and polycarbosilane to form a fibrous structure and dense protective film to improve mechanics and flame retardancy. performance, and improves mechanical strength and wear resistance through boron nitride microtubes.

Benefits of technology

Significantly improve the mechanical properties and flame retardant properties of flame retardant materials, provide higher tensile strength, wear resistance and flame retardant efficiency, can effectively resist the spread of flames in extreme environments, ensuring the long-term stability and safety of the material .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118420996B_ABST
    Figure CN118420996B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of cable materials, and provides a modified high-strength flame-retardant cable protection material and a preparation method. The modified high-strength flame-retardant cable protection material includes the following raw materials in parts by weight: 20 to 45 parts of surface-modified magnesium hydroxide whiskers, 25 to 45 parts of boron nitride microtube-coated flame retardants, 10 to 35 parts of high-density polyethylene, 15 to 30 parts of polyethylene-vinyl acetate, 15 to 35 parts of acrylonitrile-butadiene-styrene copolymers, 2 to 5 parts of antioxidants, 1 to 4 parts of lubricants, and 2 to 6 parts of sodium dodecyl sulfonate. The surface-modified magnesium hydroxide whiskers significantly improve the mechanical properties and flame retardant properties of the flame retardant material; it can improve the flame retardant efficiency of the flame retardant material, reduce the release of smoke and toxic gases, and enhance the mechanical properties and durability of the material. The flame retardant material of the present invention has excellent mechanical properties and flame retardant properties, and has a wide range of application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of cable materials, and in particular to a modified high-strength flame-retardant cable protective material and a preparation method thereof. Background Art

[0002] As the demand for electricity and communications in modern society continues to rise, the importance of cables as a core component of energy transmission and information transmission is self-evident. However, traditional cables often suffer from safety hazards such as damage, short circuits, and even fires when facing harsh environments such as high temperature, chemical corrosion, and external force impact. In order to improve the safety and reliability of cables, the market demand for high-strength flame-retardant cables is becoming increasingly urgent. This type of cable can not only maintain structural integrity in extreme environments and effectively prevent the spread of fire, but also provide long-lasting and stable power and communication transmission. Its excellent tensile strength, wear resistance, and impact resistance enable it to easily cope with a variety of harsh conditions such as high temperature, high pressure, and chemical corrosion. For this reason, high-strength flame-retardant cables have been widely used in industries such as construction, transportation, and petrochemicals, providing a strong guarantee for ensuring the safety of power supply and communication transmission.

[0003] Although high-strength flame-retardant cables have broad application prospects, they still face some challenges. First, traditional high-strength flame-retardant cables are still insufficient in strength and are difficult to meet the needs of some special working conditions. At present, flame-retardant materials mainly achieve flame-retardant effects by adding hydroxides (such as magnesium hydroxide) to the substrate, but this method has problems such as large hydroxide dosage and low flame-retardant efficiency, and can only meet general flame-retardant requirements. In addition, the agglomeration phenomenon between hydroxide particles also affects its uniform dispersion in the material, thereby adversely affecting the flame-retardant and mechanical properties of the material. For example, although the Chinese patent with publication number CN109810404A discloses a method of using hydroxide as a flame retardant, the amount of hydroxide added is large, which may lead to a decrease in the mechanical properties of the material. Secondly, the current high-strength flame-retardant cables still need to be improved in terms of flame-retardant effects, especially in extreme environments, the cables may not be able to effectively prevent the spread of fire, posing a potential threat to people's lives and property safety. Therefore, in order to meet the growing market demand, researchers are committed to improving the performance of high-strength flame-retardant cables and exploring new materials and preparation methods in order to achieve breakthroughs in improving the tensile strength and flame-retardant properties of cables. At present, cable materials still face many challenges in terms of strength and flame retardancy. It is necessary to develop a new type of flame retardant material with both high strength and flame retardancy to meet the demand for high-performance flame retardant materials and provide strong guarantees for the safe development of the power and communications industries. Summary of the invention

[0004] (1) Technical problems solved

[0005] The purpose of the present invention is to provide a modified high-strength flame-retardant cable protective material and a preparation method thereof, so as to solve the problem that the current flame-retardant materials are insufficient in strength and flame-retardant performance.

[0006] (2) Technical solution

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] A modified high-strength flame-retardant cable protection material and a preparation method thereof, comprising the following raw materials in parts by weight: 20 to 45 parts of surface-modified magnesium hydroxide whiskers, 25 to 45 parts of boron nitride microtube-coated flame retardant, 10 to 35 parts of high-density polyethylene, 15 to 30 parts of polyethylene-vinyl acetate, 15 to 35 parts of acrylonitrile-butadiene-styrene copolymer, 2 to 5 parts of antioxidant, 1 to 4 parts of lubricant, and 2 to 6 parts of sodium dodecyl sulfonate.

[0009] Furthermore, the preparation method of the surface modified magnesium hydroxide whisker is as follows: by weight, 20 to 50 parts of magnesium hydroxide whisker, 3 to 6 parts of hydrated iron oxide, 5 to 15 parts of silane coupling agent, 3 to 9 parts of polycarbosilane and 60 to 100 parts of ethanol are added to a reaction kettle, then heated to 50 to 80° C., stirred for reaction for 2 to 4 hours, and then filtered and dried to obtain the surface modified magnesium hydroxide whisker.

[0010] Preferably, the silane coupling agent is 3-aminopropyltriethoxysilane or octyltriethoxysilane.

[0011] Preferably, the preparation method of the magnesium hydroxide whisker is as follows: by weight, 20 to 40 parts of magnesium chloride, 10 to 25 parts of sodium hydroxide and 40 to 70 parts of a 1:1 mixed solution of ethanol and water are added to a high-temperature and high-pressure reactor, heated to 150 to 200° C. and kept warm for 10 to 15 hours, cooled, immersed, washed and dried to obtain the magnesium hydroxide whisker.

[0012] The present invention uses magnesium hydroxide to prepare whiskers for the following purposes. First, compared with traditional granular magnesium hydroxide flame retardant materials, magnesium hydroxide whiskers exhibit excellent mechanical reinforcement effects in flame retardant materials due to their unique fibrous structure and large specific surface area. The fibrous structure of the whiskers can form a three-dimensional network inside the material, greatly enhancing the strength and toughness of the material. Its high specific surface area not only provides more reaction interfaces, but also enhances the adhesion between the substrate and the substrate, thereby further improving the mechanical properties of the overall material. Secondly, in terms of flame retardant properties, the addition of magnesium hydroxide whiskers has brought significant improvements in flame retardant effects. The magnesium oxide component in the whiskers has excellent flame retardant properties. When exposed to flames, it can quickly undergo thermal decomposition reactions, release a large amount of water vapor and inert gases, and effectively inhibit flame combustion. Its fibrous structure not only increases the contact area with the flame, but also improves the flame retardant efficiency, making the material more effective in resisting the spread of flames. It is worth mentioning that magnesium hydroxide whiskers also have excellent thermal stability and can maintain the stability of their structure and performance under high temperature environments. The magnesium oxide in the whiskers has a high melting point and good thermal stability, and is not easy to melt and decompose at high temperatures, thereby ensuring its flame retardant effect and durability of mechanical properties under extreme conditions. In summary, the present invention adopts the design of magnesium hydroxide whiskers, which significantly improves the mechanical properties and flame retardant properties of flame retardant materials. Its unique fibrous structure and high specific surface area enhance the mechanical strength of the material, while the magnesium oxide in the whiskers provides efficient flame retardant function. In addition, its excellent thermal stability enables the modified flame retardant material to maintain excellent performance under high temperature conditions. Therefore, the present invention uses magnesium hydroxide whiskers to improve the flame retardant and mechanical properties of flame retardant materials, and is suitable for various fields with strict requirements on flame retardant properties.

[0013] As a concept of the present invention, the modification of magnesium hydroxide whiskers by using silane coupling agents and polycarbosilane has the following multiple purposes: first, chemical reaction and formation of chemical bonds: the organic functional groups in the silane coupling agent and polycarbosilane react chemically with the active hydroxyl groups on the surface of magnesium hydroxide to form chemical bonds. This chemical bonding not only enhances the interaction between the magnesium hydroxide particles, but also forms a dense protective film on its surface. The presence of this protective film can effectively prevent the magnesium hydroxide particles from breaking or decomposing when subjected to external stress or environmental factors, thereby improving its mechanical properties and stability. Secondly, the improvement of interfacial affinity: the introduction of silane coupling agents and polycarbosilane significantly improves the interfacial affinity between magnesium hydroxide and the substrate. This is because the organic functional groups in the silane coupling agent and polycarbosilane can form a stronger bond with the substrate surface, enhancing the adhesion of the interface. This enhanced interfacial affinity not only helps to reduce the interfacial peeling and fracture between the fireproof layer and the substrate, but also improves the adhesion of the fireproof layer on the substrate, thereby enhancing the overall stability and durability. Finally, the improvement of flame retardant mechanism: The introduction of silane coupling agent and polycarbosilane improves the flame retardant properties of the fireproof layer through multiple mechanisms. First, they can form a dense protective film on the surface of magnesium hydroxide particles to prevent the entry of external oxygen, thereby reducing the combustion reaction of the flame. Secondly, the protective film can reduce the thermal radiation transfer of the flame and effectively inhibit the spread and diffusion of the flame. In addition, silane coupling agent and polycarbosilane also have self-extinguishing properties, which can quickly form a non-combustible isolation layer in the flame, thereby inhibiting the continued burning of the flame and significantly improving the flame retardant properties of the fireproof layer. In summary, the modification of magnesium hydroxide whiskers by silane coupling agent and polycarbosilane can play an important role in chemical reaction, improvement of interface affinity and improvement of flame retardant mechanism, and significantly improve the mechanical properties and flame retardant properties of magnesium hydroxide materials. This provides a broader prospect for the application of magnesium hydroxide in the field of fire protection.

[0014] Furthermore, the preparation method of the boron nitride microtube coated flame retardant is as follows: in parts by weight, 15 to 45 parts of magnesium nitrate, 10 to 30 parts of sodium hydroxide and 4 to 8 parts of triglycerides are mixed evenly, and then 3 to 8 parts of zinc borate and 10 to 20 parts of boron nitride microtubes are added, stirred evenly, and then added into a high-temperature reactor, heated to 150 to 200° C. and reacted for 4 to 8 hours to obtain a boron nitride microtube coated flame retardant.

[0015] Preferably, the mass ratio of the magnesium hydroxide to the sodium hydroxide is 1.5:1.

[0016] Furthermore, the preparation method of the boron nitride microtube is as follows: by weight, 20 to 50 parts of cotton are heated to 600 to 800° C. in an Ar atmosphere and calcined for 3 to 6 hours to obtain micron carbon tubes, and then 20 to 40 parts of micron carbon tubes, 10 to 20 parts of boric acid, 10 to 20 parts of urea and 30 to 50 parts of deionized water are stirred and mixed evenly, filtered and placed in a high-temperature tubular furnace, in a nitrogen atmosphere, at 600 to 900° C. for 2 to 4 hours to obtain boron nitride-coated micron carbon tubes, and then calcined at 500 to 600° C. in an air atmosphere for 2 to 4 hours to remove the micron carbon tubes to obtain boron nitride microtubes.

[0017] The present invention adopts boron nitride microtubes to coat the flame retardant mainly for the following purposes: From a mechanical point of view, to enhance mechanical strength: boron nitride microtubes have excellent mechanical properties, including high modulus and high strength, and can effectively increase the mechanical strength of the flame retardant. When the material is subjected to external force, the boron nitride microtubes can withstand and disperse part of the stress, reduce the breakage and deformation of the flame retardant, thereby improving the overall strength and durability of the material. Secondly, to improve wear resistance: the hardness of the boron nitride microtubes is relatively high, which can effectively improve the wear resistance of the flame retardant. During the use of the material, the boron nitride microtubes can reduce the wear on the surface of the flame retardant, extend the service life of the flame retardant, and improve the material's resistance to damage to the external environment. Improve processing performance: boron nitride microtubes can be used as a dispersant and play the role of an auxiliary agent in the preparation process of the flame retardant. It can improve the dispersibility of the flame retardant, making it easier to disperse evenly in the matrix, thereby improving the processing efficiency and product quality of the flame retardant. From the perspective of flame retardant performance: First, improve flame retardant efficiency: Boron nitride microtubes have excellent thermal stability and chemical stability, and can maintain structural stability under high temperature and flame environment. When the flame retardant is subjected to flame, the boron nitride microtubes can effectively isolate oxygen and heat, reduce the combustion of the flame retardant, thereby improving the flame retardant efficiency and reducing the occurrence of fire accidents. Reduce the release of smoke and toxic gases: During the combustion process, the boron nitride microtubes can absorb part of the heat and reduce the combustion temperature of the flame retardant, thereby reducing the release of smoke and toxic gases. This is of great significance for improving the safety and environmental protection of flame retardant materials, protecting personnel from the hazards of smoke and toxic gases. Enhance the durability of flame retardants: Boron nitride microtubes have high thermal stability and can maintain good flame retardant properties after multiple combustions. This enhances the durability of flame retardants, giving them better long-term performance in practical applications and reducing the frequency and cost of replacement and maintenance. In summary, the main purpose of using boron nitride microtubes to coat the flame retardant in the present invention is to improve the comprehensive performance of the material from the perspectives of mechanics and flame retardancy. This innovative design concept provides a new direction and possibility for the development of flame retardant materials.

[0018] Furthermore, the antioxidant is pentaerythritol tetrakis-(dibutylhydroxyhydrocinnamate), tris(2,4-di-tert-butylphenyl) phosphite or diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate].

[0019] Furthermore, the lubricant is zinc stearate or magnesium stearate.

[0020] The present invention also provides a method for preparing a modified high-strength flame-retardant cable protective material:

[0021] According to the ratio, the surface modified magnesium hydroxide whisker and boron nitride microtube coated flame retardant, lubricant and sodium dodecyl sulfonate are added to a high-speed mixer and mixed for 10 to 30 minutes; then, high-density polyethylene, polyethylene-vinyl acetate, acrylonitrile-butadiene-styrene copolymer and antioxidant are added and mixed evenly, and then transferred from the high-speed mixer to a mixer for mixing, and the mixing temperature is 125 to 155°C and the time is 15 to 30 minutes. After the mixing is completed, the material is transferred to a feeder and extruded using a twin-screw extruder at a temperature of 110 to 130°C to obtain a modified high-strength flame-retardant cable protective material.

[0022] (3) Beneficial technical effects

[0023] The invention adopts magnesium hydroxide whiskers for modification, which significantly improves the mechanical properties and flame retardant properties of the flame retardant material. The fibrous structure and high specific surface area of ​​the whiskers enhance the mechanical strength of the material. The magnesium oxide component provides efficient flame retardant function. The introduction of silane coupling agent and polycarbosilane improves the interface affinity and flame retardant mechanism. Boron nitride microtubes are coated with flame retardants to improve the mechanical properties and flame retardant properties of the material. Boron nitride microtubes have high mechanical strength and wear resistance, which can increase the strength and durability of the flame retardant. At the same time, it can also improve the processing performance of the flame retardant and improve the flame retardant efficiency, reduce the release of smoke and toxic gases, and enhance the durability of the flame retardant. High-density polyethylene is used as a matrix material to provide the overall strength and durability of the material. It has good chemical stability and wear resistance, and can increase the damage resistance of the material. Polyethylene-vinyl acetate is used as a plasticizer to improve the flexibility and processing performance of the material. It can increase the ductility and plasticity of the material, improve the processing efficiency of the material and product quality. Acrylonitrile-butadiene-styrene copolymer, as an elastic agent, can improve the toughness and impact resistance of the material. It can increase the toughness and tensile strength of the material and improve the impact resistance of the material. Antioxidants can prevent the material from undergoing oxidation reactions when exposed to air for a long time, thereby extending the service life of the material. It can inhibit the aging and degradation of the material and maintain the stability of the material's performance. Lubricants can reduce the friction coefficient of the material, reduce the wear and deformation of the material, improve the wear resistance and service life of the material, and also improve the processing performance of the material. Sodium dodecyl sulfate, as a dispersant, can improve the dispersibility of the flame retardant. It can make it easier for the flame retardant to be evenly dispersed in the matrix, thereby improving the processing efficiency and product quality of the flame retardant. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM morphology image of the magnesium hydroxide whisker prepared in Example 1 of the present invention.

[0025] Figure 2 This is the XRD phase analysis spectrum of the magnesium hydroxide whisker prepared in Example 1 of the present invention.

[0026] Figure 3 This is a SEM morphology image of the boron nitride microtube prepared in Example 1 of the present invention.

[0027] Figure 4 This is a SEM morphology of the boron nitride microtube coated with flame retardant prepared in Example 1 of the present invention.

[0028] Figure 5 This is the XRD phase analysis spectrum of the boron nitride microtube coated flame retardant prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] To make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0030] In the case of not specifying specific conditions, the operation in the examples is carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not indicated, are all common products on the market. Parts not mentioned in the technical content of the present invention will be processed with reference to the prior art. Unless otherwise specified, the following examples and comparative examples will be tested in parallel and use the same processing steps and parameters.

[0031] The following table shows the reagents required for the examples and comparative examples and the corresponding purchasing companies.

[0032] Table 1 Reagents required for the examples and comparative examples and the corresponding purchasing companies

[0033]

[0034] Example 1

[0035] A modified high-strength flame-retardant cable protective material comprises the following raw materials in parts by weight: 20 parts of surface-modified magnesium hydroxide whiskers, 25 parts of boron nitride microtube-coated flame retardant, 10 parts of high-density polyethylene, 15 parts of polyethylene-vinyl acetate, 15 parts of acrylonitrile-butadiene-styrene copolymer, 2 parts of antioxidant, 1 part of lubricant and 2 parts of sodium dodecyl sulfonate.

[0036] The preparation method of the surface modified magnesium hydroxide whisker is as follows: by weight, 20 parts of magnesium hydroxide whisker, 3 parts of hydrated iron oxide, 5 parts of silane coupling agent, 3 parts of polycarbosilane and 60 parts of ethanol are added into a reaction kettle, and then heated to 50° C., stirred for reaction for 2 hours, and then filtered and dried to obtain the surface modified magnesium hydroxide whisker.

[0037] The above-mentioned silane coupling agent is 3-aminopropyltriethoxysilane.

[0038] The preparation method of the above-mentioned magnesium hydroxide whisker is as follows: by weight, 20 parts of magnesium chloride, 10 parts of sodium hydroxide and 40 parts of a 1:1 mixed solution of ethanol and water are added to a high-temperature and high-pressure reactor, heated to 150° C. and kept warm for 10 hours, and then cooled, immersed, washed and dried to obtain magnesium hydroxide whiskers.

[0039] The preparation method of the above-mentioned boron nitride microtube coated flame retardant is as follows: in parts by weight, 15 parts of magnesium nitrate, 10 parts of sodium hydroxide and 4 parts of triglycerides are mixed evenly, and then 3 parts of zinc borate and 10 parts of boron nitride microtubes are added and stirred evenly, and then added into a high-temperature reactor, heated to 150°C and reacted for 4 hours to obtain the boron nitride microtube coated flame retardant.

[0040] The preparation method of the above-mentioned boron nitride microtube is as follows: by weight fraction, 20 parts of cotton are heated to 600°C in an Ar atmosphere and calcined for 3 hours to obtain micron carbon tubes, and then 20 parts of micron carbon tubes, 10 parts of boric acid, 10 parts of urea and 30 parts of deionized water are stirred and mixed evenly, filtered and placed in a high-temperature tubular furnace, in a nitrogen atmosphere, at 600°C for 2 hours to obtain boron nitride-coated micron carbon tubes, and then calcined at 500°C in an air atmosphere for 2 hours to remove the micron carbon tubes to obtain boron nitride microtubes.

[0041] The antioxidant is pentaerythritol tetrakis-(dibutylhydroxyhydrocinnamate).

[0042] The lubricant mentioned above is zinc stearate.

[0043] The present invention also provides a method for preparing a modified high-strength flame-retardant cable protective material:

[0044] According to the ratio, the surface modified magnesium hydroxide whisker and boron nitride microtube coated flame retardant, lubricant and sodium dodecyl sulfonate are added to a high-speed mixer and mixed for 10 minutes; then, high-density polyethylene, polyethylene-vinyl acetate, acrylonitrile-butadiene-styrene copolymer and antioxidant are added and mixed evenly, and then transferred from the high-speed mixer to a mixer for mixing at a mixing temperature of 125°C and a time of 15 minutes. After the mixing is completed, the material is transferred to a feeder and extruded using a twin-screw extruder at a temperature of 110°C to obtain a modified high-strength flame-retardant cable protective material.

[0045] Example 2

[0046] A modified high-strength flame-retardant cable protective material comprises the following raw materials in parts by weight: 25 parts of surface-modified magnesium hydroxide whiskers, 30 parts of boron nitride microtube-coated flame retardant, 15 parts of high-density polyethylene, 20 parts of polyethylene-vinyl acetate, 20 parts of acrylonitrile-butadiene-styrene copolymer, 3 parts of antioxidant, 2 parts of lubricant, and 3 parts of sodium dodecyl sulfonate.

[0047] The preparation method of the surface modified magnesium hydroxide whisker is as follows: by weight, 30 parts of magnesium hydroxide whisker, 4 parts of hydrated iron oxide, 8 parts of silane coupling agent, 4 parts of polycarbosilane and 70 parts of ethanol are added into a reaction kettle, and then heated to 60° C., stirred for reaction for 3 hours, and then filtered and dried to obtain the surface modified magnesium hydroxide whisker.

[0048] The above-mentioned silane coupling agent is octyltriethoxysilane.

[0049] The preparation method of the above-mentioned magnesium hydroxide whisker is as follows: by weight, 30 parts of magnesium chloride, 20 parts of sodium hydroxide and 50 parts of a 1:1 mixed solution of ethanol and water are added to a high-temperature and high-pressure reactor, heated to 170° C. and kept warm for 12 hours, and then cooled, immersed, washed and dried to obtain magnesium hydroxide whiskers.

[0050] The preparation method of the above-mentioned boron nitride microtube coated flame retardant is as follows: in parts by weight, 30 parts of magnesium nitrate, 20 parts of sodium hydroxide and 5 parts of triglyceride are mixed evenly, and then 4 parts of zinc borate and 13 parts of boron nitride microtubes are added, stirred evenly, and then added into a high-temperature reactor, heated to 160°C and reacted for 5 hours to obtain the boron nitride microtube coated flame retardant.

[0051] The preparation method of the above-mentioned boron nitride microtube is as follows: by weight fraction, 30 parts of cotton are heated to 700°C in an Ar atmosphere and calcined for 4 hours to obtain micron carbon tubes, and then 30 parts of micron carbon tubes, 14 parts of boric acid, 15 parts of urea and 40 parts of deionized water are stirred and mixed evenly, filtered and placed in a high-temperature tubular furnace, in a nitrogen atmosphere, at 700°C for 3 hours to obtain boron nitride-coated micron carbon tubes, and then calcined at 550°C in an air atmosphere for 3 hours to remove the micron carbon tubes to obtain boron nitride microtubes.

[0052] The antioxidant is diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate].

[0053] The lubricant mentioned above is magnesium stearate.

[0054] The present invention also provides a method for preparing a modified high-strength flame-retardant cable protective material:

[0055] According to the ratio, the surface modified magnesium hydroxide whisker and boron nitride microtube coated flame retardant, lubricant and sodium dodecyl sulfonate are added to a high-speed mixer and mixed for 20 minutes; then, high-density polyethylene, polyethylene-vinyl acetate, acrylonitrile-butadiene-styrene copolymer and antioxidant are added and mixed evenly, and then transferred from the high-speed mixer to a mixer for mixing at a mixing temperature of 135°C and a time of 20 minutes. After the mixing is completed, the material is transferred to a feeder and extruded using a twin-screw extruder at a temperature of 120°C to obtain a modified high-strength flame-retardant cable protective material.

[0056] Example 3

[0057] A modified high-strength flame-retardant cable protective material comprises the following raw materials in parts by weight: 40 parts of surface-modified magnesium hydroxide whiskers, 40 parts of boron nitride microtube-coated flame retardant, 30 parts of high-density polyethylene, 25 parts of polyethylene-vinyl acetate, 30 parts of acrylonitrile-butadiene-styrene copolymer, 4 parts of antioxidant, 3 parts of lubricant and 5 parts of sodium dodecyl sulfonate.

[0058] The preparation method of the surface modified magnesium hydroxide whisker is as follows: by weight, 40 parts of magnesium hydroxide whisker, 5 parts of hydrated iron oxide, 12 parts of silane coupling agent, 8 parts of polycarbosilane and 90 parts of ethanol are added into a reaction kettle, and then heated to 70°C, stirred for reaction for 3 hours, and then filtered and dried to obtain the surface modified magnesium hydroxide whisker.

[0059] The above-mentioned silane coupling agent is octyltriethoxysilane.

[0060] The preparation method of the above-mentioned magnesium hydroxide whisker is as follows: by weight, 30 parts of magnesium chloride, 20 parts of sodium hydroxide and 60 parts of a 1:1 mixed solution of ethanol and water are added to a high-temperature and high-pressure reactor, heated to 180° C. and kept warm for 12 hours, and then cooled, immersed, washed and dried to obtain magnesium hydroxide whiskers.

[0061] The preparation method of the above-mentioned boron nitride microtube coated flame retardant is as follows: in parts by weight, 30 parts of magnesium nitrate, 20 parts of sodium hydroxide and 7 parts of triglycerides are stirred evenly, and then 6 parts of zinc borate and 16 parts of boron nitride microtubes are added and stirred evenly, and then added into a high-temperature reactor, heated to 1180°C and reacted for 6 hours to obtain the boron nitride microtube coated flame retardant.

[0062] The mass ratio of the above-mentioned magnesium hydroxide to sodium hydroxide is 1.5:1.

[0063] The preparation method of the above-mentioned boron nitride microtube is as follows: by weight fraction, 40 parts of cotton are heated to 700°C in an Ar atmosphere and calcined for 5 hours to obtain micron carbon tubes, and then 30 parts of micron carbon tubes, 16 parts of boric acid, 16 parts of urea and 40 parts of deionized water are stirred and mixed evenly, filtered and placed in a high-temperature tubular furnace, in a nitrogen atmosphere, at 800°C for 3 hours to obtain boron nitride-coated micron carbon tubes, and then calcined at 580°C in an air atmosphere for 3 hours to remove the micron carbon tubes to obtain boron nitride microtubes.

[0064] The antioxidant is diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate].

[0065] The lubricant mentioned above is magnesium stearate.

[0066] The present invention also provides a method for preparing a modified high-strength flame-retardant cable protective material:

[0067] According to the ratio, the surface modified magnesium hydroxide whisker and boron nitride microtube coated flame retardant, lubricant and sodium dodecyl sulfonate are added to a high-speed mixer and mixed for 20 minutes; then, high-density polyethylene, polyethylene-vinyl acetate, acrylonitrile-butadiene-styrene copolymer and antioxidant are added and mixed evenly, and then transferred from the high-speed mixer to a mixer for mixing at a mixing temperature of 145°C and a time of 25 minutes. After the mixing is completed, the material is transferred to a feeder and extruded using a twin-screw extruder at a temperature of 120°C to obtain a modified high-strength flame-retardant cable protective material.

[0068] Example 4

[0069] A modified high-strength flame-retardant cable protective material comprises the following raw materials in parts by weight: 45 parts of surface-modified magnesium hydroxide whiskers, 45 parts of boron nitride microtube coated flame retardant, 35 parts of high-density polyethylene, 30 parts of polyethylene-vinyl acetate, 35 parts of acrylonitrile-butadiene-styrene copolymer, 5 parts of antioxidant, 4 parts of lubricant and 6 parts of sodium dodecyl sulfonate.

[0070] The preparation method of the surface modified magnesium hydroxide whisker is as follows: by weight, 50 parts of magnesium hydroxide whisker, 6 parts of hydrated iron oxide, 15 parts of silane coupling agent, 9 parts of polycarbosilane and 100 parts of ethanol are added into a reaction kettle, and then heated to 80°C, stirred for reaction for 4 hours, and then filtered and dried to obtain the surface modified magnesium hydroxide whisker.

[0071] The above-mentioned silane coupling agent is octyltriethoxysilane.

[0072] The preparation method of the above-mentioned magnesium hydroxide whisker is as follows: by weight, 40 parts of magnesium chloride, 25 parts of sodium hydroxide and 70 parts of a 1:1 mixed solution of ethanol and water are added to a high-temperature and high-pressure reactor, heated to 200° C. and kept warm for 15 hours, and then cooled, immersed, washed and dried to obtain magnesium hydroxide whiskers.

[0073] The preparation method of the above-mentioned boron nitride microtube coated flame retardant is as follows: in parts by weight, 45 parts of magnesium nitrate, 30 parts of sodium hydroxide and 8 parts of triglycerides are mixed evenly, and then 8 parts of zinc borate and 20 parts of boron nitride microtubes are added, stirred evenly, and then added into a high-temperature reactor, heated to 200°C and reacted for 8 hours to obtain the boron nitride microtube coated flame retardant.

[0074] The preparation method of the above-mentioned boron nitride microtube is as follows: by weight fraction, 50 parts of cotton are heated to 800°C in an Ar atmosphere and calcined for 6 hours to obtain micron carbon tubes, and then 40 parts of micron carbon tubes, 20 parts of boric acid, 20 parts of urea and 50 parts of deionized water are stirred and mixed evenly, filtered and placed in a high-temperature tubular furnace, in a nitrogen atmosphere, at 900°C for 4 hours to obtain boron nitride-coated micron carbon tubes, and then calcined at 600°C in an air atmosphere for 4 hours to remove the micron carbon tubes to obtain boron nitride microtubes.

[0075] The antioxidant is diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate].

[0076] The lubricant mentioned above is magnesium stearate.

[0077] The present invention also provides a method for preparing a modified high-strength flame-retardant cable protective material:

[0078] According to the ratio, the surface modified magnesium hydroxide whisker and boron nitride microtube coated flame retardant, lubricant and sodium dodecyl sulfonate are added to a high-speed mixer and mixed for 30 minutes; then, high-density polyethylene, polyethylene-vinyl acetate, acrylonitrile-butadiene-styrene copolymer and antioxidant are added and mixed evenly, and then transferred from the high-speed mixer to a mixer for mixing at a mixing temperature of 155°C for 30 minutes. After the mixing is completed, the material is transferred to a feeder and extruded using a twin-screw extruder at a temperature of 130°C to obtain a modified high-strength flame-retardant cable protective material.

[0079] Comparative Example 1

[0080] The method is substantially the same as Example 1, except that an equal amount of magnesium hydroxide powder is used to replace the magnesium hydroxide whisker.

[0081] Comparative Example 2

[0082] The method is basically the same as Example 1, except that the surface of the magnesium hydroxide whisker is not subjected to surface modification treatment.

[0083] Comparative Example 3

[0084] It is basically the same as Example 1, except that the boron nitride microtubes and the flame retardant are not in a coating relationship, but are added separately.

[0085] Characterization Tests:

[0086] X-ray diffraction (XRD) is a very effective method for characterizing the phase information of flame retardants. In the XRD experiment, the X-ray diffraction pattern of the flame retardant sample is first collected. By comparing the diffraction pattern obtained in the experiment with the standard diffraction pattern in the database, the type of phase present in the flame retardant can be determined. Scanning electron microscopy (SEM) is a commonly used method for observing and analyzing the morphological characteristics of flame retardants. In the SEM experiment, the flame retardant sample is placed on the sample stage of the SEM, and the sample surface is scanned using a high-energy electron beam. By detecting the electron signal reflected from the sample surface, a morphological image of the sample can be generated. SEM images have the characteristics of high resolution and high magnification, and detailed features such as the shape, size, and distribution of flame retardant particles can be observed. In addition, the distribution and composition information of elements in flame retardants can also be obtained through energy spectrum analysis technology. SEM can help understand the morphology, surface morphology, and interactions between flame retardant particles, thereby revealing the flame retardant mechanism and performance optimization methods. Figure 1 This is a SEM morphology image of the magnesium hydroxide whisker prepared in Example 1 of the present invention. It can be seen that the magnesium hydroxide whisker has a higher aspect ratio. Figure 2 The XRD phase analysis spectrum of the magnesium hydroxide whisker prepared in Example 1 of the present invention shows the presence of a single magnesium hydroxide phase. Figure 3 This is a SEM morphology image of the boron nitride microtube prepared in Example 1 of the present invention, and the hollow structure of the boron nitride microtube can be seen. Figure 4 This is a SEM morphology image of the flame retardant coated with boron nitride microtubes prepared in Example 1 of the present invention, in which the flame retardant coated with the microtubes can be seen. Figure 5 The XRD phase analysis spectrum of the boron nitride microtube coated flame retardant prepared in Example 1 of the present invention shows that the phases of the coated flame retardant are magnesium hydroxide and zinc borate flame retardant.

[0087] Performance Test:

[0088] The hardness test is carried out according to GB / T531.1, and the sample is measured using a hardness tester. This standard specifies the method and requirements for hardness testing. By measuring the hardness value of the sample, its hardness characteristics can be evaluated.

[0089] The tensile strength and elongation at break test is carried out according to GB / T2951.12 and is tested using a tensile testing machine. The sample is subjected to tensile loading under standard specimen size, and the strength and elongation of the sample during the tensile process can be measured. This test can evaluate the mechanical properties and ductility of the sample.

[0090] The low temperature bending performance test is carried out according to GB / T2951.14 and is carried out under the condition of (-40±2°C)×30h. By placing the sample in a low temperature environment and then performing a bending test, the bending performance and cold brittleness resistance of the sample in a low temperature environment can be evaluated. This test can determine the reliability and application range of the material in a low temperature environment.

[0091] The thermal shock resistance test is carried out according to GB / T2951.31 and is carried out under the condition of (150±1°C)×3h. By placing the sample in a high temperature environment and then performing an impact test, the heat resistance and impact resistance of the sample in a high temperature environment can be evaluated. This test can determine the reliability and scope of use of the material in a high temperature environment.

[0092] The flame retardant performance test is carried out according to the UL94 fire test. The flame retardant performance of the sample can be evaluated by placing the sample in a flame and observing its combustion performance. This test can determine the safety and fire resistance of the material in the event of a fire.

[0093] The heat deformation test is carried out according to the UL1581 standard at 150°C. By placing the sample in a high temperature environment and then conducting a heat deformation test, the deformation performance and stability of the sample under high temperature can be evaluated. This test can determine the reliability and scope of use of the material under high temperature environment.

[0094] Resistivity: The reference value of volume resistivity at 20°C can be tested according to GB / T1410-2006.

[0095] The mechanical properties, flame retardant properties, resistivity and other properties of the flame retardant materials of Examples 1 to 4 and Comparative Examples 1 to 3 are summarized in Table 2.

[0096] Table 2 Performance parameters of flame retardant materials

[0097]

[0098] The main difference between Example 1 and Comparative Example 1 is the morphological characteristics of magnesium hydroxide. From Table 2, it can be seen that magnesium hydroxide whiskers can significantly improve the mechanical properties and flame retardant properties of flame retardant materials, and the resistivity is less affected.

[0099] In Example 1 and Comparative Example 2, whether the magnesium hydroxide whisker is subjected to surface modification treatment or not, it can be seen from Table 2 that the surface treatment of the magnesium hydroxide whisker can significantly improve the mechanical properties and flame retardant properties of the flame retardant material, and has little effect on the resistivity.

[0100] The main difference between Example 1 and Comparative Example 3 is whether the flame retardant adopts a coated structure. From Table 2, it can be seen that the flame retardant and the boron nitride microtube coating structure can significantly improve the mechanical properties and flame retardant properties of the flame retardant material, and the resistivity is less affected.

[0101] In summary, the surface-modified magnesium hydroxide whiskers and boron nitride microtube-coated flame-retardant materials in the present invention achieve a synergistic effect, can significantly improve mechanical properties and flame-retardant properties, and can provide excellent performance and effects in multiple fields.

[0102] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that all equivalent structural changes made under the concept of the present invention and using the contents of the present invention specification and drawings should be covered within the scope of protection of the claims of the present invention.

Claims

1. A modified high-strength flame-retardant cable protective material, comprising the following raw materials in parts by weight: 20-45 parts of surface modified magnesium hydroxide whisker, 25-45 parts of boron nitride microtube coated flame retardant, 10-35 parts of high-density polyethylene, 15-30 parts of polyethylene-vinyl acetate, 15-35 parts of acrylonitrile-butadiene-styrene copolymer, 2-5 parts of antioxidant, 1-4 parts of lubricant, 2-6 parts of sodium dodecyl sulfonate; The preparation method of the surface-modified magnesium hydroxide whisker is as follows: by weight, 20-50 parts of magnesium hydroxide whisker, 3-6 parts of hydrated iron oxide, 5-15 parts of silane coupling agent, 3-9 parts of polycarbosilane and 60-100 parts of ethanol are added into a reaction kettle, and then heated to 50-80° C., stirred for reaction for 2-4 hours, and then filtered and dried to obtain the surface-modified magnesium hydroxide whisker; The preparation method of the boron nitride microtube coated flame retardant is as follows: by weight, 15 to 45 parts of magnesium nitrate, 10 to 30 parts of sodium hydroxide and 4 to 8 parts of triglyceride are mixed evenly, and then 3 to 8 parts of zinc borate and 10 to 20 parts of boron nitride microtubes are added, stirred evenly, and then added into a high-temperature reactor, heated to 150 to 200° C. and reacted for 4 to 8 hours to obtain the boron nitride microtube coated flame retardant.

2. A modified high-strength flame-retardant cable protective material as claimed in claim 1, characterized in that: The silane coupling agent is 3-aminopropyltriethoxysilane or octyltriethoxysilane.

3. A modified high-strength flame-retardant cable protective material as claimed in claim 1, characterized in that: The preparation method of the magnesium hydroxide whisker is as follows: by weight, 20-40 parts of magnesium chloride, 10-25 parts of sodium hydroxide and 40-70 parts of a mixed solution of ethanol and water in a ratio of 1:1 are added into a high-temperature and high-pressure reactor, heated to 150-200° C. and kept warm for 10-15 hours, cooled and then allowed to stand, washed and dried to obtain the magnesium hydroxide whisker.

4. A modified high-strength flame-retardant cable protective material as claimed in claim 1, characterized in that: The mass ratio of the magnesium hydroxide to the sodium hydroxide is 1.5:

1.

5. The modified high-strength flame-retardant cable protective material according to claim 1, characterized in that: The preparation method of the boron nitride microtube is as follows: by weight, 20 to 50 parts of cotton are heated to 600 to 800° C. in an Ar atmosphere, calcined and kept warm for 3 to 6 hours to obtain micron carbon tubes, and then 20 to 40 parts of micron carbon tubes, 10 to 20 parts of boric acid, 10 to 20 parts of urea and 30 to 50 parts of deionized water are stirred and mixed evenly, and then filtered and placed in a high-temperature tubular furnace, and kept warm at 600 to 900° C. for 2 to 4 hours in a nitrogen atmosphere to obtain boron nitride-coated micron carbon tubes, and then calcined at 500 to 600° C. in an air atmosphere for 2 to 4 hours to remove the micron carbon tubes to obtain boron nitride microtubes.

6. A modified high-strength flame-retardant cable protective material as claimed in claim 1, characterized in that: The antioxidant is tetrakis-(dibutylhydroxyhydrocinnamic acid) pentaerythritol ester, tris(2,4-di-tert-butylphenyl) phosphite or diethylene thiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate].

7. A modified high-strength flame-retardant cable protective material as claimed in claim 1, characterized in that: The lubricant is zinc stearate or magnesium stearate.

8. The method for preparing the modified high-strength flame-retardant cable protective material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Add surface modified magnesium hydroxide whiskers and boron nitride microtube coated flame retardant, lubricant and sodium dodecyl sulfate into a high-speed mixer and mix for 10-30 minutes; then, continue to add high-density polyethylene, polyethylene-vinyl acetate, acrylonitrile-butadiene-styrene copolymer and antioxidant, mix well and then transfer from the high-speed mixer to an internal mixer for internal mixing at a temperature of 125-155°C for 15-30 minutes. After the internal mixing is completed, transfer the material to a feeder and extrude it using a twin-screw extruder at a temperature of 110-130°C to obtain a modified high-strength flame-retardant cable protective material.

Citation Information

Patent Citations

  • Polypropylene / metal hydroxide / rare earth compound flame retardant material

    CN109810404A

  • Polypropylene material modified by magnesium hydroxide crystal whiskers and preparation method of polypropylene material

    CN105330967A

  • Nuclear power cable insulating material of metal hydroxide-boron nitride hybridized filler / blended rubber and preparation method thereof