A kind of high temperature acidification corrosion inhibitor and preparation method thereof
By adding a specific combination of main corrosion inhibitors and additives to the acidifying corrosion inhibitor, a protective film and a hydrophobic film are formed, which solves the problems of weakened adsorption and reduced water solubility at high temperatures, and achieves high-efficiency corrosion inhibition in high-temperature environments. Thermal stability is improved.
Patent Information
- Application Number
- CN202410540792.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-30
AI Technical Summary
The adsorption of existing acidifying corrosion inhibitors weakens at high temperatures, resulting in poor corrosion inhibition effect, and it is difficult to effectively protect under different corrosion conditions. How to ensure water solubility and thermal stability while enhancing the corrosion inhibition effect is a challenge.
A corrosion inhibitor for high-temperature acidification is used, including a main corrosion inhibitor, a synergist, an additive, a gelling agent and a porogen. The main corrosion inhibitor forms a protective film on the metal surface through adsorption of quaternary ammonium cations to enhance the adsorption effect. , and prevent the precipitation of inorganic salts through aminotrimethylenephosphonic acid and sodium ethylenediaminetetramethylenephosphonate, and combine with materials such as polyvinyl alcohol and barium sulfate to improve thermal stability and water solubility.
It can significantly improve the adsorption force and thermal stability of corrosion inhibitors in high-temperature environments, reduce the corrosion rate, and enhance the protective effect on metal surfaces. It is suitable for different corrosion conditions.
Smart Images

Figure BDA0004820967960000031 
Figure BDA0004820967960000032 
Figure BDA0004820967960000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of acidizing and corrosion inhibition, and in particular to a high temperature resistant acidizing corrosion inhibitor and a preparation method thereof. Background Art
[0002] During the oil development process, the mining environment becomes more and more complex as the mining industry deepens. The temperature and pressure of the mines gradually increase, and the mining efficiency gradually decreases. In order to increase the production of oil and gas wells, acidizing fluid is usually added to oil and gas wells. However, during the acidizing process, it is usually accompanied by the dissolution of carbonates, which causes serious corrosion of equipment and downhole oil pipes and casings. In order to reduce corrosion, corrosion inhibitors are usually added to the acidizing fluid. Existing acidizing corrosion inhibitors have disadvantages such as weakened adsorption at high temperatures, resulting in poor corrosion inhibition effects. Therefore, it is particularly necessary to improve the high temperature resistance of acidizing corrosion inhibitors.
[0003] Imidazoline derivatives are environmentally friendly corrosion inhibitors, which are widely used in the field of oil and gas wells. Currently, the most commonly used imidazoline quaternary ammonium salt corrosion inhibitors are obtained by dehydration condensation of organic acids and polyamines to obtain oil-soluble imidazolines, which are then obtained by alkylation. Imidazoline quaternary ammonium salt corrosion inhibitors are adsorption film-type corrosion inhibitors. The larger the molecular group of the corrosion inhibitor, the more adsorption points, and the more complete the adsorption on the metal surface, the slower the desorption rate at high temperature, and the better the corrosion inhibition effect of the corrosion inhibitor at high temperature. However, as the molecular weight of the corrosion inhibitor increases, the water solubility decreases, and high temperature will also affect the thermal stability of the corrosion inhibitor itself. Therefore, how to ensure the water solubility and thermal stability of the corrosion inhibitor itself while enhancing the corrosion inhibition effect is worthy of in-depth study. In addition, the function of the corrosion inhibitor in the prior art is relatively single, and it is difficult to effectively protect against different corrosion conditions such as scaling corrosion. It is necessary to develop a suitable modification method. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a high temperature resistant acidification corrosion inhibitor and a preparation method thereof.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A high temperature resistant acidification corrosion inhibitor comprises the following raw materials in parts by weight: 40-48 parts of a main corrosion inhibitor, 10-15 parts of a synergist, 1.5-2.5 parts of an additive, 30-36 parts of a gelling agent, 15-18 parts of a weighting agent and 15-18 parts of a porogen.
[0007] The synergist is antimony trioxide;
[0008] The additive is prepared by mixing aminotri(methylenephosphonic acid) and sodium ethylenediaminetetra(methylenephosphonic acid) in a mass ratio of 1:1;
[0009] The gelling agent is polyvinyl alcohol;
[0010] The weighting agent is barium sulfate;
[0011] The porogen is 5-methylbenzotriazole;
[0012] The preparation of the main corrosion inhibitor comprises the following steps:
[0013] Step A1: 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid and water are added to a flask, stirred at 30°C for 30 minutes, and then cooled to 0°C in an ice-water bath, and sodium nitrite solution is slowly added dropwise to the flask, and the reaction is stirred for 20-30 minutes to obtain a reaction solution, and urea is added until the reaction solution turns starch-potassium iodide test paper blue to obtain a diazonium salt intermediate; 4-allyl-2-methoxyphenol and methanol are then added to a three-necked flask, and sodium carbonate is added to adjust the pH to 7.5-8.5. Under stirring in an ice-water bath, the diazonium salt intermediate is slowly added dropwise, and the addition is completed within 45-60 minutes, and the reaction is continued with stirring for 2-2.5 hours to obtain a reaction product a;
[0014] Further, the dosage ratio of 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid, water, and sodium nitrite solution is 0.032 mol: 8 mL: 4 mL: 40-48 mL; the dosage ratio of 4-allyl-2-methoxyphenol, methanol, sodium carbonate, and diazonium salt intermediate is 0.016 mol: 100-120 mL: 0.005-0.010 mol: 0.016 mol; the mass fraction of concentrated hydrochloric acid is 36.5%, and the concentration of sodium nitrite solution is 1 mol / L;
[0015] During the reaction of step A1, 4-amino-3-nitrobenzoic acid first reacts with concentrated hydrochloric acid and sodium nitrite to generate a diazonium salt intermediate, and the diazonium salt intermediate then adds to the ortho position of the phenolic hydroxyl group on the benzene ring of 4-allyl-2-methoxyphenol to generate an azo-containing reaction product a; the structure of the reaction product a is shown below:
[0016]
[0017] Step A2: Add the reaction product a, ethanol and sodium hydroxide into a three-necked flask, heat to 65-75°C, start reflux stirring, then add sodium dithionite in three equal amounts, reflux stirring and react for 1-1.5h, cool to room temperature, add hydrochloric acid to adjust the pH to 5-6, filter, wash the filter cake with anhydrous ethanol, and dry to obtain the reaction product b;
[0018] Furthermore, the dosage ratio of the reaction product a, ethanol, sodium hydroxide and sodium dithionite is 0.1 mol: 135-155 mL: 0.02-0.05 mol: 0.1-0.2 mol; the dosage of sodium dithionite is the sum of the three additions; the volume fraction of ethanol is 95%;
[0019] During the reaction of step A2, under the action of sodium dithionite, the azo group on the benzene ring in the reaction product a and the nitro group adjacent to the azo group are ring-closed to form a benzotriazole ring, thereby obtaining a reaction product b; the structure of the reaction product b is shown below:
[0020]
[0021] Step A3: Add perfluorooctanoic acid, diethylenetriamine and xylene into a three-necked flask, introduce nitrogen, start reflux stirring, raise the temperature to 140-150°C, reflux stirring and react at a constant temperature for 3-3.5 hours, then quickly raise the temperature to 200°C, reflux stirring and react at a constant temperature for 2-2.5 hours to obtain a reaction product c;
[0022] Furthermore, the usage ratio of perfluorooctanoic acid, diethylenetriamine and xylene is 0.1 mol: 0.12-0.15 mol: 40-48 mL;
[0023] During the reaction of step A3, perfluorooctanoic acid first reacts with diethylenetriamine to generate a terminal amide product. After rapid heating, the terminal amide product undergoes a closed ring to generate a reaction product c. The structure of the reaction product c is shown below:
[0024]
[0025] Step A4: Add the reaction product b, toluene and the reaction product c to a reaction flask, heat it to 135-145°C, stir and react at a constant temperature for 10-12h to obtain the reaction product d, then add the reaction product d, benzyl chloride and n-propanol to a flask, heat it to 110-120°C, stir and react at a constant temperature for 6-7h to obtain the main corrosion inhibitor;
[0026] Further, the usage ratio of the reaction product b, toluene and the reaction product c is 1.05 mol:700-800 mL:1.00 mol; the usage ratio of the reaction product d, benzyl chloride and n-propanol is 1 mol:1.02 mol:850-950 mL;
[0027] In the reaction process of step A4, toluene is used as a water-carrying agent, and the carboxyl group of the reaction product b reacts with the amino group of the reaction product c to generate a reaction product d; the reaction product d then reacts with benzyl chloride to generate a quaternary ammonium salt product, i.e., the main corrosion inhibitor.
[0028] The preparation of the high temperature resistant acidification corrosion inhibitor comprises the following steps:
[0029] The main corrosion inhibitor, synergist, additive, gelling agent, weighting agent and pore-forming agent are mixed and stirred for 30-40 minutes, then transferred to an internal mixer and mixed at 140-150°C for 25-35 minutes, then cooled, crushed and formed by an injection molding machine to obtain a high temperature acidification resistant corrosion inhibitor with the same diameter and height of 3-5 mm.
[0030] Beneficial effects of the invention: The invention discloses a corrosion inhibitor for high temperature acidification, comprising a corrosion inhibitor main agent, a synergist, an additive, a gelling agent, a weighting agent and a porogen. The aminotrimethylphosphonic acid and sodium ethylenediaminetetramethylphosphonic acid in the additives used can prevent or reduce the precipitation and scaling of insoluble inorganic salts in water on the metal surface, and avoid the presence of scales leading to the weakening of the adsorption of the corrosion inhibitor main agent on the metal surface, which has an adverse effect on the corrosion inhibition function.
[0031] The synthesized main corrosion inhibitor belongs to the imidazoline quaternary ammonium salt type corrosion inhibitor. It adsorbs quaternary ammonium cations on the negatively charged metal surface. The long carbon chain acts as a hydrophobic group away from the metal, forming a protective film to keep hydrogen ions away from the metal. The molecular structure of the main corrosion inhibitor includes carbon-carbon double bonds, ether bonds, phenolic hydroxyl groups, amide bonds, triazole rings, imidazole rings, quaternary ammonium salts and long chains of fluorinated alkanes. The π electrons of the carbon-carbon double bond easily interact with the empty orbitals of metal atoms, which not only enhances the adsorption of the corrosion inhibitor to the metal, but also increases the water solubility of the corrosion inhibitor. The imidazole ring and triazole ring can complex with the metal to enhance the adsorption of the corrosion inhibitor on the metal surface, making it less likely to desorb at high temperatures. The ether bond, phenolic hydroxyl group, and amide bond increase the number of O and N atoms. The O and N atoms contain unshared lone electron pairs, which will interact with the empty d orbitals on the metal surface to form coordination bonds, further enhancing the adsorption of the corrosion inhibitor on the metal surface. The long chains of fluorinated alkanes are more hydrophobic and are closely arranged on the metal surface to form a denser hydrophobic protective film, which keeps hydrogen ions away from the metal, thereby better inhibiting corrosion. And because the CF bond has a higher bond energy, it is not easy to break when heated, which improves the thermal stability of the corrosion inhibitor and enables the corrosion inhibitor to act more stably in a high temperature environment. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A main corrosion inhibitor, the preparation of which comprises the following steps:
[0035] Step A1: 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid and water are added to a flask, stirred at 30°C for 30 minutes, and then cooled to 0°C with an ice-water bath. Sodium nitrite solution is slowly added dropwise to the flask, stirred and reacted for 20 minutes to obtain a reaction solution, and urea is added until the reaction solution turns starch-potassium iodide test paper blue to obtain a diazonium salt intermediate; 4-allyl-2-methoxyphenol and methanol are then added to a three-necked flask, sodium carbonate is added to adjust the pH to 7.5, and the diazonium salt intermediate is slowly added dropwise under stirring in an ice-water bath, and the addition is completed within 45 minutes, and the reaction is continued with stirring for 2 hours to obtain a reaction product a; the dosage ratio of 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid, water and sodium nitrite solution is 0.032 mol:8 mL:4 mL:40 mL; the dosage ratio of 4-allyl-2-methoxyphenol, methanol, sodium carbonate and diazonium salt intermediate is 0.016 mol l: 100mL: 0.005mol: 0.016mol; the mass fraction of concentrated hydrochloric acid is 36.5%, and the concentration of sodium nitrite solution is 1mol / L;
[0036] Step A2: Add the reaction product a, ethanol and sodium hydroxide into a three-necked flask, heat to 65°C, start reflux stirring, then add sodium dithionite in three equal amounts, reflux stirring and react for 1 hour, cool to room temperature, add hydrochloric acid to adjust the pH to 5, filter, wash the filter cake with anhydrous ethanol, and dry to obtain the reaction product b; the amount ratio of the reaction product a, ethanol, sodium hydroxide and sodium dithionite is 0.1 mol: 135 mL: 0.02 mol: 0.1 mol; the amount of sodium dithionite is the sum of the amounts added three times; the volume fraction of ethanol is 95%;
[0037] Step A3: Add perfluorooctanoic acid, diethylenetriamine and xylene into a three-necked flask, introduce nitrogen, start reflux stirring, heat to 140°C, reflux and react with constant temperature stirring for 3 hours, then quickly heat to 200°C, reflux and react with constant temperature stirring for 2 hours to obtain reaction product c; the dosage ratio of perfluorooctanoic acid, diethylenetriamine and xylene is 0.1 mol:0.12 mol:40 mL;
[0038] Step A4: Add the reaction product b, toluene and the reaction product c to a reaction flask, heat it to 135°C, and stir the reaction at a constant temperature for 10 hours to obtain a reaction product d, then add the reaction product d, benzyl chloride and n-propanol to a flask, heat it to 110°C, and stir the reaction at a constant temperature for 6 hours to obtain a corrosion inhibitor; the amount ratio of the reaction product b, toluene and the reaction product c is 1.05 mol:700 mL:1.00 mol; the amount ratio of the reaction product d, benzyl chloride and n-propanol is 1 mol:1.02 mol:850 mL.
[0039] Example 2
[0040] A main corrosion inhibitor, the preparation of which comprises the following steps:
[0041] Step A1: 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid and water are added to a flask, stirred at 30°C for 30 minutes, and then cooled to 0°C with an ice-water bath. Sodium nitrite solution is slowly added dropwise to the flask, stirred and reacted for 25 minutes to obtain a reaction solution, and urea is added until the reaction solution turns starch-potassium iodide test paper blue to obtain a diazonium salt intermediate; 4-allyl-2-methoxyphenol and methanol are then added to a three-necked flask, sodium carbonate is added to adjust the pH to 8.0, and the diazonium salt intermediate is slowly added dropwise under stirring in an ice-water bath, and the addition is completed within 55 minutes, and the reaction is continued with stirring for 2.2 hours to obtain a reaction product a; the dosage ratio of 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid, water and sodium nitrite solution is 0.032 mol:8 mL:4 mL:44 mL; the dosage ratio of 4-allyl-2-methoxyphenol, methanol, sodium carbonate and diazonium salt intermediate is 0.016 mol l: 110mL: 0.008mol: 0.016mol; the mass fraction of concentrated hydrochloric acid is 36.5%, and the concentration of sodium nitrite solution is 1mol / L;
[0042] Step A2: Add the reaction product a, ethanol and sodium hydroxide into a three-necked flask, heat to 70°C, start reflux stirring, then add sodium dithionite in three equal amounts, reflux stirring and react for 1.2 hours, cool to room temperature, add hydrochloric acid to adjust the pH to 5.5, filter, wash the filter cake with anhydrous ethanol, and dry to obtain the reaction product b; the amount ratio of the reaction product a, ethanol, sodium hydroxide and sodium dithionite is 0.1 mol: 145 mL: 0.035 mol: 0.15 mol; the amount of sodium dithionite is the sum of the three additions; the volume fraction of ethanol is 95%;
[0043] Step A3: Add perfluorooctanoic acid, diethylenetriamine and xylene into a three-necked flask, introduce nitrogen, start reflux stirring, heat to 145°C, reflux stirring and react at a constant temperature for 3.2 hours, then quickly heat to 200°C, reflux stirring and react at a constant temperature for 2.2 hours to obtain a reaction product c; the amount ratio of perfluorooctanoic acid, diethylenetriamine and xylene is 0.1 mol: 0.135 mol: 44 mL;
[0044] Step A4: Add the reaction product b, toluene and the reaction product c to a reaction flask, heat it to 140°C, and stir the mixture for 11 hours to obtain a reaction product d. Then add the reaction product d, benzyl chloride and n-propanol to a flask, heat it to 115°C, and stir the mixture for 6.5 hours to obtain a main corrosion inhibitor. The dosage ratio of the reaction product b, toluene and the reaction product c is 1.05 mol:750 mL:1.00 mol; the dosage ratio of the reaction product d, benzyl chloride and n-propanol is 1 mol:1.02 mol:900 mL.
[0045] Example 3
[0046] A main corrosion inhibitor, the preparation of which comprises the following steps:
[0047] Step A1: 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid and water are added to a flask, stirred at 30°C for 30 minutes, and then cooled to 0°C with an ice-water bath. Sodium nitrite solution is slowly added dropwise to the flask, stirred and reacted for 30 minutes to obtain a reaction solution, and urea is added until the reaction solution turns starch-potassium iodide test paper blue to obtain a diazonium salt intermediate; 4-allyl-2-methoxyphenol and methanol are then added to a three-necked flask, sodium carbonate is added to adjust the pH to 8.5, and the diazonium salt intermediate is slowly added dropwise under stirring in an ice-water bath, and the addition is completed within 60 minutes, and the reaction is continued with stirring for 2.5 hours to obtain a reaction product a; the dosage ratio of 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid, water and sodium nitrite solution is 0.032 mol:8 mL:4 mL:48 mL; the dosage ratio of 4-allyl-2-methoxyphenol, methanol, sodium carbonate and diazonium salt intermediate is 0.016 mol l: 120mL: 0.010mol: 0.016mol; the mass fraction of concentrated hydrochloric acid is 36.5%, and the concentration of sodium nitrite solution is 1mol / L;
[0048] Step A2: Add the reaction product a, ethanol and sodium hydroxide into a three-necked flask, heat to 75°C, start reflux stirring, then add sodium dithionite in three equal amounts, reflux stirring and react for 1.5 hours, cool to room temperature, add hydrochloric acid to adjust the pH to 6, filter, wash the filter cake with anhydrous ethanol, and dry to obtain the reaction product b; the amount ratio of the reaction product a, ethanol, sodium hydroxide and sodium dithionite is 0.1 mol:155 mL:0.05 mol:0.2 mol; the amount of sodium dithionite is the sum of the amounts added three times; the volume fraction of ethanol is 95%;
[0049] Step A3: Add perfluorooctanoic acid, diethylenetriamine and xylene into a three-necked flask, introduce nitrogen, start reflux stirring, heat to 150°C, reflux and react with constant temperature stirring for 3.5 hours, then quickly heat to 200°C, reflux and react with constant temperature stirring for 2.5 hours to obtain reaction product c; the dosage ratio of perfluorooctanoic acid, diethylenetriamine and xylene is 0.1 mol:0.15 mol:48 mL;
[0050] Step A4: Add the reaction product b, toluene and the reaction product c to a reaction flask, heat it to 145°C, stir and react at a constant temperature for 12 hours to obtain a reaction product d, then add the reaction product d, benzyl chloride and n-propanol to a flask, heat it to 120°C, stir and react at a constant temperature for 7 hours to obtain a corrosion inhibitor; the amount ratio of the reaction product b, toluene and the reaction product c is 1.05 mol:800 mL:1.00 mol; the amount ratio of the reaction product d, benzyl chloride and n-propanol is 1 mol:1.02 mol:950 mL.
[0051] Example 4
[0052] A high temperature resistant acidification corrosion inhibitor, comprising the following raw materials by weight: 40 parts of corrosion inhibitor, 10 parts of synergist, 1.5 parts of additive, 30 parts of gelling agent, 15 parts of weighting agent and 15 parts of porogen. The synergist is antimony trioxide; the additive is aminotri(methylenephosphonic acid) and sodium ethylenediaminetetra(methylenephosphonic acid) mixed in a mass ratio of 1:1; the gelling agent is polyvinyl alcohol; the weighting agent is barium sulfate; the porogen is 5-methylbenzotriazole;
[0053] The preparation of the high temperature resistant acidification corrosion inhibitor comprises the following steps:
[0054] The main corrosion inhibitor, synergist, additive, gelling agent, weighting agent and pore-forming agent obtained in Example 1 were mixed and stirred for 30 minutes, then transferred to an internal mixer and mixed at 140°C for 25 minutes, then cooled, crushed, and formed by an injection molding machine to obtain a high-temperature acidification-resistant corrosion inhibitor with the same diameter and height of 3 mm.
[0055] Example 5
[0056] A corrosion inhibitor for high temperature acidification, comprising the following raw materials by weight: 44 parts of corrosion inhibitor, 12 parts of synergist, 2.0 parts of additive, 33 parts of gelling agent, 16 parts of weighting agent and 16 parts of porogen. The synergist is antimony trioxide; the additive is aminotri(methylenephosphonic acid) and sodium ethylenediaminetetra(methylenephosphonic acid) mixed in a mass ratio of 1:1; the gelling agent is polyvinyl alcohol; the weighting agent is barium sulfate; the porogen is 5-methylbenzotriazole;
[0057] The preparation of the high temperature resistant acidification corrosion inhibitor comprises the following steps:
[0058] The main corrosion inhibitor, synergist, additive, gelling agent, weighting agent and pore-forming agent obtained in Example 2 were mixed and stirred for 35 minutes, then transferred to an internal mixer and mixed at 145°C for 30 minutes, then cooled, crushed, and formed by an injection molding machine to obtain a high-temperature acidification-resistant corrosion inhibitor with the same diameter and height of 4 mm.
[0059] Example 6
[0060] A high temperature resistant acidification corrosion inhibitor, comprising the following raw materials by weight: 48 parts of corrosion inhibitor, 15 parts of synergist, 2.5 parts of additive, 36 parts of gelling agent, 18 parts of weighting agent and 18 parts of porogen. The synergist is antimony trioxide; the additive is aminotri(methylenephosphonic acid) and sodium ethylenediaminetetra(methylenephosphonic acid) mixed in a mass ratio of 1:1; the gelling agent is polyvinyl alcohol; the weighting agent is barium sulfate; the porogen is 5-methylbenzotriazole;
[0061] The preparation of the high temperature resistant acidification corrosion inhibitor comprises the following steps:
[0062] The main corrosion inhibitor, synergist, additive, gelling agent, weighting agent and pore-forming agent obtained in Example 3 were mixed and stirred for 40 minutes, then transferred to an internal mixer and mixed at 150°C for 35 minutes, then cooled, crushed, and formed by an injection molding machine to obtain a high-temperature acidification-resistant corrosion inhibitor with the same diameter and height of 5 mm.
[0063] Comparative Example 1
[0064] This comparative example is a commercially available corrosion inhibitor for acidification.
[0065] Comparative Example 2
[0066] Compared with Example 6, the perfluorooctanoic acid used in the synthesis of the main corrosion inhibitor was replaced with octanoic acid, and the rest was exactly the same as Example 6 to prepare a high temperature acidification resistant corrosion inhibitor.
[0067] Comparative Example 3
[0068] Compared with Example 6, the 4-allyl-2-methoxyphenol used in the synthesis of the main corrosion inhibitor was replaced with 4-ethyl-2-methoxyphenol, and the rest was exactly the same as Example 6 to prepare a high temperature acidification resistant corrosion inhibitor.
[0069] Comparative Example 4
[0070] Compared with Example 6, a main corrosion inhibitor of imidazoline quaternary ammonium salt without triazole ring was synthesized using perfluorooctanoic acid, diethylenetriamine, acrylic acid and benzyl chloride as raw materials, and the main corrosion inhibitor synthesized in Example 6 was replaced to obtain a high temperature resistant acidification corrosion inhibitor.
[0071] The effect of the high temperature acidification resistant corrosion inhibitor disclosed in the present invention is further tested below, and the test results are as follows.
[0072] In order to test the high temperature resistant acidizing corrosion inhibitor disclosed in the present invention, the static corrosion rate at normal pressure and the dynamic corrosion rate at high temperature and high pressure were measured under different conditions with reference to the method in SY / T5405-2019 "Performance Test Method and Evaluation Method of Corrosion Inhibitor for Acidizing"; the water solubility was measured with reference to SY / T5273-2018 "Performance Index and Evaluation Method of Corrosion Inhibitor for Oilfield Produced Water"; the results are recorded in Table 1;
[0073] Condition 1: The acid solution is a hydrochloric acid solution with a mass fraction of 20%, the reaction time is 4 hours, the temperature is 90°C, the pressure is normal pressure, and the mass fraction of the corrosion inhibitor is 1.0%;
[0074] Condition 2: The acid solution is a hydrochloric acid solution with a mass fraction of 20%, the reaction time is 4 hours, the temperature is 180°C, the pressure is 16MPa, and the mass fraction of the corrosion inhibitor is 5.0%;
[0075] Table 1:
[0076]
[0077] According to the data in Table 1, compared with Comparative Example 1, Examples 4, 5 and 6 show that, compared with commercially available acidification corrosion inhibitors, the high temperature resistant acidification corrosion inhibitor disclosed in the present invention can better reduce the corrosion rate under high temperature and high pressure conditions, and has excellent corrosion inhibition performance. Compared with Comparative Example 2, Example 6 shows that the perfluoroalkyl chain makes the thermal stability of the corrosion inhibitor better and the hydrophobic film formed is more compact, which more effectively prevents hydrogen ions from approaching, reduces the corrosion rate, and improves the corrosion inhibition of the corrosion inhibitor; Compared with Comparative Example 3, Example 6 shows that the carbon-carbon double bond enhances the adsorption of the corrosion inhibitor to the metal and increases the solubility of the corrosion inhibitor in water, which is more conducive to reducing the corrosion rate and has better corrosion inhibition performance; Compared with Comparative Example 4, Example 6 shows that the triazole ring is added to the corrosion inhibitor molecule, the metal complexing point is increased, and it is not easy to desorb at high temperature, which reduces the corrosion rate and improves the corrosion inhibition.
[0078] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A high temperature resistant acidification corrosion inhibitor, characterized in that: The invention comprises the following raw materials in parts by weight: 40-48 parts of corrosion inhibitor, 10-15 parts of synergist, 1.5-2.5 parts of additive, 30-40 parts of gelling agent, 15-25 parts of weighting agent and 15-18 parts of porogen; The preparation of the main corrosion inhibitor comprises the following steps: Step A1: 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid and water are added to a flask, stirred at 30°C for 30 minutes, and then cooled to 0°C in an ice-water bath, and sodium nitrite solution is slowly added dropwise to the flask, and the reaction is stirred for 20-30 minutes to obtain a reaction solution, and urea is added until the reaction solution turns starch-potassium iodide test paper blue to obtain a diazonium salt intermediate; 4-allyl-2-methoxyphenol and methanol are then added to a three-necked flask, and sodium carbonate is added to adjust the pH to 7.5-8.
5. Under stirring in an ice-water bath, the diazonium salt intermediate is slowly added dropwise, and the addition is completed within 45-60 minutes, and the reaction is continued with stirring for 2-2.5 hours to obtain a reaction product a; Step A2: Add the reaction product a, ethanol and sodium hydroxide into a three-necked flask, heat to 65-75°C, start reflux stirring, then add sodium dithionite in three equal amounts, reflux stirring and react for 1-1.5h, cool to room temperature, add hydrochloric acid to adjust the pH to 5-6, filter, wash the filter cake with anhydrous ethanol, and dry to obtain the reaction product b; Step A3: Add perfluorooctanoic acid, diethylenetriamine and xylene into a three-necked flask, introduce nitrogen, start reflux stirring, raise the temperature to 140-150°C, reflux stirring and react at a constant temperature for 3-3.5 hours, then quickly raise the temperature to 200°C, reflux stirring and react at a constant temperature for 2-2.5 hours to obtain a reaction product c; Step A4: Add the reaction product b, toluene and the reaction product c to a reaction flask, heat it to 135-145°C, stir and react at a constant temperature for 10-12h to obtain the reaction product d, then add the reaction product d, benzyl chloride and n-propanol to a flask, heat it to 110-120°C, stir and react at a constant temperature for 6-7h to obtain the main corrosion inhibitor; The synergist is antimony trioxide; the additive is prepared by mixing aminotris(methylenephosphonic acid) and sodium ethylenediaminetetra(methylenephosphonic acid) in a mass ratio of 1:1; the gelling agent is polyvinyl alcohol; the weighting agent is barium sulfate; and the porogen is 5-methylbenzotriazole; In step A1, the dosage ratio of 4-amino-3-nitrobenzoic acid, concentrated hydrochloric acid, water, and sodium nitrite solution is 0.032 mol: 8 mL: 4 mL: 40-48 mL; the dosage ratio of 4-allyl-2-methoxyphenol, methanol, sodium carbonate, and diazonium salt intermediate is 0.016 mol: 100-120 mL: 0.005-0.010 mol: 0.016 mol; the mass fraction of concentrated hydrochloric acid is 36.5%, and the concentration of sodium nitrite solution is 1 mol / L; In step A2, the dosage ratio of reaction product a, ethanol, sodium hydroxide and sodium dithionite is 0.1 mol: 135-155 mL: 0.02-0.05 mol: 0.1-0.2 mol; the dosage of sodium dithionite is the sum of the three additions; the volume fraction of ethanol is 95%; In step A3, the usage ratio of perfluorooctanoic acid, diethylenetriamine and xylene is 0.1 mol: 0.12-0.15 mol: 40-48 mL; In step A4, the usage ratio of reaction product b, toluene and reaction product c is 1.05 mol:700-800 mL:1.00 mol; the usage ratio of reaction product d, benzyl chloride and n-propanol is 1 mol:1.02 mol:850-950 mL.
2. The method for preparing a high temperature resistant acidification corrosion inhibitor according to claim 1, characterized in that: The steps include: The main corrosion inhibitor, synergist, additive, gelling agent, weighting agent and pore-forming agent are mixed and stirred for 30-40 minutes, then transferred to an internal mixer and mixed at 140-150°C for 25-35 minutes, then cooled, crushed and formed by an injection molding machine to obtain a high temperature acidification resistant corrosion inhibitor with the same diameter and height of 3-5 mm.