Matt black shading film and preparation method thereof

By using a composite resin liquid of crystalline and amorphous saturated polyester resin in the light-shielding film, combined with dispersant and other ingredients, the problem of poor compatibility between resin and carbon black is solved, high shielding and conductive properties are achieved, and light leakage is reduced. Suitable for optical equipment.

CN118440382BActive Publication Date: 2024-10-22ANHUI MINGXUN NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410645658.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-22
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

The existing light-shielding film has poor compatibility, adhesion and dispersion between the resin and carbon black, resulting in insufficient shielding ability and prone to light leakage, affecting the optical effect.

Method used

Using a resin liquid containing crystalline saturated polyester resin and non-crystalline saturated polyester resin, combined with dispersant, dye, catalyst and matting powder, through the design of base coat and matte black coating, the properties of carbon black and resin liquid are improved. Compatibility and dispersion, forming excellent shielding and conductive properties.

Benefits of technology

It significantly improves the shielding ability and conductive performance of the light-shielding film, reduces light leakage, improves the surface finish, and is suitable for light-shielding parts of optical equipment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a matte black shading film and a preparation method thereof, wherein the matte black shading film comprises a substrate layer, a primer layer and a matte black coating layer; wherein one side of the substrate layer comprises at least a primer layer, and the other side of the substrate layer comprises at least a matte black coating layer; the raw materials for preparing the primer layer comprise a resin liquid, a dispersant, conductive carbon black, a dye, a catalyst, a matte powder and an organic solvent; the raw materials for preparing the matte black coating layer comprise a resin liquid, a polycarbonate diol, a dispersant, conductive carbon black, a dye, a silicon powder, a catalyst, a matte powder and an organic solvent; the resin liquid comprises a crystalline saturated polyester resin, a non-crystalline saturated polyester resin and an organic solvent. The matte black shading film provided by the present invention has excellent shielding performance and electrical conductivity, and can reduce the light leakage phenomenon of the shading film, improve the surface finish of the shading film, so that it can be widely used in shading components of optical equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of light-shielding components of optical equipment, and in particular to a matte black light-shielding film and a preparation method thereof. Background Art

[0002] Usually, electronic devices such as mobile phones, smart phones and other information communication terminals, pocket cameras, digital cameras, digital video cameras, projectors, and car cameras have built-in camera modules for photographing a subject and converting it into an image signal. The camera module usually includes an imaging element for photographing the subject and a lens unit for imaging the image of the subject on the imaging element, and the lens unit is usually composed of a combination of multiple lenses.

[0003] In such optical devices, it is expected to remove unnecessary incident light and reflected light, prevent the generation of halo, lens glare, ghosting and other phenomena that affect the optical effect, and improve the quality of the captured image. For the fixed components such as baffles, annular components, movable components such as shutter blades and aperture blades, and module inner wall components that are used to limit the light receiving range or prevent light leakage between components, high light shielding properties are usually required. Therefore, various lens units, camera modules, etc. equipped with components with high light shielding properties have appeared in the prior art.

[0004] Based on the requirements of high light-shielding properties and lens structure, the prior art uses a light-absorbing film containing materials such as carbon black, lubricants, particles and binder resins disposed on the surface of a substrate film to form a light-shielding film with light-shielding capabilities, which is then disposed on the surface of optical devices such as lenses to achieve the effect of light-shielding and improving optical quality.

[0005] A light-shielding film generally includes a substrate layer and a light-shielding layer, wherein the substrate layer material of the light-shielding film is generally a polymer material, including polyolefin film, polyethylene terephthalate, polyimide film or polyurethane film, etc., wherein polyethylene terephthalate (PET) material has excellent physical and mechanical properties and stable chemical properties, and is low in price and recyclable, and is often used as the substrate layer material of the light-shielding film; and the light-shielding layer material generally contains carbon black, lubricant, microparticles and binder resin, etc., and the light-shielding layer material thus formed not only has good light-shielding ability, but can also be effectively bonded to the substrate layer and the light-shielding component.

[0006] However, the shielding ability of the existing shading film still needs to be improved. At the same time, in order to improve the shading and sliding properties of the shading film, a large amount of lubricant and matting powder need to be added to the shading ink. However, in the shading film materials of the existing technology, the compatibility and adhesion between the resin and the carbon black are poor, and light leakage often occurs, affecting the optical effect. In addition, the dispersion uniformity between the resin and the carbon black is low, resulting in low surface finish and low sliding ability of the shading film.

[0007] Therefore, there is an urgent need for a matte black shading film that has excellent compatibility, adhesion and dispersibility between resin and carbon black, and thus has excellent shielding ability and conductive properties, and has a high surface finish and can prevent light leakage. Summary of the invention

[0008] Purpose of the invention: In view of the defects of the prior art, the purpose of the present invention is to provide a matte black shading film and its preparation method which has excellent compatibility, adhesion and dispersibility between resin and carbon black, and thus has excellent shielding ability and conductive properties, and has a high surface finish and can prevent light leakage.

[0009] Technical solution:

[0010] A matte black shading film, comprising:

[0011] - substrate layer, base coating and matte black coating;

[0012] Wherein, one side of the substrate layer at least comprises a primer layer, and the other side of the substrate layer at least comprises a matte black coating layer;

[0013] The raw materials for preparing the primer layer include resin liquid, dispersant, conductive carbon black, dye, catalyst, matting powder and organic solvent;

[0014] The raw materials for preparing the matte black coating include resin liquid, polycarbonate diol, dispersant, conductive carbon black, dye, silicon powder, catalyst, matting powder and organic solvent;

[0015] The resin solution comprises a crystalline saturated polyester resin, a non-crystalline saturated polyester resin and an organic solvent; the weight average molecular weight of the crystalline saturated polyester resin is 8000-30000, and the TG is 35-50°C; the weight average molecular weight of the non-crystalline saturated polyester resin is 10000-30000, and the TG is 40-60°C.

[0016] The resin liquid in the present invention is prepared by mixing crystalline saturated polyester resin, non-crystalline saturated polyester resin and organic solvent. On the one hand, based on the crystalline saturated polyester resin with strong cohesive force, it has excellent adhesion ability with carbon black; on the other hand, by adding non-crystalline saturated polyester resin, the dispersion ability of carbon black in the resin liquid can be improved; finally, by the composite use of crystalline saturated polyester resin and non-crystalline saturated polyester resin, the compatibility of carbon black in the resin liquid can be improved, and then through the excellent compatibility, adhesion and dispersibility between carbon black and resin liquid, the shielding ability and conductive performance of the shading film can be significantly improved, and the occurrence of light leakage can be reduced.

[0017] The present invention further limits the molecular weight and glass transition temperature of the crystalline saturated polyester resin and the non-crystalline saturated polyester resin. The limited crystalline saturated polyester resin and the non-crystalline saturated polyester resin have better compatibility, adhesion and dispersibility with carbon black, which can further improve the shielding ability and conductive performance of the shading film.

[0018] Furthermore, the crystalline saturated polyester resin is prepared by esterification and polycondensation of adipic acid, terephthalic acid, ethylene glycol and polyethylene glycol.

[0019] Furthermore, the mass ratio of adipic acid, terephthalic acid, ethylene glycol and polyethylene glycol is (3-8): (8-12): (2-6): (10-25); the molecular weight of the polyethylene glycol is 200-1000, and the obtained crystalline saturated polyester resin includes but is not limited to Toyobo GK780.

[0020] The present invention further limits the mass ratio of adipic acid, terephthalic acid, ethylene glycol and polyethylene glycol in the crystalline saturated polyester resin. The crystalline saturated polyester resin prepared within the limited range has stable chemical properties and can produce the effect of improving the compatibility between the resin liquid and the carbon black. Too high or too low a ratio will lead to unstable properties of the obtained resin and affect the compatibility between the resin liquid and the carbon black.

[0021] The present invention further limits the molecular weight of polyethylene glycol in the crystalline saturated polyester resin. The polyethylene glycol within the limited range has the function of graftability and improving the cohesiveness of the resin.

[0022] Furthermore, the non-crystalline saturated polyester resin is prepared by reacting isophthalic acid, ethylene glycol and propylene glycol. The prepared non-crystalline saturated polyester resin includes but is not limited to Toyobo 103.

[0023] Furthermore, the amine value of the dispersant is 8-25 mgKOH / g; the dispersants in the primer layer are dispersant A and dispersant B, the dispersant A is a polyester dispersant, the dispersant B is a polyurethane dispersant, and the mass ratio of the dispersant A to the dispersant B is (1-3): (5-10).

[0024] The present invention further limits the selection of the dispersant in the base coating layer and further limits the ratio of the dispersant A to the dispersant B. The limited dispersant can improve the dispersibility between the carbon black and the resin liquid.

[0025] The present invention further defines dispersant A as Euka 605S dispersant and dispersant B as BYK163 dispersant. The defined dispersants can further improve the dispersibility between carbon black and resin liquid.

[0026] The present invention adds a dispersant to the base coating and the matte black coating, which not only improves the dispersibility between carbon black and the resin liquid, further improves the shielding ability and conductivity of the shading film, but also overcomes the problem of poor dispersibility between the resin liquid and the polycarbonate diol in the matte black coating, thereby making the polycarbonate diol and the carbon black have excellent dispersibility and adhesion ability, further improving the shielding ability of the matte black coating.

[0027] Furthermore, the material of the substrate layer is at least one of PET and PI, and the PET is selected from one of APET and RPET; the particle size d of the silicon powder is 50 The catalyst is selected from at least one of an organic tin catalyst, an organic zirconium catalyst or an organic bismuth catalyst; and the organic solvent is selected from at least one of a ketone solvent or an ester solvent.

[0028] Furthermore, the dye is selected from at least one of reactive black, reactive brown or inorganic blue; the conductive carbon black is selected from at least one of Ketjen black, acetylene black or Cabot black; and the matting powder is a silica-based matting powder.

[0029] Further, by weight,

[0030] The resin solution comprises 10-20 parts of crystalline saturated polyester resin, 20-30 parts of non-crystalline saturated polyester resin and 50-70 parts of organic solvent;

[0031] The raw materials for preparing the base coating layer include 70-100 parts of resin liquid, 7-15 parts of dispersant, 15-25 parts of conductive carbon black, 3-8 parts of dye, 0.1-0.5 parts of catalyst, 3-8 parts of matting powder and 60-90 parts of organic solvent;

[0032] The raw materials for preparing the matte black coating include 50-70 parts of resin liquid, 8-15 parts of polycarbonate diol, 5-8 parts of dispersant, 3-5 parts of conductive carbon black, 12-18 parts of dye, 8-12 parts of silicon powder, 0.1-0.5 parts of catalyst, 3-5 parts of matting powder and 60-90 parts of organic solvent.

[0033] Furthermore, the thickness of the substrate layer is 1-300 μm; the thickness of the primer layer is 1-10 μm; and the thickness of the matte black coating layer is 0.3-5 μm.

[0034] Any one of the above-mentioned methods for preparing a matte black light-shielding film comprises the following steps:

[0035] (1) coating silica gel and a substrate layer on the protective layer in sequence, then mixing the raw materials for preparing the matte black coating and coating them on the substrate layer, and forming a matte black coating on the substrate layer after aging;

[0036] (2) After rewinding and peeling, the silicone and protective layer on the substrate layer are removed, and the silicone and protective layer are sequentially formed on the matte black coating layer;

[0037] (3) The raw materials for preparing the primer layer are mixed and coated on the other side of the substrate layer, and the primer layer is formed on the other side of the substrate layer after aging. After the silica gel and the protective layer are removed, the matte black light-shielding film is obtained after extrusion and packaging.

[0038] Furthermore, the aging temperature is 40-60° C. and the aging time is 36-72 hours.

[0039] Beneficial effects:

[0040] (1) The matte black shading film provided by the present invention has excellent compatibility, adhesion and dispersibility between the uniquely configured resin liquid and carbon black, and is made into a base coating and a matte black coating by combining other ingredients such as a dispersant, a dye, a catalyst, a matting powder, and silica powder. Not only can the prepared matte black shading film have excellent shielding performance and conductivity, but it can also reduce the light leakage phenomenon of the shading film and improve the surface finish of the shading film, so that it can be widely used in shading components of optical equipment.

[0041] (2) The resin liquid in the matte black shading film provided by the present invention is prepared by mixing crystalline saturated polyester resin, non-crystalline saturated polyester resin and organic solvent. On the one hand, based on the crystalline saturated polyester resin with strong cohesive force, it has excellent adhesion ability with carbon black; on the other hand, by adding non-crystalline saturated polyester resin, the dispersion ability of carbon black in the resin liquid can be improved; finally, by the composite use of crystalline saturated polyester resin and non-crystalline saturated polyester resin, the compatibility of carbon black in the resin liquid can be improved. Furthermore, through the excellent compatibility, adhesion and dispersibility between carbon black and resin liquid, the shielding ability and conductive performance of the shading film can be significantly improved, and the occurrence of light leakage can be reduced.

[0042] (3) In the matte black shading film provided by the present invention, by adding a dispersant to the base coating and the matte black coating, not only can the dispersibility between carbon black and the resin liquid be improved, thereby further improving the shielding ability and conductivity of the shading film, but also the problem of poor dispersibility between the resin liquid and the polycarbonate diol in the matte black coating can be overcome, thereby making the polycarbonate diol and the carbon black have excellent dispersibility and adhesion ability, thereby further improving the shielding ability of the matte black coating.

[0043] (4) In the matte black light-shielding film provided by the present invention, by adding dye, silicon powder, catalyst and matting powder to the base coating and the matte black coating, the prepared light-shielding film can have a stable and uniform structure and performance, and the shielding ability and conductive performance of the light-shielding film can be improved. DETAILED DESCRIPTION

[0044] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0045] The commercially available shading film is matte black PET film polyester film YZ017-XX purchased from Dongguan Yizhou New Material Technology Co., Ltd.; the commercially available resin liquid is polyurethane S-335 purchased from Wengkaier (Shanghai) International Trading Co., Ltd.; the polyester dispersant is purchased from Shizhong Mingzhi Chemical (Shanghai) Co., Ltd., and the Uka 605S dispersant with the item number yk-029; the polyurethane dispersant is purchased from Guangdong Sandingjia New Material Technology Co., Ltd., and the BYK163 dispersant with the item number SDJ8006; the remaining reagents and equipment are conventional reagents and equipment in this technical field.

[0046] Preparation of crystalline saturated polyester resin-1

[0047] The crystalline saturated polyester resin-1 was prepared by the following steps:

[0048] In a reactor, 3 g of adipic acid, 10 g of terephthalic acid and 5 g of ethylene glycol were added, heated to 130° C. and reacted under acidic conditions for 5 hours, then 15 g of polyethylene glycol with a molecular weight of 400 and 0.3 g of titanate were added, the temperature was raised to 160° C. and reacted for 3 hours, then cooled, filtered, washed and dried to obtain the crystalline saturated polyester resin-1;

[0049] The obtained crystalline saturated polyester resin-1 had a weight average molecular weight of 15,000 and a TG of 40°C.

[0050] Preparation of crystalline saturated polyester resin-2

[0051] The preparation method is basically the same as that of crystalline saturated polyester resin-1, except that the masses of adipic acid, terephthalic acid, ethylene glycol and polyethylene glycol with a molecular weight of 400 are changed to 5g, 5g, 10g and 5g respectively. The obtained crystalline saturated polyester resin-2 has a weight average molecular weight of 11000 and a TG of 37°C.

[0052] Preparation of crystalline saturated polyester resin-3

[0053] The preparation method is basically the same as that of crystalline saturated polyester resin-1, except that the polyethylene glycol with a molecular weight of 400 is replaced with polyethylene glycol with an equivalent molecular weight of 3000. The obtained crystalline saturated polyester resin-3 has a weight average molecular weight of 18000 and a TG of 55°C.

[0054] Preparation of non-crystalline saturated polyester resin-1

[0055] The non-crystalline saturated polyester resin-1 was prepared by the following steps:

[0056] In a reactor, 10 g of isophthalic acid, 2 g of ethylene glycol and 2.5 g of propylene glycol were added, heated to 120° C. and reacted under acidic conditions for 4 hours, then heated to 180° C. and reacted for 4 hours, then cooled, filtered, washed and dried to obtain the non-crystalline saturated polyester resin-1;

[0057] The obtained non-crystalline saturated polyester resin-1 had a weight average molecular weight of 25,000 and a TG of 50°C.

[0058] Example 1

[0059] The matte black light-shielding film was prepared by the following steps:

[0060] (1) coating silica gel and a substrate layer on the protective layer in sequence, and then coating the raw materials for preparing a matte black coating layer on the substrate layer after mixing them evenly, and forming a matte black coating on the substrate layer after aging at 50° C. for 48 hours;

[0061] (2) After rewinding and peeling, the silicone and protective layer on the substrate layer are removed, and the silicone and protective layer are sequentially formed on the matte black coating layer;

[0062] (3) Mixing the raw materials for preparing the primer layer and coating them on the other side of the substrate layer, and curing them at 50° C. for 48 hours to form a primer layer on the other side of the substrate layer. After removing the silica gel and the protective layer, the thickness of the substrate layer is controlled to be 8 μm, the thickness of the primer layer is 3 μm, and the thickness of the matte black coating layer is 2 μm. After extrusion and packaging, the matte black light-shielding film is obtained;

[0063] The substrate layer material is RPET;

[0064] By weight,

[0065] The raw materials for preparing the primer layer include 80 parts of resin liquid, 2 parts of polyester dispersant, 7 parts of polyurethane dispersant, 6 parts of Ketjen black, 15 parts of acetylene black, 5 parts of Prussian blue dye, 0.3 parts of zirconium isooctanoate, 5 parts of Evonik 8018-1 matting powder, 20 parts of cyclohexanone and 60 parts of ethyl ester;

[0066] The raw materials for preparing the matte black coating include 60 parts of resin liquid, 10 parts of polycarbonate diol, 6 parts of polyurethane dispersant, 4 parts of ultra-high 250G, 15 parts of active black BL / GR, 10 parts of particle size d 50 1 μm silicon powder, 0.2 parts of TIN-22 organotin catalyst, 5 parts of Evonik 8018-1 matting powder, 20 parts of cyclohexanone and 60 parts of ethyl ester;

[0067] The resin solution includes 15 parts of crystalline saturated polyester resin-1, 25 parts of non-crystalline saturated polyester resin-1, 30 parts of butanone, 20 parts of ethyl acetate and 10 parts of cyclohexanone.

[0068] Example 2

[0069] The same as Example 1, except that the substrate material is changed to PI of equal thickness; by weight,

[0070] The raw materials for preparing the primer layer include 90 parts of resin liquid, 3 parts of polyester dispersant, 8 parts of polyurethane dispersant, 8 parts of Temega 250G, 12 parts of Mitsubishi MA100, 3 parts of Prussian blue dye, 0.3 parts of TIN-22 organotin catalyst, 6 parts of Evonik 8018-1 matting powder, 20 parts of cyclohexanone and 60 parts of ethyl ester;

[0071] The raw materials for preparing the matte black coating include 65 parts of resin liquid, 8 parts of polycarbonate diol, 8 parts of polyurethane dispersant, 3 parts of acetylene black, 12 parts of active black BL / GR, 8 parts of particle size d 50 0.5 μm silica powder, 0.1 parts of zirconium isooctanoate, 5 parts of Evonik 8018-1 matting powder, 20 parts of cyclohexanone and 60 parts of ethyl acetate;

[0072] The resin solution includes 10 parts of Toyobo GK780, 25 parts of Toyobo 103, 30 parts of butanone, 20 parts of ethyl acetate and 10 parts of cyclohexanone.

[0073] Example 3

[0074] The same as Example 1, except that the substrate material is changed to APET of equal thickness; by weight,

[0075] The raw materials for preparing the primer layer include 70 parts of resin liquid, 4 parts of polyester dispersant, 8 parts of polyurethane dispersant, 10 parts of Cabot carbon black M1400, 15 parts of Mitsubishi MA100, 8 parts of active black BL / GR, 0.3 parts of TIN-22 organic tin catalyst, 4 parts of Evonik 8018-1 matting powder, 20 parts of cyclohexanone and 60 parts of ethyl ester;

[0076] The raw materials for preparing the matte black coating include 55 parts of resin liquid, 15 parts of polycarbonate diol, 7 parts of polyurethane dispersant, 5 parts of Ketjen black, 18 parts of active black BL / GR, 12 parts of particle size d 50 1.5 μm silicon powder, 0.3 parts of TIN-22 organotin catalyst, 5 parts of Evonik 8018-1 matting powder, 20 parts of cyclohexanone and 60 parts of ethyl ester;

[0077] The resin solution includes 15 parts of crystalline saturated polyester resin-1, 30 parts of Toyobo 103, 30 parts of butanone, 20 parts of ethyl acetate and 10 parts of cyclohexanone.

[0078] Example 4

[0079] The method is basically the same as Example 1, except that the 2 parts of polyester dispersant and 7 parts of polyurethane dispersant in the dispersant base coat are replaced with 9 parts of polyurethane dispersant.

[0080] Example 5

[0081] The method is basically the same as Example 1, except that the crystalline saturated polyester resin-1 in the resin solution is replaced by an equal amount of crystalline saturated polyester resin-2.

[0082] Example 6

[0083] The method is basically the same as Example 1, except that the crystalline saturated polyester resin-1 in the resin solution is replaced by an equal amount of crystalline saturated polyester resin-3.

[0084] Comparative Example 1

[0085] Commercially available light-shielding film.

[0086] Comparative Example 2

[0087] The process is basically the same as Example 1, except that the resin liquid is replaced with an equal amount of commercially available resin liquid.

[0088] Comparative Example 3

[0089] The method is basically the same as Example 1, except that the non-crystalline saturated polyester resin-1 in the resin solution is replaced with an equal amount of crystalline saturated polyester resin-1.

[0090] Comparative Example 4

[0091] The method is basically the same as Example 1, except that the crystalline saturated polyester resin-1 in the resin solution is replaced by an equal amount of non-crystalline saturated polyester resin-1.

[0092] Performance Testing

[0093] Total thickness test: According to the ASTM D3652 standard for testing the length, width and thickness of adhesive tapes, the total thickness of the products of Examples 1-6 and Comparative Examples 1-4 was tested.

[0094] Surface cleanliness detection: According to the JIS B 0601 surface roughness test standard, the roughness Ra of the products of Examples 1-6 and Comparative Examples 1-4 was detected.

[0095] Shielding ability test: According to JIS-K7651:1988, an optical densitometer was used to test the optical transmission density of the products of Examples 1-6 and Comparative Examples 1-4.

[0096] Conductivity test: According to JIS-K6911:1995, the surface resistivity of the products of Examples 1-6 and Comparative Examples 1-4 was tested.

[0097] The test results are shown in the following table:

[0098] Total thickness (μm) Roughness Ra (μm) Optical transmittance concentration OD value Surface resistivity (Ω) Example 1 13 0.2 8.7 10^4.5 Example 2 13 0.2 8.8 10^4.4 Example 3 13 0.2 8.7 10^4.4 Example 4 13 0.7 6.7 10^4.9 Example 5 13 0.4 7.0 10^4.6 Example 6 13 0.4 7.2 10^4.6 Comparative Example 1 20 1.3 4.3 10^5.0 Comparative Example 2 13 0.4 6.1 10^5.1 Comparative Example 3 13 0.4 6.8 10^4.8 Comparative Example 4 13 0.3 6.5 10^4.7

[0099] According to the comparison of the test results of Examples 1-3 with Comparative Example 1, it can be seen that the matte black light-shielding film provided by the present invention has better shielding ability and conductive ability than the light-shielding film in the prior art, and has high surface cleanliness.

[0100] According to the comparison of the test results of Examples 1-3 and Comparative Examples 2-4, it can be seen that the resin liquid prepared by compounding saturated polyester resin and non-crystalline saturated polyester resin in the present invention can significantly improve the shielding ability and conductivity of the light-shielding film, and can improve the surface cleanliness of the light-shielding film.

[0101] According to the comparison of the test results of Examples 1-3 and Example 4, it can be seen that by adding a specific dispersant in the present invention, not only the surface cleanliness of the light-shielding film can be improved, but also the shielding ability and conductivity of the light-shielding film can be further improved.

[0102] According to the comparison of the test results of Examples 1-3 and 5-6, it can be seen that the present invention limits the mass ratio of each component in the crystalline saturated polyester resin and the molecular weight of polyethylene glycol, so that the prepared crystalline saturated polyester resin can improve the compatibility between the resin liquid and carbon black, thereby affecting the surface smoothness, shielding ability and conductivity of the shading film.

[0103] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A matte black shading film, characterized in that: The matte black shading film contains: - substrate layer, base coating and matte black coating; Wherein, one side of the substrate layer at least comprises a primer layer, and the other side of the substrate layer at least comprises a matte black coating layer; The raw materials for preparing the primer layer include resin liquid, dispersant, conductive carbon black, dye, catalyst, matting powder and organic solvent; The raw materials for preparing the matte black coating include resin liquid, polycarbonate diol, dispersant, conductive carbon black, dye, silicon powder, catalyst, matting powder and organic solvent; The resin solution comprises a crystalline saturated polyester resin, a non-crystalline saturated polyester resin and an organic solvent; the crystalline saturated polyester resin has a weight average molecular weight of 8000-30000 and a Tg of 35-50° C.; the non-crystalline saturated polyester resin has a weight average molecular weight of 10000-30000 and a Tg of 40-60° C.; The crystalline saturated polyester resin is prepared by esterification and polycondensation of adipic acid, terephthalic acid, ethylene glycol and polyethylene glycol; The mass ratio of adipic acid, terephthalic acid, ethylene glycol and polyethylene glycol is (3-8): (8-12): (2-6): (10-25); the molecular weight of the polyethylene glycol is 200-1000; The non-crystalline saturated polyester resin is prepared by reacting isophthalic acid, ethylene glycol and propylene glycol.

2. The matte black light-shielding film according to claim 1, characterized in that: The amine value of the dispersant is 8-25 mgKOH / g; the dispersants in the primer layer are dispersant A and dispersant B, the dispersant A is a polyester dispersant, the dispersant B is a polyurethane dispersant, and the mass ratio of the dispersant A to the dispersant B is (1-3): (5-10).

3. The matte black light-shielding film according to claim 1, characterized in that: The material of the substrate layer is at least one of PET and PI, and the PET is selected from one of APET and RPET; the particle size of the silicon powder is d 50 The catalyst is selected from at least one of an organic tin catalyst, an organic zirconium catalyst or an organic bismuth catalyst; and the organic solvent is selected from at least one of a ketone solvent or an ester solvent.

4. The matte black light-shielding film according to claim 1, characterized in that: By weight, The resin solution comprises 10-20 parts of crystalline saturated polyester resin, 20-30 parts of non-crystalline saturated polyester resin and 50-70 parts of organic solvent; The raw materials for preparing the base coating layer include 70-100 parts of resin liquid, 7-15 parts of dispersant, 15-25 parts of conductive carbon black, 3-8 parts of dye, 0.1-0.5 parts of catalyst, 3-8 parts of matting powder and 60-90 parts of organic solvent; The raw materials for preparing the matte black coating include 50-70 parts of resin liquid, 8-15 parts of polycarbonate diol, 5-8 parts of dispersant, 3-5 parts of conductive carbon black, 12-18 parts of dye, 8-12 parts of silicon powder, 0.1-0.5 parts of catalyst, 3-5 parts of matting powder and 60-90 parts of organic solvent.

5. The matte black light-shielding film according to claim 1, characterized in that: The thickness of the substrate layer is 1-300 μm; the thickness of the primer layer is 1-10 μm; and the thickness of the matte black coating layer is 0.3-5 μm.

6. The method for preparing the matte black light-shielding film according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) coating silica gel and a substrate layer on the protective layer in sequence, then mixing the raw materials for preparing the matte black coating and coating them on the substrate layer, and forming a matte black coating on the substrate layer after aging; (2) After rewinding and peeling, the silicone and protective layer on the substrate layer are removed, and the silicone and protective layer are sequentially formed on the matte black coating layer; (3) The raw materials for preparing the primer layer are mixed and coated on the other side of the substrate layer, and the primer layer is formed on the other side of the substrate layer after aging. After the silica gel and the protective layer are removed, the matte black light-shielding film is obtained after extrusion and packaging.

7. The method for preparing a matte black light-shielding film according to claim 6, characterized in that: The aging temperature is 40-60° C. and the aging time is 36-72 hours.