Weather-resistant adhesive for doors and windows and preparation method thereof

By preparing copolymer-coated zirconia hollow spheres in door and window weathering glue, using eugenol to form hydrogen bonds and ion bonds with polyurethane system, the problem of poor compatibility between hollow zirconia microspheres and organic resins is solved, and doors and windows are significantly improved The mechanical and thermal stability of weathering rubber enhances its weathering resistance.

CN118421253BActive Publication Date: 2024-11-01佛山巨马新材料有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410568134.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-11-01
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

The compatibility of hollow zirconium dioxide microspheres with organic resin is not ideal, resulting in agglomeration of door and window weathering glues during use, affecting their mechanical and thermal stability properties.

Method used

Using compound initiator and optimized reaction time, a copolymer-coated zirconia hollow sphere is prepared, and hydrogen bonds and ion bonds are formed with eugenol and polyurethane system to improve the dispersion and cross-linking density of zirconia hollow spheres to form a compact structure. Enhance the mechanical and thermal stability properties of weathering adhesives in doors and windows.

Benefits of technology

It significantly improves the tensile strength and thermal stability of door and window weathering glue, enhances its weathering resistance and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004830006690000021
    Figure BDA0004830006690000021
  • Figure BDA0004830006690000041
    Figure BDA0004830006690000041
  • Figure BDA0004830006690000051
    Figure BDA0004830006690000051
Patent Text Reader

Abstract

The present invention relates to a weather-resistant glue for doors and windows and a preparation method thereof, and belongs to the technical field of sealants. A weather-resistant glue for doors and windows includes components: a polyurethane prepolymer, a copolymer-coated hollow zirconia ball, a filler, a silane coupling agent, a plasticizer, a defoamer and a catalyst; the present invention adopts a compound initiator and optimizes the reaction time to prepare a copolymer-coated hollow zirconia ball, generate a compact structure, reduce the particle size, and improve the mechanical properties and thermal stability of the weather-resistant glue for doors and windows. The hydroxyl group of eugenol and the tertiary amine group of (N, N-dimethylamino) ethyl acrylate form hydrogen bonds and ionic bonds with the polyurethane system, improve the dispersibility of the hollow zirconia ball in the polyurethane, and enhance the thermal stability and mechanical properties. At the same time, the benzene ring and ether bond in eugenol increase the cross-linking density of the polyurethane, and further improve the tensile strength and thermal stability of the weather-resistant glue for doors and windows.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sealants and relates to a weather-resistant sealant for doors and windows and a preparation method thereof. Background Art

[0002] Weatherproof glue for doors and windows is a sealant specially designed for door and window installation. It must show excellent weather resistance to cope with the changing outdoor environment, such as exposure to sunlight, wind and rain, and other natural forces. Hollow ceramic microspheres, as a new type of lightweight industrial basic material, have the advantages of low density, low thermal conductivity, sound insulation, strong electrical insulation and high thermal stability due to their unique hollow structure. In the application of weatherproof glue for doors and windows, it shows excellent heat resistance.

[0003] Among the many hollow ceramic microspheres, hollow zirconium dioxide microspheres combine the low thermal conductivity, ablation resistance, and chemical corrosion resistance of hollow structural materials and zirconium dioxide, making them one of the preferred raw materials for manufacturing thermal insulation materials. The weather-resistant adhesive for doors and windows prepared using hollow zirconium dioxide microspheres not only has excellent thermal insulation and corrosion resistance, but also ensures the reliability and service life of the product. However, as an inorganic substance, hollow zirconium dioxide microspheres are not ideally compatible with organic resins and are prone to agglomeration. Summary of the invention

[0004] The object of the present invention is to provide a weather-resistant adhesive for doors and windows and a preparation method thereof. The present invention adopts a compound initiator and optimizes the reaction time to prepare a copolymer-coated zirconia hollow sphere, generate a compact structure, reduce the particle size, and improve the mechanical properties and thermal stability of the weather-resistant adhesive for doors and windows. The hydroxyl group of eugenol and the tertiary amine group of (N, N-dimethylamino) ethyl acrylate form hydrogen bonds and ionic bonds with the polyurethane system, improve the dispersibility of the zirconia hollow sphere in the polyurethane, and enhance the thermal stability and mechanical properties. At the same time, the benzene ring and ether bond in eugenol increase the crosslinking density of the polyurethane, further improving the tensile strength and thermal stability of the weather-resistant adhesive for doors and windows.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A weather-resistant adhesive for doors and windows, comprising the following components by weight:

[0007]

[0008] The preparation of the copolymer-coated zirconia hollow spheres comprises the following steps:

[0009] S1, adding pretreated zirconia hollow spheres and a coupling agent to anhydrous ethanol, then stirring to react, filtering, removing the filtrate, washing, and finally vacuum drying until constant weight, to obtain modified zirconia hollow spheres;

[0010] S2. After mixing the modified zirconia hollow spheres and the organic solvent, acrylate and initiator are added, and the mixture is heated and stirred under a nitrogen atmosphere. Then, eugenol is added and stirring is continued. After cooling to room temperature, the mixture is centrifuged and the solid is vacuum dried to a constant weight to obtain polymer-coated zirconia hollow spheres.

[0011] As a preferred technical solution of the present invention, in step S1, the pretreated zirconia hollow spheres are obtained by stirring and soaking the zirconia hollow spheres in a 30% by mass sodium hydroxide aqueous solution for 60 minutes, washing until the surface pH value is neutral, and drying.

[0012] As a preferred technical solution of the present invention, in step S1, the stirring reaction is carried out at 60-70°C and stirred for 6-8h; the washing is washed 3 times with anhydrous ethanol; the temperature of the vacuum drying is 70-80°C; the mass ratio of the pretreated zirconia hollow spheres, anhydrous ethanol and coupling agent is 4-6:80-90:15-18; the coupling agent is one or two of vinyltriethoxysilane and vinyltrimethoxysilane.

[0013] As a preferred technical solution of the present invention, in step S2, the heating and stirring temperature is 60-70°C; the continued stirring is at 70-80°C for 6-8h; and the vacuum drying temperature is 70-80°C.

[0014] As a preferred technical solution of the present invention, in step S2, the mass ratio of the modified zirconia hollow spheres, the organic solvent, the acrylate, the eugenol and the initiator is 14-16:60-65:26-30:2.5-3.0:1.5-1.8; the organic solvent is tetrahydrofuran; the acrylate is 3-(N,N-dimethylamino)ethyl acrylate; the initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, azoisobutylcyanamide, tert-butyl hydroperoxide, dibenzoyl peroxide and isopropylbenzene hydroperoxide; preferably, the initiator is a mixture of azobisisobutyronitrile and dibenzoyl peroxide in a mass ratio of 6:2-2.5.

[0015] As a preferred technical solution of the present invention, the polyurethane prepolymer is prepared by the following method: polyether diol and polyether triol are stirred and mixed at 80-90°C, vacuum dried, cooled to 40-50°C, and then isocyanate is added, and reacted at 70-80°C for 2-3h to obtain a polyurethane prepolymer.

[0016] As a preferred technical solution of the present invention, the polyether diol is one or more of polyether N210, polyether N220 and polyether N204; the polyether triol is one or two of polyether N330 and polyether 330N; the mass ratio of the isocyanate, the polyether diol and the polyether triol is 30-50:6-15:30-60; the isocyanate is one or both of MDI and TDI.

[0017] As a preferred technical solution of the present invention, MDI is diphenylmethane diisocyanate; TDI is toluene diisocyanate.

[0018] As a preferred technical solution of the present invention, the plasticizer is one or more of dioctyl phthalate, diisononyl phthalate, di-n-octyl phthalate and diisodecyl phthalate;

[0019] As a preferred technical solution of the present invention, the filler is one or more of heavy calcium carbonate, talc and zeolite; the silane coupling agent is one or more of KH-550 silane coupling agent, KH-560 silane coupling agent and KH-570 silane coupling agent;

[0020] As a preferred technical solution of the present invention, the catalyst is one or two of dibutyltin dilaurate, stannous octoate and dibutyltin diacetate; and the defoamer is BYK-141 organosilicon defoamer.

[0021] The invention discloses a method for preparing weather-resistant glue for doors and windows. The preparation method comprises the following steps: after stirring and mixing a filler and a silane coupling agent, adding a polyurethane prepolymer, a copolymer-coated zirconia hollow sphere, a plasticizer, a catalyst and a defoamer, heating and mixing at 50-70°C, and stirring for 4-5h to obtain the weather-resistant glue for doors and windows.

[0022] Beneficial effects of the present invention:

[0023] The invention compounds the initiator in the preparation of the copolymer-coated zirconia hollow spheres, combines the reaction time with the reaction, and makes the reaction proceed evenly and slowly. The generated copolymer can grow slowly to form a more compact coating structure, so that the particle size of the product is smaller, thereby improving the mechanical properties and thermal stability of the weather-resistant adhesive for doors and windows; the polar hydroxyl groups on eugenol and the tertiary amine groups on (N, N-dimethylamino) ethyl acrylate can interact with the components of the polyurethane system to form hydrogen bonds and ionic bonds, thereby significantly improving the dispersibility of the zirconia hollow spheres in the polyurethane system, thereby significantly improving the thermal stability and mechanical properties; in addition, the rigid and heat-resistant benzene ring structure and ether bond in eugenol can improve the crosslinking density of the polyurethane, thereby improving the tensile strength and thermal stability of the weather-resistant adhesive for doors and windows. DETAILED DESCRIPTION

[0024] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0025] Example 1

[0026] A weather-resistant adhesive for doors and windows, comprising the following components by weight:

[0027]

[0028]

[0029] Wherein, the plasticizer is dioctyl phthalate;

[0030] The filler is heavy calcium carbonate;

[0031] The silane coupling agent is KH-560 silane coupling agent;

[0032] The catalyst is dibutyltin dilaurate;

[0033] The defoamer is BYK-141 organosilicon defoamer.

[0034] The preparation of the copolymer-coated zirconia hollow spheres comprises the following steps:

[0035] S1. Add the pretreated zirconia hollow spheres and the coupling agent to anhydrous ethanol, then stir at 60° C. for 8 h, filter, remove the filtrate, wash with anhydrous ethanol for 3 times, and finally vacuum dry at 70° C. until constant weight, to obtain modified zirconia hollow spheres;

[0036] In step S1, the pretreated zirconia hollow spheres are obtained by stirring and soaking the zirconia hollow spheres in a 30% by mass sodium hydroxide aqueous solution for 60 minutes, washing until the surface pH value is neutral, and drying;

[0037] Wherein, the mass ratio of the pretreated zirconia hollow spheres, anhydrous ethanol and coupling agent is 4:80:15; the coupling agent is vinyl trimethoxy silane;

[0038] S2, after mixing the modified zirconia hollow spheres and the organic solvent, adding acrylate and initiator, heating and stirring at 60°C under a nitrogen atmosphere, adding eugenol and continuing stirring at 70°C for 8 hours, cooling to room temperature, centrifuging, taking the solid and vacuum drying it at 70°C to constant weight, to obtain polymer-coated zirconia hollow spheres;

[0039] In step S2, the mass ratio of the modified zirconia hollow spheres, the organic solvent, the acrylate, the eugenol and the initiator is 14:60:26:2.5:1.5; the organic solvent is tetrahydrofuran; the acrylate is 3-(N,N-dimethylamino)ethyl acrylate; wherein the initiator is a mixture of azobisisobutyronitrile and dibenzoyl peroxide in a mass ratio of 6:2;

[0040] The polyurethane prepolymer is prepared by the following method: polyether N210 and polyether N330 are stirred and mixed at 80°C, vacuum dried, cooled to 40°C, TDI is added, and reacted at 70°C for 3h to obtain the polyurethane prepolymer; wherein the mass ratio of the isocyanate, the polyether diol and the polyether triol is 30:6:30.

[0041] A method for preparing a weather-resistant adhesive for doors and windows comprises the following steps:

[0042] After the filler and the silane coupling agent are stirred and mixed, the polyurethane prepolymer, the copolymer-coated zirconia hollow spheres, the plasticizer, the catalyst and the defoamer are added, the mixture is heated and mixed at 50° C., and stirred for 5 hours to obtain the weather-resistant adhesive for doors and windows.

[0043] Example 2

[0044] A weather-resistant adhesive for doors and windows, comprising the following components by weight:

[0045]

[0046] Wherein, the plasticizer is dioctyl phthalate;

[0047] The filler is heavy calcium carbonate;

[0048] The silane coupling agent is KH-560 silane coupling agent;

[0049] The catalyst is dibutyltin dilaurate;

[0050] The defoamer is BYK-141 organosilicon defoamer.

[0051] The preparation of the copolymer-coated zirconia hollow spheres comprises the following steps:

[0052] S1. Add the pretreated zirconia hollow spheres and the coupling agent to anhydrous ethanol, then stir at 65° C. for 7 h, filter, remove the filtrate, wash with anhydrous ethanol for 3 times, and finally vacuum dry at 75° C. until constant weight, to obtain modified zirconia hollow spheres;

[0053] In step S1, the pretreated zirconia hollow spheres are obtained by stirring and soaking the zirconia hollow spheres in a 30% by mass sodium hydroxide aqueous solution for 60 minutes, washing until the surface pH value is neutral, and drying;

[0054] Wherein, the mass ratio of the pretreated zirconia hollow spheres, anhydrous ethanol and coupling agent is 5:85:16; the coupling agent is vinyl trimethoxy silane;

[0055] S2, after mixing the modified zirconia hollow spheres and the organic solvent, adding acrylate and initiator, heating and stirring at 65° C. under a nitrogen atmosphere, adding eugenol and continuing stirring at 75° C. for 7 h, cooling to room temperature, centrifuging, taking the solid and vacuum drying it at 75° C. to constant weight, to obtain polymer-coated zirconia hollow spheres;

[0056] In step S2, the mass ratio of the modified zirconia hollow spheres, the organic solvent, the acrylate, the eugenol and the initiator is 15:62:28:2.8:1.6; the organic solvent is tetrahydrofuran; the acrylate is 3-(N,N-dimethylamino)ethyl acrylate; wherein the initiator is a mixture of azobisisobutyronitrile and dibenzoyl peroxide in a mass ratio of 6:2.2;

[0057] The polyurethane prepolymer is prepared by the following method: polyether N210 and polyether N330 are stirred and mixed at 85°C, vacuum dried, cooled to 45°C, TDI is added, and reacted at 75°C for 2.5 hours to obtain the polyurethane prepolymer; wherein the mass ratio of the isocyanate, the polyether diol and the polyether triol is 40:10:45.

[0058] A method for preparing a weather-resistant adhesive for doors and windows comprises the following steps:

[0059] After the filler and the silane coupling agent are stirred and mixed, the polyurethane prepolymer, the copolymer-coated zirconia hollow spheres, the plasticizer, the catalyst and the defoamer are added, the mixture is heated and mixed at 60° C., and the mixture is stirred for 4.5 hours to obtain the weather-resistant adhesive for doors and windows.

[0060] Example 3

[0061] A weather-resistant adhesive for doors and windows, comprising the following components by weight:

[0062]

[0063]

[0064] Wherein, the plasticizer is dioctyl phthalate;

[0065] The filler is heavy calcium carbonate;

[0066] The silane coupling agent is KH-560 silane coupling agent;

[0067] The catalyst is dibutyltin dilaurate;

[0068] The defoamer is BYK-141 organosilicon defoamer.

[0069] The preparation of the copolymer-coated zirconia hollow spheres comprises the following steps:

[0070] S1. Add the pretreated zirconia hollow spheres and the coupling agent to anhydrous ethanol, then stir at 70° C. for 6 h, filter, remove the filtrate, wash with anhydrous ethanol for 3 times, and finally vacuum dry at 80° C. until constant weight, to obtain modified zirconia hollow spheres;

[0071] In step S1, the pretreated zirconia hollow spheres are obtained by stirring and soaking the zirconia hollow spheres in a 30% by mass sodium hydroxide aqueous solution for 60 minutes, washing until the surface pH value is neutral, and drying;

[0072] Wherein, the mass ratio of the pretreated zirconia hollow spheres, anhydrous ethanol and coupling agent is 6:90:18; the coupling agent is vinyl trimethoxy silane;

[0073] S2, after mixing the modified zirconia hollow spheres and the organic solvent, adding acrylate and initiator, heating and stirring at 70°C under a nitrogen atmosphere, adding eugenol and continuing stirring at 80°C for 6 hours, cooling to room temperature, centrifuging, taking the solid and vacuum drying it at 80°C to constant weight, to obtain polymer-coated zirconia hollow spheres;

[0074] In step S2, the mass ratio of the modified zirconia hollow spheres, the organic solvent, the acrylate, the eugenol and the initiator is 16:65:30:3.0:1.8; the organic solvent is tetrahydrofuran; the acrylate is 3-(N,N-dimethylamino)ethyl acrylate; wherein the initiator is a mixture of azobisisobutyronitrile and dibenzoyl peroxide in a mass ratio of 6:2.5;

[0075] The polyurethane prepolymer is prepared by the following method: polyether N210 and polyether N330 are stirred and mixed at 90°C, vacuum dried, cooled to 50°C, TDI is added, and reacted at 80°C for 2h to obtain the polyurethane prepolymer; wherein the mass ratio of the isocyanate, the polyether diol and the polyether triol is 50:15:60.

[0076] A method for preparing a weather-resistant adhesive for doors and windows comprises the following steps:

[0077] After the filler and the silane coupling agent are stirred and mixed, the polyurethane prepolymer, the copolymer-coated zirconia hollow spheres, the plasticizer, the catalyst and the defoamer are added, heated and mixed at 70° C., and stirred for 4 hours to obtain the weather-resistant glue for doors and windows.

[0078] Comparative Example 1

[0079] Compared with Example 2, the difference is that styrene replaces eugenol, and the other components, preparation steps and parameters are the same.

[0080] Comparative Example 2

[0081] Compared with Example 2, the difference is that ethyl acrylate replaces 3-(N,N-dimethylamino)ethyl acrylate, and the other components, preparation steps and parameters are the same.

[0082] Comparative Example 3

[0083] Compared with Example 2, the difference is that the mixture is used instead of the polymer to coat the zirconia hollow spheres;

[0084] S1. Add the pretreated zirconia hollow spheres and the coupling agent to anhydrous ethanol, then stir at 65° C. for 7 h, filter, remove the filtrate, wash with anhydrous ethanol for 3 times, and finally vacuum dry at 75° C. until constant weight, to obtain modified zirconia hollow spheres;

[0085] In step S1, the pretreated zirconia hollow spheres are obtained by stirring and soaking the zirconia hollow spheres in a 30% by mass sodium hydroxide aqueous solution for 60 minutes, washing until the surface pH value is neutral, and drying;

[0086] Wherein, the mass ratio of the pretreated zirconia hollow spheres, anhydrous ethanol and coupling agent is 5:85:16; the coupling agent is vinyl trimethoxy silane;

[0087] S2, adding acrylate and initiator to an organic solvent, heating and stirring at 65° C. under a nitrogen atmosphere, adding eugenol and continuing stirring at 75° C. for 7 h, cooling to room temperature, centrifuging, taking the solid and drying it at 75° C. in vacuum until constant weight, adding modified zirconia hollow balls, stirring and mixing, and obtaining a mixture;

[0088] In step S2, the mass ratio of the modified zirconia hollow spheres, the organic solvent, the acrylate, the eugenol and the initiator is 15:62:28:2.8:1.6; the organic solvent is tetrahydrofuran; the acrylate is 3-(N,N-dimethylamino)ethyl acrylate; wherein the initiator is a mixture of azobisisobutyronitrile and dibenzoyl peroxide in a mass ratio of 6:2.2;

[0089] The remaining components, preparation steps and parameters were the same.

[0090] Comparative Example 4

[0091] Compared with Example 2, the difference is that the initiator is dibenzoyl peroxide, and the other components, preparation steps and parameters are the same.

[0092] Comparative Example 5

[0093] Compared with Example 2, the difference is that the initiator is azobisisobutyronitrile, and the other components, preparation steps and parameters are the same.

[0094] Examples 1-3 and Comparative Examples 1-5 were tested as follows, and the test results are shown in Table 1.

[0095] Thermal conductivity test (22.5℃): Test according to GB3399-82; Sampling rules: Sampling at a location where a suitable test sample can be obtained, 3 samples, and the average value is taken. Test conditions: EKO flat plate mutual heat method, average temperature 22.5℃, cold plate set to 10℃, hot plate set to 35℃; 200mm×200mm×25mm standard sample, constant temperature and humidity indoor test (temperature is 25±2℃, humidity is 50±10%);

[0096] Tensile strength test: The sample was pressed into a dumbbell-shaped specimen by hot molding at 150°C and measured according to the GB / T13022-1991 method with a tensile rate of 50 mm / min.

[0097] Table 1

[0098]

[0099] From the test results in Table 1, it can be seen that compared with Comparative Examples 1-5, the weather-resistant adhesive for doors and windows prepared by the invention in Examples 1-3 is significantly better than Comparative Examples 1-5.

[0100] By comparing Examples 1-3 with Comparative Examples 1-5, combined with the analysis of Table 1, it can be seen that the present invention uses a compound initiator and optimizes the reaction time to prepare a copolymer-coated zirconia hollow sphere, form a compact structure, reduce the particle size, and improve the mechanical and thermal stability of the door and window weathering glue. The hydroxyl group of eugenol and the tertiary amine group of (N, N-dimethylamino) ethyl acrylate form hydrogen bonds and ionic bonds with the polyurethane system, enhancing the dispersibility, thermal stability and mechanical properties of the zirconia hollow sphere in the polyurethane. At the same time, the benzene ring and ether bond in eugenol increase the crosslinking density of the polyurethane, further improving the tensile strength and thermal stability of the door and window weathering glue.

[0101] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A weather-resistant adhesive for doors and windows, characterized in that: The components include the following by weight: The polyurethane prepolymer is prepared by the following method: mixing polyether diol and polyether triol at 80-90° C., vacuum drying, adding isocyanate after cooling to 40-50° C., and reacting at 70-80° C. for 2-3 hours to obtain the polyurethane prepolymer; The preparation of the copolymer-coated zirconia hollow spheres comprises the following steps: S1, adding pretreated zirconia hollow spheres and a coupling agent to anhydrous ethanol, then stirring to react, filtering, removing the filtrate, washing, and finally vacuum drying until constant weight, to obtain modified zirconia hollow spheres; S2. After mixing the modified zirconia hollow spheres and the organic solvent, add acrylate and an initiator, heat and stir under a nitrogen atmosphere, add eugenol and continue stirring, cool to room temperature, centrifuge, take the solid and vacuum dry it to constant weight to obtain polymer-coated zirconia hollow spheres; the acrylate is 3-(N,N-dimethylamino)ethyl acrylate; the initiator is composed of azobisisobutyronitrile and dibenzoyl peroxide.

2. The weather-resistant adhesive for doors and windows according to claim 1, characterized in that: In step S1, the pretreated zirconia hollow spheres are obtained by stirring and soaking the zirconia hollow spheres in a 30% by mass sodium hydroxide aqueous solution for 60 minutes, washing until the surface pH value is neutral, and drying; In step S1, the stirring reaction is carried out at 60-70°C and stirred for 6-8h; the washing is carried out 3 times with anhydrous ethanol; the temperature of the vacuum drying is 70-80°C; the mass ratio of the pretreated zirconia hollow spheres, anhydrous ethanol and coupling agent is 4-6:80-90:15-18; the coupling agent is one or both of vinyl triethoxy silane and vinyl trimethoxy silane.

3. The weather-resistant adhesive for doors and windows according to claim 1, characterized in that: In step S2, the heating and stirring temperature is 60-70°C; the continued stirring is at 70-80°C for 6-8h; the vacuum drying temperature is 70-80°C; In step S2, the mass ratio of the modified zirconia hollow spheres, the organic solvent, the acrylate, the eugenol and the initiator is 14-16: 60-65: 26-30: 2.5-3.0: 1.5-1.8; and the organic solvent is tetrahydrofuran.

4. The weather-resistant adhesive for doors and windows according to claim 1, characterized in that: In step S2, the initiator is prepared by mixing azobisisobutyronitrile and dibenzoyl peroxide in a mass ratio of 6:2-2.

5.

5. The weather-resistant adhesive for doors and windows according to claim 1, characterized in that: The polyether diol is one or more of polyether N210, polyether N220 and polyether N204; the polyether triol is one or two of polyether N330 and polyether 330N; the mass ratio of the isocyanate, the polyether diol and the polyether triol is 30-50:6-15:30-60; the isocyanate is one or two of MDI and TDI.

6. The weather-resistant adhesive for doors and windows according to claim 1, characterized in that: The plasticizer is one or more of dioctyl phthalate, diisononyl phthalate and diisodecyl phthalate.

7. The weather-resistant adhesive for doors and windows according to claim 1, characterized in that: The filler is one or more of heavy calcium carbonate, talcum powder and zeolite; the silane coupling agent is one or more of KH-550 silane coupling agent, KH-560 silane coupling agent and KH-570 silane coupling agent.

8. The weather-resistant adhesive for doors and windows according to claim 1, characterized in that: The catalyst is one or two of dibutyltin dilaurate, stannous octoate and dibutyltin diacetate.

9. A method for preparing the weather-resistant adhesive for doors and windows according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: after stirring and mixing the filler and the silane coupling agent, adding the polyurethane prepolymer, the copolymer-coated zirconia hollow spheres, the plasticizer, the catalyst and the defoamer, heating and mixing at 50-70° C., and stirring for 4-5 hours to obtain the weather-resistant glue for doors and windows.