A lithium ion adsorbent based on biochar and preparation method thereof

Through lithium-ion adsorbent based on biochar, lithium-aluminum hydroxide-carboxylated biochar composite material is prepared by using the impregnation, pyrolysis carbonization and conversion methods of NaAlO2 and NaOH, which solves the lithium-ion adsorption in brine The problems of poor results and difficulty in separation achieve efficient separation of lithium ions and calcium magnesium ions, reducing process complexity and cost.

CN118437288BActive Publication Date: 2024-11-15INST OF MINERAL RESOURCES CHINESE ACAD OF GEOLOGICAL SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410608626.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-11-15
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

In the prior art, the adsorption effect of lithium ions in brine is poor and lacks selectivity. The aluminum-based adsorbents used in industrial applications are complex and costly, so they cannot effectively separate lithium ions from calcium and magnesium ions.

Method used

Using lithium-ion adsorbent based on biochar, lithium-aluminum hydroxide-carboxylated biochar composite materials are prepared by impregnation, pyrolysis and conversion of NaAlO2 and NaOH, and their selection of lithium ions is used. The adsorption characteristics of calcium and magnesium ions can achieve the separation of lithium ions and calcium and magnesium ions.

Benefits of technology

The efficient adsorption of lithium ions in brine and the separation of calcium and magnesium ions is achieved, reducing process complexity and cost, and at the same time, the porous structure and active groups of biochar are used to improve the performance and application value of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118437288B_ABST
    Figure CN118437288B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of lithium ion enrichment and extraction in lithium-containing energy minerals, and in particular to an adsorption material for lithium ions in brine, specifically a lithium ion adsorbent based on biochar and a preparation method thereof. The present invention uses nut shells as raw materials, and adopts a combination of aluminum salt-alkali carbonization and chemical grafting to prepare a lithium ion adsorbent based on biochar, which provides a new idea for the development of biochar-based lithium ion adsorption materials, which is not only conducive to the extraction of lithium resources in brine, but also conducive to the effective utilization of biochar resources. The lithium ion adsorbent based on biochar prepared by the present invention can effectively separate lithium ions and calcium and magnesium ions in brine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion enrichment and extraction in lithium-containing energy minerals, and in particular to an adsorption material for lithium ions in brine, specifically a lithium ion adsorbent based on biochar and a preparation method thereof. Background Art

[0002] Lithium resources in brine are an important source of lithium in my country. With the rapid development of my country's new energy industry, research on materials and technologies related to lithium extraction from brine has become a hot spot and focus of lithium resource development.

[0003] At present, among the numerous lithium extraction technologies, adsorption has attracted much attention due to its advantages such as simple process flow, easy implementation and regenerable adsorbents. At present, the most studied adsorbents include ion sieve adsorbents, aluminum adsorbents and natural mineral adsorbents. All three types of adsorbent materials have a certain lithium ion adsorption capacity, but the main industrial application is aluminum adsorbents, which are characterized by environmentally friendly adsorption regeneration process and good lithium ion selectivity. The core of aluminum adsorbents is LiCl·2Al(OH) 3 ·nH 2 O or its derived lithium aluminum composite hydroxide. Currently, aluminum-based adsorbents are mostly synthesized by chemical precipitation, and the synthesized aluminum-based adsorbent materials are mostly powdery and often need to be formed before use. The process is relatively complicated and the cost needs to be reduced.

[0004] As a common adsorption material, biochar is widely used in the adsorption research of organic dyes and heavy metals. It has a porous structure, a large specific surface area and can be granulated. It can be used as a basis for the development of adsorption materials without secondary molding. Its surface contains a variety of active groups and has good functionalization potential. However, directly using it to adsorb lithium ions in brine often results in poor adsorption effect and no selectivity.

[0005] Therefore, it is necessary to develop a biochar-based granular lithium ion adsorption material by combining the respective characteristics and advantages of aluminum-based adsorbents and biochar, and use it for the separation of lithium ions in brine. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a biochar-based lithium ion adsorbent and a preparation method thereof. The method uses biochar as a raw material, and the prepared biochar-based lithium ion adsorbent can effectively separate lithium ions and calcium and magnesium ions in brine.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a lithium ion adsorbent based on biochar, the preparation method comprising the following steps:

[0008] (1) NaAlO2 and NaOH are added into distilled water to prepare a mixed solution, the crushed nut shells are placed in a beaker, the mixed solution is added, and after standing, the mixed solution is dried to constant weight to obtain the solid phase of step (1);

[0009] (2) placing the solid phase of step (1) in a crucible, reacting in a tube furnace, and then cooling to room temperature to obtain the solid phase of step (2);

[0010] (3) Dissolve LiCl and polybasic organic acid in water, add the solid phase of step (2), mix thoroughly and adjust the pH to 4-5, stir to react, dry to constant weight, continue to react, wash the solid phase after the reaction with NaOH solution and HCl solution, and dry to constant weight to obtain a biochar-based lithium ion adsorbent.

[0011] The various steps of the method are described below. In step (1), NaAlO 2 The nut particles are soaked in a mixed solution of NaOH to make NaAlO 2 and NaOH into the biomass structure, on the one hand for subsequent activation and pore formation, and on the other hand to introduce aluminum sources to facilitate the subsequent NaAlO 2 In step (2), the biomass is converted into biochar, and NaAlO 2 and NaOH into the biochar; in step (3), LiCl and polybasic organic acid are added and reacted at room temperature for a period of time at a certain pH, in order to convert NaAlO 2 It is converted into lithium aluminum hydroxide, and then the water is evaporated at 120°C and the reaction is continued for a period of time. The purpose is to allow the polybasic organic acid to dehydrate with the hydroxyl (-OH) groups on the surface of the biochar, thereby introducing more carboxyl groups (-COOH).

[0012] Preparation process of the present invention: NaAlO 2 and NaOH impregnation - pyrolysis carbonization - organic acid conversion. 2 The biomass was first impregnated with NaOH to make NaAlO 2 The NaOH molecules enter the organic structure and fiber of biomass. The pyrolysis carbonization process can not only play a role in pore formation, but also ensure that NaAlO 2 Then, LiCl and polybasic organic acid were used to embed NaAlO 2 The biochar reacts with NaOH, which mainly involves two reactions: one is NaAlO 2 It reacts with LiCl and polybasic organic acid to form lithium aluminum layered hydroxide, which is then converted into LiCl·2Al(OH) by washing with HCl.3 ·nH 2 O. Second, polybasic organic acids contain multiple carboxyl groups (-COOH). At high temperatures, part of the carboxyl groups (-COOH) in their structure undergo esterification reaction with the hydroxyl groups on the surface of biochar, while the remaining carboxyl groups in the organic acid continue to exist, thereby introducing carboxyl groups (-COOH) into biochar.

[0013] Since lithium aluminum hydroxide has a selective adsorption effect on lithium ions in brine, -COOH also has a certain adsorption effect on calcium and magnesium ions. After lithium aluminum hydroxide adsorbs lithium ions, water can be used to elute lithium ions, while calcium and magnesium ions coordinated with carboxyl groups can only be eluted with acid. The biochar-based organic-inorganic composite lithium ion adsorption material (i.e., lithium ion adsorbent) prepared by the present invention can not only adsorb lithium ions, but also adsorb calcium and magnesium ions, and elute lithium ions from the adsorption material by first washing with water, and then washing the calcium and magnesium ions on the adsorbent with acid, thereby realizing the gradual separation of lithium ions and calcium and magnesium ions. Therefore, the biochar-based organic-inorganic composite lithium ion adsorption material prepared by this method can simultaneously adsorb lithium, calcium, and magnesium ions in brine, and successively achieve the separation of lithium ions and calcium and magnesium by washing with water and acid.

[0014] As a preferred embodiment of the preparation method of the present invention, in the step (1), the nut shell is at least one of macadamia nut shell, walnut shell, and peanut shell.

[0015] As a preferred embodiment of the preparation method of the present invention, in step (1), nut shells and NaAlO 2 The mass ratio of NaAlO in the mixed solution is 10:(2-5), the mass ratio of nut shell to NaOH is 10:(0.2-0.5), 2 The concentration of is (20~50) g / L, and the concentration of NaOH is (2~5) g / L.

[0016] As a preferred embodiment of the preparation method of the present invention, in the step (1), the mesh size of the crushed nut shells is 40 to 60 meshes, the standing time is 12 to 24 hours, and the drying temperature is 80°C.

[0017] As a preferred embodiment of the preparation method of the present invention, in the step (2), the reaction conditions are: reacting at 400-600° C. for 1-3 hours under a nitrogen atmosphere.

[0018] As a preferred embodiment of the preparation method of the present invention, in the step (3), the mass ratio of LiCl to nut shell is (1-2.5):10, the mass ratio of the polybasic organic acid to the nut shell is (2-5):10, the concentration of LiCl dissolved in water is (20-50) g / L, and the concentration of the polybasic organic acid dissolved in water is (40-100) g / L.

[0019] As a preferred embodiment of the preparation method of the present invention, in the step (3), the stirring reaction conditions are stirring the reaction at room temperature for 6 to 12 hours, and the drying temperature is 120°C, and the continued reaction conditions are stirring the reaction at room temperature for 6 to 12 hours, and the drying temperature is 80°C.

[0020] As a preferred embodiment of the preparation method of the present invention, in the step (3), the concentration of the NaOH solution is 0.01 mol / L, the concentration of the HCl solution is 0.01 mol / L, and the washing conditions are to use NaOH solution and HCl solution for alternating, repeated, and multiple washings.

[0021] As a preferred embodiment of the preparation method of the present invention, in the step (3), the polybasic organic acid is at least one of tartaric acid, citric acid and malic acid.

[0022] In a second aspect, the present invention also provides a biochar-based lithium ion adsorbent prepared by the above preparation method.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention uses nut shells as raw materials and adopts NaAlO 2 The biochar was prepared by using NaOH as an activator, and a granular lithium aluminum hydroxide-carboxylated biochar composite lithium ion adsorption material was prepared by organic acid conversion and chemical grafting. This is not only beneficial for the extraction of lithium resources in brine, but also for the application of biochar-based lithium ion adsorption materials.

[0025] (2) The biochar-based organic-inorganic composite lithium ion adsorption material prepared by this method can simultaneously adsorb lithium, calcium, and magnesium ions in brine, and can effectively separate lithium ions and calcium and magnesium ions in brine through water washing and acid washing.

[0026] (3) The biochar used in this method is widely available, easy to obtain, and has controllable costs.

[0027] (4) The adsorption material prepared based on biochar in this method fully utilizes the physical and chemical properties of biochar itself to prepare an organic-inorganic composite lithium ion adsorption material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a process flow chart of the biochar-based lithium ion adsorbent in the present invention.

[0029] Figure 2 These are SEM images of biochar and the lithium ion adsorbent based on biochar in Example 3, wherein (a) is the SEM image of biochar, and (b) is the SEM image of the lithium ion adsorbent based on biochar.

[0030] Figure 3 This is the XRD pattern of the biochar-based lithium ion adsorbent prepared in Example 3. DETAILED DESCRIPTION

[0031] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0032] The process flow chart of the lithium ion adsorbent based on biochar in the present invention is as follows Figure 1 shown.

[0033] The test method for lithium ion adsorption and regeneration performance in brine used in the embodiment of the present invention is as follows:

[0034] (1) 0.5 g of lithium ion adsorbent was added to a conical flask containing 100 mL of brine, and the adsorbent was shaken and adsorbed for 12 h at room temperature. The lithium ion concentration in the brine was determined by ICP-OES, and the amount of lithium ions adsorbed in the brine was calculated.

[0035] (2) After the adsorbent that has adsorbed lithium ions in step (1) is shaken and desorbed with 50 mL of distilled water at room temperature for 6 h, the adsorbent is dried for later use.

[0036] (3) Steps (1) and (2) were repeated five times to test the recycling performance of the adsorbent.

[0037] The lithium ion concentration in the brine used in the adsorption process was 60.46 mg / L, the calcium ion concentration was 178.62 mg / L, and the magnesium ion concentration was 62.84 mg / L.

[0038] Example 1

[0039] A method for preparing a lithium ion adsorbent based on biochar, comprising the following steps:

[0040] (1) Weigh 2g NaAlO 2 and 0.2g NaOH were added to 100mL distilled water to prepare a mixed solution. After crushing the peanut shells, collect the 40-60 mesh particles, weigh 10g and place them in a beaker, add the mixed solution, let it stand for 12 hours, and then place it in a constant temperature drying oven at 80°C to dry to constant weight to obtain the solid phase of step (1).

[0041] (2) The solid phase of step (1) is transferred to a nickel crucible, reacted at 400° C. for 3 h in a tube furnace under a nitrogen atmosphere, and then taken out and cooled to room temperature for standby use to obtain the solid phase of step (2).

[0042] (3) Dissolve 1g LiCl and 2g malic acid in 50mL water, add the solid phase of step (2), mix thoroughly and adjust pH to 4, and stir at room temperature for 6h. Then transfer to a constant temperature drying oven, dry to constant weight at 120°C, and continue to react for 6h. The solid phase after the reaction is washed alternately, repeatedly, and multiple times with 0.01mol / L NaOH solution and 0.01mol / L HCl solution, and then dried at 80°C to constant weight to obtain a lithium ion adsorbent based on biochar.

[0043] The lithium ion adsorption and regeneration performance of the biochar-based lithium ion adsorbent prepared in this embodiment: 1.0g of the adsorbent was weighed and mixed with 25mL of brine in a conical flask, and adsorbed at room temperature for 6h. After testing, the lithium ion adsorption amount was 3.38mg / g, the calcium ion adsorption amount was 17.64mg / g, and the magnesium ion adsorption amount was 14.48mg / g. After 5 cycles of adsorption-desorption, the adsorbent had an adsorption capacity of 3.75mg / g for lithium ions, 15.26mg / g for calcium ions, and 12.66mg / g for magnesium ions.

[0044] Example 2

[0045] A method for preparing a lithium ion adsorbent based on biochar, comprising the following steps:

[0046] (1) Weigh 3g NaAlO 2 and 0.4 g NaOH were added to 100 mL distilled water to prepare a mixed solution. After crushing the walnut shell, collect 40-60 mesh particles, weigh 10 g and place them in a beaker, add the mixed solution, let it stand for 18 hours, and then place it in a constant temperature drying oven at 80°C to dry to constant weight to obtain the solid phase of step (1).

[0047] (2) The solid phase of step (1) is transferred to a nickel crucible, reacted at 500° C. for 2 h in a tube furnace under a nitrogen atmosphere, and then taken out and cooled to room temperature for standby use to obtain the solid phase of step (2).

[0048] (3) Dissolve 2.0g LiCl and 3.5g tartaric acid in 50mL water, add the solid phase of step (2), mix thoroughly and adjust pH to 4.5, and stir at room temperature for 10h. Then transfer to a constant temperature drying oven, dry to constant weight at 120°C, and continue to react for 10h. The solid phase after the reaction is washed alternately, repeatedly, and multiple times with 0.01mol / LNaOH solution and 0.01mol / L HCl solution, and then dried at 80°C to constant weight to obtain a lithium ion adsorbent based on biochar.

[0049] The lithium ion adsorption and regeneration performance of the biochar-based lithium ion adsorbent prepared in this example: 1.0g of the adsorbent was weighed, mixed with 25mL of brine in a conical flask, and adsorbed at room temperature for 6 hours. After testing, the lithium ion adsorption capacity was 4.06mg / g, the calcium ion adsorption capacity was 22.52mg / g, and the magnesium ion adsorption capacity was 18.98mg / g. After 5 cycles of adsorption-desorption, the adsorbent adsorbed 3.52mg / g of lithium ions, 19.38mg / g of calcium ions, and 16.24mg / g of magnesium ions.

[0050] Example 3

[0051] A method for preparing a lithium ion adsorbent based on biochar, comprising the following steps:

[0052] (1) Weigh 5g NaAlO 2 and 0.5 g NaOH were added to 100 mL distilled water to prepare a mixed solution. After crushing the macadamia nut shell, collect the particles of 40-60 mesh, weigh 10 g and put them in a beaker, add the mixed solution, let it stand for 24 hours, and then place it in a constant temperature drying oven at 80°C to dry to constant weight to obtain the solid phase of step (1).

[0053] (2) The solid phase of step (1) is transferred to a nickel crucible, reacted at 600° C. for 1 h in a tube furnace under a nitrogen atmosphere, and then taken out and cooled to room temperature for standby use to obtain the solid phase of step (2).

[0054] (3) Dissolve 2.5g LiCl and 5g citric acid in 50mL water, add the solid phase of step (2), mix thoroughly and adjust pH to 5, and stir the reaction at room temperature for 12h. Then transfer to a constant temperature drying oven, dry to constant weight at 120°C, and continue to react for 12h. The solid phase after the reaction is washed alternately, repeatedly, and multiple times with 0.01mol / L NaOH solution and 0.01mol / L HCl solution, and then dried at 80°C to constant weight to obtain a lithium ion adsorbent based on biochar.

[0055] The SEM images of the biochar and the lithium ion adsorbent based on biochar in this embodiment are as follows: Figure 2 As shown in the figure, (a) is a SEM image of biochar (i.e., the solid phase of step (2)), and (b) is a SEM image of a lithium ion adsorbent based on biochar. It can be seen that the biochar is granular, has sharp edges and corners, a smooth surface, and a porous structure; after functional modification, a large number of nanoparticles cover its surface, indicating that new substances are generated, making its surface rougher. The XRD pattern of the lithium ion adsorbent based on biochar prepared in this embodiment is shown in FIG. Figure 3 As shown, there is obvious LiCl·2Al(OH) 3 ·nH 2O diffraction peak, proving that LiCl·2Al(OH) 3 ·nH 2 O was loaded on the surface of biochar.

[0056] The lithium ion adsorption and regeneration performance of the biochar-based lithium ion adsorbent prepared in this example: 1.0g of the adsorbent was weighed, mixed with 25mL of brine in a conical flask, and adsorbed at room temperature for 6 hours. After testing, the lithium ion adsorption capacity was 4.68mg / g, the calcium ion adsorption capacity was 30.60mg / g, and the magnesium ion adsorption capacity was 26.72mg / g. After 5 cycles of adsorption-desorption, the adsorbent adsorbed 3.94mg / g of lithium ions, 25.88mg / g of calcium ions, and 23.10mg / g of magnesium ions.

[0057] Comparative Example 1

[0058] The specific method is the same as that of Example 3, except that NaAlO is not added in step (1). 2 , and in step (3) NaAlO is added 2 The adsorbent prepared by this method has an adsorption capacity of 1.24 mg / g for lithium ions, 28.22 mg / g for calcium ions, and 25.96 mg / g for magnesium ions.

[0059] Comparative Example 2

[0060] The specific method is the same as that of Example 3, except that the NaAlO 2 Replace with Al(OH) 3 , other conditions remain unchanged, the prepared adsorbent is used to adsorb lithium ions in brine, and the adsorption capacity of lithium ions by the adsorbent prepared in this way is 0.78 mg / g. The adsorption capacity of calcium ions is 29.78 mg / g, and the adsorption capacity of magnesium ions is 26.06 mg / g.

[0061] Comparative Example 3

[0062] The specific method is the same as that of Example 3, except that the NaAlO 2 Replace with AlCl 3 , other conditions remain unchanged, the prepared adsorbent is used to adsorb lithium ions in brine. The adsorbent prepared in this way has an adsorption capacity of 1.50 mg / g for lithium ions, 31.32 mg / g for calcium ions, and 27.46 mg / g for magnesium ions.

[0063] Comparative Example 4

[0064] The specific method is the same as that of Example 3, except that the amount of LiCl in step (3) is changed to 0.5 g, and other conditions remain unchanged. The prepared adsorbent is used to adsorb lithium ions in brine. The adsorbent prepared in this way has an adsorption capacity of 2.66 mg / g for lithium ions, 29.38 mg / g for calcium ions, and 24.64 mg / g for magnesium ions.

[0065] Comparative Example 5

[0066] The specific method is the same as that of Example 3, except that the citric acid in step (3) is replaced by HCl, and other conditions remain unchanged. The prepared adsorbent is used to adsorb lithium ions in brine. The adsorbent prepared in this way has an adsorption capacity of 4.46 mg / g for lithium ions, 1.28 mg / g for calcium ions, and 1.04 mg / g for magnesium ions.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a lithium ion adsorbent based on biochar, It is characterized in that The preparation method comprises the following steps: (1) NaAlO 2 and NaOH are added into distilled water to prepare a mixed solution, the crushed nut shells are placed in a beaker, the mixed solution is added, and after standing, the mixed solution is dried to constant weight to obtain the solid phase of step (1); (2) placing the solid phase of step (1) in a crucible, reacting in a tube furnace, and then cooling to room temperature to obtain the solid phase of step (2); (3) dissolving LiCl and a polybasic organic acid in water, adding the solid phase of step (2), mixing thoroughly, adjusting the pH to 4-5, stirring for reaction, drying to constant weight, and continuing the reaction. The solid phase after the reaction is washed with a NaOH solution and an HCl solution, and then dried to constant weight to obtain a biochar-based lithium ion adsorbent; In the step (2), the reaction conditions are: reacting at 400-600° C. for 1-3 hours under a nitrogen atmosphere; In the step (3), the polybasic organic acid is at least one of tartaric acid, citric acid and malic acid.

2. The preparation method according to claim 1, It is characterized in that In the step (1), the nut shell is at least one of macadamia nut shell, walnut shell, and peanut shell.

3. The preparation method according to claim 1, It is characterized in that In the step (1), the nut shell and NaAlO 2 The mass ratio of NaAlO in the mixed solution is 10:(2-5), the mass ratio of nut shell to NaOH is 10:(0.2-0.5), 2 The concentration of is (20~50) g / L, and the concentration of NaOH is (2~5) g / L.

4. The preparation method according to claim 1, It is characterized in that In the step (1), the mesh size of the crushed nut shells is 40 to 60 meshes, the standing time is 12 to 24 hours, and the drying temperature is 80°C.

5. The preparation method according to claim 1, It is characterized in that In the step (3), the mass ratio of LiCl to nut shell is (1-2.5):10, the mass ratio of the polybasic organic acid to the nut shell is (2-5):10, the concentration of LiCl dissolved in water is (20-50) g / L, and the concentration of the polybasic organic acid dissolved in water is (40-100) g / L.

6. The preparation method according to claim 1, It is characterized in that In the step (3), the stirring reaction conditions are stirring the reaction at room temperature for 6 to 12 hours and the drying temperature is 120° C., and the continued reaction conditions are stirring the reaction at room temperature for 6 to 12 hours and the drying temperature is 80° C.

7. The preparation method according to claim 1, It is characterized in that In the step (3), the concentration of the NaOH solution is 0.01 mol / L, the concentration of the HCl solution is 0.01 mol / L, and the washing conditions are to use the NaOH solution and the HCl solution to wash alternately, repeatedly, and multiple times.

8. A biochar-based lithium ion adsorbent prepared by the preparation method according to any one of claims 1 to 7.