A silicon carbide-coated diamond particle, its low-temperature preparation method and application

By preparing silicon carbide films on diamond surfaces through low-temperature heat treatment, the problem of high cost in high-temperature preparation was solved, and mass production of silicon carbide-coated diamond particles and performance improvement of composite materials were achieved at low temperatures.

CN118441262BActive Publication Date: 2026-11-17HUNAN INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410568197.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2026-11-17
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare micro- and nano-scale silicon carbide coatings on diamond surfaces at low temperatures. Furthermore, preparation at high temperatures is costly and prone to oxidation and graphitization. Traditional methods involve expensive equipment or high costs, making mass production difficult.

Method used

A low-temperature heat treatment method is used to introduce trimethylaluminum and a gaseous or liquid silicon source through an inert gas and react them at 600-1000℃ to prepare a silicon carbide film. A silicon carbide coating layer is formed on the diamond surface by chemical reaction, and the film thickness is controlled by controlling the reaction temperature and time.

Benefits of technology

This method enables the preparation of silicon carbide-coated diamond particles at temperatures below 1000℃, avoiding high-temperature oxidation, reducing costs, and facilitating mass production. It also improves the thermal conductivity and insulation properties of the composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118441262B_ABST
    Figure CN118441262B_ABST
Patent Text Reader

Abstract

A silicon carbide-coated diamond particle, its low-temperature preparation method, and its application are disclosed, relating to the field of diamond surface treatment technology. The preparation method includes the following steps: S1, placing diamond particles in a reaction vessel and introducing trimethylaluminum through an inert gas; S2, under continuous trimethylaluminum introduction, heating to 600-700°C and holding at this temperature for 0.1-4 hours; S3, stopping the supply of trimethylaluminum and directly introducing a gaseous silicon source or introducing a liquid silicon source through an inert gas; S4, further heating the temperature to 700-1000°C and holding at this temperature for 0.5-4 hours; S5, cooling to room temperature to form a silicon carbide film on the diamond surface. This invention enables the low-temperature preparation of silicon carbide-coated diamond particles, avoiding high-temperature oxidation and graphitization transformation of diamond, ensuring the intrinsic physical properties of diamond, and possessing advantages such as adjustable and controllable properties, low cost, high efficiency, mass production capability, and good repeatability. Furthermore, the silicon carbide, coated on the diamond particle surface through a chemical reaction, exhibits excellent adhesion strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of diamond surface treatment technology, and in particular to a method for preparing silicon carbide thin films at low temperature on diamond surfaces, silicon carbide-coated diamond particles, and their applications. Background Technology

[0002] Diamond's non-conductive properties and poor wettability with metals limit its application in metal matrix composites. Diamond surface coating technology can effectively address these issues. Studies have shown that different coating techniques and coatings have a significant impact on the performance of composite materials, especially for diamond-coated metal matrix composites used in electronic packaging. The choice of interface modification layer and the coating method directly determine the thermal conductivity of the composite material.

[0003] Silicon carbide (SiC), with its high hardness, strong wear resistance, high thermal conductivity, and low coefficient of thermal expansion, is an ideal coating material for diamond surfaces and can be used as an interface modification layer for diamond-based composite materials in electronic packaging. However, preparing micro / nano-scale silicon carbide coatings on diamond surfaces is not easy. For example, diamond and silicon powder require temperatures as high as 1400°C to react and form a silicon carbide layer, and even in a salt bath environment, temperatures as high as 1100°C are needed to form a silicon carbide layer on the diamond surface. These high temperatures not only increase preparation costs but also easily cause oxidation and graphitization of the diamond surface. While chemical vapor deposition (CVD) can prepare silicon carbide layers at lower temperatures, the equipment is expensive and the yield is low.

[0004] Silicon carbide layers can be prepared at lower temperatures by mixing diamond micropowder (15µm) with silicon powder and sintering under a specific atmosphere (sintering temperature of 1300℃), or by depositing an aluminum-silicon bilayer film by magnetron sputtering followed by annealing (temperature of 900℃). However, although the above methods reduce the synthesis temperature, the cost is still high, and they can usually only prepare nanoscale films. Summary of the Invention

[0005] One of the objectives of this invention is to provide a novel method for preparing silicon carbide thin films by low-temperature heat treatment on the surface of diamond.

[0006] To achieve the above objectives, the present invention employs the following approach: a method for preparing silicon carbide thin films at low temperatures on diamond surfaces, comprising the following steps: S1. Place diamond particles in a reaction vessel and introduce trimethylaluminum through an inert gas; S2. Under the condition of continuous introduction of trimethylaluminum, the temperature is raised to 600-700℃ and held for 0.1-4 hours; S3. Stop the supply of trimethylaluminum and directly introduce a gaseous silicon source or introduce a liquid silicon source through an inert gas; S4. Further raise the temperature to 700-1000℃ and maintain the temperature for 0.5-4 hours; S5. Cool to room temperature to form a silicon carbide film on the diamond surface.

[0007] In step S1, the reaction vessel can be a mesh tube inside a furnace tube. In step S2, before heating, a motor can be started to rotate the mesh tube (at a speed of 0.5-10 r / min, preferably 2 r / min), causing the diamond particles to tumble within it. The sidewall of the mesh tube is provided with several through holes to allow gas flow and prevent diamond particles from leaking out.

[0008] Furthermore, in step S3, the gaseous silicon source can be a gas that provides the silicon source, such as silane; the liquid silicon source can be a liquid compound that provides the silicon source, such as methyltrichlorosilane.

[0009] Further, in step S4, the reaction temperature is 800-1000℃. Preferably, it is 800-900℃, more preferably 800-850℃, and even more preferably 800℃ or 850℃.

[0010] Furthermore, in step S4, the thickness of the silicon carbide film is controlled by adjusting the holding time, thereby forming a silicon carbide film with a thickness of nanometer or micrometer on the diamond surface. For example, when the holding time is 0.5 hours, the thickness of the formed silicon carbide film is in the nanometer range (e.g., 145 nm); when the holding time is 4 hours, the thickness of the formed silicon carbide film is in the micrometer range (e.g., 2.63 μm).

[0011] Furthermore, in steps S1 and S2, the mass concentration of trimethylaluminum does not exceed 20%.

[0012] Furthermore, in steps S2 and S4, the temperature is increased at a rate of ≤15℃ / min.

[0013] Furthermore, in steps S1 and S3, hydrogen gas is introduced simultaneously with the introduction of an inert gas or a gaseous silicon source. The introduced hydrogen gas can promote the reduction reaction of aluminum and silicon, thereby improving the reaction efficiency and effect.

[0014] Furthermore, in step S1, the diamond particles have a particle size of 40-600 μm.

[0015] Another object of the present invention is to provide silicon carbide-coated diamond particles, which are prepared by the low-temperature preparation method described above.

[0016] In addition, the silicon carbide-coated diamond particles prepared by the above method can also be used in the preparation of diamond / silicon composite materials.

[0017] Among them, applying silicon carbide-coated diamond particles to prepare diamond / silicon composite materials can improve the thermal conductivity and electrical insulation properties of the composite materials. Silicon carbide, as a transition layer at the interface between diamond and silicon, plays an interfacial bonding role and improves the breakdown strength of diamond / silicon composite materials.

[0018] This invention utilizes the following chemical reaction characteristics to prepare silicon carbide-coated diamond particles through low-temperature heat treatment, and its main principle is as follows: The first step involves the decomposition of trimethylaluminum at low temperatures (200-300℃): Al(CH3)3(l) → CH4(g) + Al(s). The second step involves a combination reaction between aluminum and carbon atoms on the diamond surface at 650-700℃: 4Al(l) + 3C(s) → Al4C3(s). The third step (using silane as an example) involves the decomposition of silane above 700℃: SiH4(g) → 2H2(g) + Si(s). The fourth step involves a substitution reaction where silicon is deposited on the aluminum carbide surface: Al4C3(s) + 3Si(s) ⇋ 3SiC(s) + 4Al(l). The aluminum generated by this substitution almost completely evaporates at high temperatures, thus achieving the low-temperature preparation of silicon carbide-coated diamond particles. This method is simple, easy to operate, low-cost, highly efficient, and suitable for mass production with good repeatability.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The present invention can reduce the preparation temperature of silicon carbide to below 1000°C (the lowest temperature can be reduced to 700°C), and truly realize the low-temperature preparation of silicon carbide coated diamond particles.

[0020] (2) The low-temperature preparation method of the present invention can effectively avoid the high-temperature oxidation and graphitization transformation of diamond, thus ensuring the intrinsic physical properties of diamond.

[0021] (3) The silicon carbide film prepared by the present invention is adjustable and controllable, low in cost and high in efficiency. It can be mass-produced and has good repeatability. Furthermore, silicon carbide is coated on the surface of diamond particles by chemical reaction, which has good bonding strength and can be used for the development of high thermal conductivity and wear-resistant diamond composite materials.

[0022] (4) Applying the silicon carbide-coated diamond particles of the present invention to diamond / silicon composite materials can significantly improve the thermal conductivity and insulation properties of the composite materials. Attached Figure Description

[0023] Figure 1 This is a schematic diagram of the apparatus for low-temperature silicon carbide thin film preparation according to the present invention; Figure 2 This is an electron microscope image of the diamond surface morphology after heat treatment at 850°C for 1 hour in Example 1. Figure 3 The images shown are EDS, XRD and Raman spectra of the sample prepared in Example 3 by holding at a heat treatment temperature of 850℃ for 1 h. Among them, (a) is an electron microscope image of the diamond surface morphology, and (b), (c) and (d) are EDS, XRD and Raman spectra, respectively. Figure 4 The images shown are electron microscope images of the cross-sectional thickness of silicon carbide films prepared for different heat treatment times in Example 4. Figure 5 The XRD patterns of silicon carbide-coated diamond particles prepared at different heat treatment temperatures in Example 5 are shown below. Figure 6 The images shown are SEM images of silicon carbide-coated diamond particles prepared at different rotation speeds in Example 6.

[0024] In the picture: 1—Mixing System 1a—Mixing Chamber 1a1 - Air Inlet; 1b - Bubble Burner 2—Heating system 2a—Furnace tube 3—Rotating Tube System 3a—Mesh Tube 3b - Motor; 4 - Exhaust Gas Treatment System 4a - Alkali washing bottle; 4b - Distilled water bottle 5 — Pressure gauge 6 — Mechanical pump. Detailed Implementation

[0025] To facilitate understanding by those skilled in the art, the present invention will be further described below with reference to embodiments. The content mentioned in the embodiments is not intended to limit the present invention. It should be noted in advance that the following embodiments were completed in a laboratory. Those skilled in the art should understand that the amounts of each component given in the embodiments only represent the ratio between the components, and are not specific limitations.

[0026] The present invention aims to provide a new method for preparing silicon carbide thin films by low-temperature heat treatment on the surface of diamond, so as to achieve micro- and nano-tunable preparation of silicon carbide thin films on the surface of diamond.

[0027] First, this invention designs an apparatus for preparing silicon carbide thin films by low-temperature heat treatment on the surface of diamond. For example... Figure 1 As shown, the device mainly includes a gas mixing system 1, a heating system 2, a rotary tube system 3, and an exhaust gas treatment system 4.

[0028] The gas mixing system 1 mainly includes a mixing chamber 1a and a bubbler 1b (e.g., a bubble bottle). The mixing chamber 1a has several inlets 1a1 for the input of inert gases, hydrogen, etc., and is connected to the bubbler 1b via pipes. Typically, only inert gas needs to be introduced into the mixing chamber 1a. The inert gas passes through the bubbler 1b, carrying the organic compounds from the bubbler 1b into the rotating tube system 3. Alternatively, hydrogen can be introduced to promote the reduction reaction of aluminum and silicon, improving reaction efficiency and effectiveness. The inert gas may include one or more of nitrogen and argon. There may be two bubblers 1b, each containing an organic compound, including one or two of trimethylaluminum (usually liquid), silane (usually gaseous), and methyltrichlorosilane (usually liquid). When trimethylaluminum and silane are selected, one bubbler 1b can be filled with trimethylaluminum and the other with silane. However, since silane is gaseous, it can also be introduced from the inlet 1a1 of the mixing chamber 1a instead of being placed in bubbler 1b. When trimethylaluminum and methyltrichlorosilane are selected, they can be placed in two separate bubblers 1b. Furthermore, each bubbler 1b and its connected upstream and downstream pipelines can be equipped with on / off valves.

[0029] The rotating tube system 3 mainly includes a mesh tube 3a and an external motor 3b connected to it. The external motor 3b controls the rotation of the mesh tube 3a. The mesh tube 3a can be made of corundum or metal. The sidewall of the mesh tube 3a is provided with many through holes, and its structure is similar to a cylindrical / tubular sieve. The sieve holes (through holes) on the sidewall not only prevent diamond particles from leaking out, but also provide channels for gas to flow, so that trimethylaluminum, methyltrichlorosilane or silane carried by inert gas can enter the mesh tube 3a and fully contact the diamond particles therein, making the reaction more complete. Moreover, the rotating mesh tube 3a can make the diamond particles tumble in it, so that each side of the diamond particles can contact trimethylaluminum, methyltrichlorosilane or silane, thereby coating every area of ​​the diamond particle surface with a silicon carbide film and achieving uniform distribution.

[0030] The heating system 2 mainly includes a heating tube furnace, which comprises a furnace tube 2a and a heating device for heating the furnace tube 2a. A mesh tube 3a is installed in the furnace tube 2a and can rotate within it. One end of the furnace tube 2a is connected to two bubblers 1b via a pipeline and is equipped with a pressure gauge 5. The other end is connected to the exhaust gas treatment system 4 via a pipeline and is also connected to a mechanical pump 6. The pressure gauge 5 is used to monitor the gas pressure inside the tube, and the mechanical pump 6 is used to evacuate the device.

[0031] The exhaust gas treatment system 4 mainly includes an alkaline washing bottle 4a and a distilled water bottle 4b, and can perform combustion treatment at the end. The alkaline washing bottle 4a and the distilled water bottle 4b are connected in sequence to the other end of the furnace tube 2a, and an exhaust port is provided at the end of the pipe of the distilled water bottle 4b. During the experiment, the gas discharged from the exhaust port can be combusted.

[0032] Secondly, the present invention uses the above-mentioned apparatus to prepare a silicon carbide thin film by low-temperature heat treatment on the surface of diamond. The specific steps are as follows: 1. Load diamond particles into the mesh tube 3a, load organic compounds (e.g., trimethylaluminum; methyltrichlorosilane or silane) into the bubbling flask, connect the gas mixing system 1, the tubular furnace heating system 2, the rotary tube system 3, and the exhaust gas treatment system 4 in sequence, and perform vacuum treatment.

[0033] Prior to step one, a step of removing impurities from the raw diamond particles is included. Optionally, this impurity removal step includes: ultrasonically cleaning the diamond particles sequentially with acetone and ethanol.

[0034] Prior to this first step, the organic compound (mainly trimethylaluminum) is diluted. Optionally, the concentration of trimethylaluminum is diluted to below 20% using a hydrocarbon solvent or similar method. This is because higher concentrations of trimethylaluminum are generally hazardous, and dilution reduces this risk.

[0035] In this first step, the diamond particle size is 40-600 μm.

[0036] In this first step, a vacuum is drawn by a mechanical pump 6. Preferably, the vacuuming time is more than 30 minutes, and the vacuum level is 1-5 Pa.

[0037] 2. Open the valve to allow the inert gas in the mixing chamber 1a to pass through the bubble bottle containing trimethylaluminum and introduce it into the diamond particles. Turn on the motor 3b to rotate the mesh tube 3a and heat it to 600-700°C at a rate of ≤15°C / min, and hold it at this temperature for 0.1-4 hours. Then, close the switch of the bubble bottle containing trimethylaluminum (stop the supply of trimethylaluminum), open the bubble bottle containing methyltrichlorosilane or silane, or open the gas path containing silane, and introduce it into the diamond particles. Then heat it to 700-1000°C (preferably 800-1000°C, more preferably 800-850°C, and even more preferably 800°C or 850°C), and hold it at this temperature for 0.5-4 hours. After the holding period, close the bubble bottle (stop the supply of methyltrichlorosilane or silane), and cool it to room temperature. Finally, a uniform silicon carbide film is obtained on the diamond surface.

[0038] In step two, the flow rate of the bubbling bottle is controlled between 20 and 60 SCCM. Preferably, the flow rate is 45 SCCM.

[0039] In step two, the rotational speed of the mesh tube 3a is 0.5-10 r / min. Preferably, the rotational speed is 2 r / min.

[0040] In this invention, the silicon carbide-coated diamond particles are used to prepare diamond / silicon composite materials, which can improve the thermal conductivity and electrical insulation properties of the composite materials. Silicon carbide, as a transition layer at the interface between diamond and silicon, plays an interfacial bonding role and improves the breakdown strength of the diamond / silicon composite materials.

[0041] The above method enables controllable fabrication of silicon carbide films with thicknesses ranging from nanometers to micrometers, with the thickness range being 0.06-5 μm. Preferably, the thickness range of the silicon carbide film is 145 nm to 2.63 μm.

[0042] The following is an explanation through a specific experiment. Example 1

[0043] Cleaned diamond particles (200 μm in diameter) are placed in a mesh tube 3a. After processes such as vacuuming, ventilation, heating, and exhaust gas treatment, a thin film can be obtained on the surface of the diamond particles. Specifically, the device is evacuated using mechanical pump 6. Then, the valve is opened, allowing the inert gas (argon in this embodiment) from mixing chamber 1a to pass through the bubbling flask containing trimethylaluminum and into furnace tube 2a and mesh tube 3a. Motor 3b is then turned on, causing mesh tube 3a to rotate. The temperature is then increased to 600-700℃ (600℃ in this embodiment) at a rate of ≤15℃ / min (15℃ / min in this embodiment), and held for 0.1-4 h (2 hours in this embodiment). Subsequently, the bubbling flask containing trimethylaluminum is closed (stopping the supply of trimethylaluminum), and the bubbling flask containing silane is opened, increasing the temperature to 700-1000℃ (850℃ in this embodiment), and held for 0.5-4 h (1 hour in this embodiment). The mesh tube 3a rotates at 2 r / min. After the holding period, the bubbling flask is closed (stopping the silane supply), and the device is cooled to room temperature, resulting in a thin film on the surface of the diamond particles. In addition, the residual gas in the furnace tube 2a can be discharged from the exhaust port at the end of the pipeline through the alkaline washing bottle 4a and the distilled water bottle 4b, and then subjected to combustion treatment.

[0044] In this embodiment, the surface morphology of the diamond is as follows: Figure 2 As shown in the figure, the diamond particles are uniformly coated with a thin film, and no plating defects were found. Example 2

[0045] In this embodiment, the silane in Example 1 was replaced with methyltrichlorosilane, while other process conditions remained the same as in Example 1. A thin film was also observed on the surface of the diamond particles by examining the diamond surface morphology. Example 3

[0046] The sample from Example 1 was characterized by EDS, XRD, and Raman spectroscopy. The characterization results are as follows: Figure 3 As shown in the figure. EDS results indicate that the film is mainly composed of Si and C elements, with an atomic ratio of approximately 1:1. XRD patterns show that the film exhibits typical silicon carbide diffraction peaks. Raman spectroscopy also detected peaks in the silicon carbide film at 794 cm⁻¹. -1 and 966 cm -1 The Raman shift peak at the diamond surface is observed. These results indicate that silicon carbide thin films can be successfully prepared on diamond surfaces through low-temperature heat treatment using this method. Example 4

[0047] By controlling the heat treatment time, silicon carbide films ranging from nanometer to micrometer scale can be obtained. The heat treatment time after stopping the supply of trimethylaluminum was set to 0.5 h, 2 h, and 4 h, with other process parameters the same as in Example 1. Silicon carbide-coated diamond particles prepared by the 0.5 h and 4 h heat treatment processes were taken, and the coating thickness was characterized. The cross-sectional morphology is shown below. Figure 4 As shown, the silicon carbide thin film prepared by heat treatment for 0.5 h has a thickness of approximately 145 nm. Figure 4 As shown in (a) and 4(b), the thickness of silicon carbide prepared by 4 h heat treatment can reach 2.63 μm, as... Figure 4 As shown in (c) and 4(d), the above results demonstrate that micro / nano tunable silicon carbide coatings can be prepared using the method of the present invention. Example 5

[0048] The heat treatment temperatures after stopping the supply of trimethylaluminum were set to 600℃, 700℃, 800℃, 850℃, 900℃, and 1000℃, with other process parameters the same as in Example 1. The XRD results of the silicon carbide-coated diamond particles prepared at different heat treatment temperatures are shown below. Figure 5 As shown in the figure, the test results indicate that a silicon carbide coating cannot be prepared at a heat treatment temperature of 600℃, and only aluminum diffraction peaks were detected. However, at temperatures above 700℃, a silicon carbide coating can be obtained on the diamond surface, indicating that the heat treatment temperature has a significant impact on the preparation of the silicon carbide coating. Example 6

[0049] The rotational speed of the mesh tube 3a was set to 0.5, 2, 4, and 8 r / min, while other process parameters remained the same as in Example 1. The surface morphology of the silicon carbide-coated diamond particles prepared under different rotational speed conditions is shown below. Figure 6As shown in the SEM image, at 2 r / min, the silicon carbide film is uniform and dense. However, as the rotation speed increases, the quality and surface smoothness of the film deteriorate. Example 7

[0050] Two silicon carbide coatings of different thicknesses on the surface of the diamond particles from Example 4 were used to prepare diamond / silicon composite materials. The melting temperature was 1450℃, and the holding time was 10 min. Subsequently, the thermal diffusivity, density, and specific heat capacity of the samples were measured. Calculations showed that the composite material with a silicon carbide layer thickness of 145 nm achieved a thermal conductivity of 340 W·m. -1 ·K -1 The composite material with a silicon carbide layer thickness of 2.63 μm has a higher thermal conductivity, reaching 429 W·m. -1 ·K -1 In contrast, a composite material was prepared using pristine diamond particles and pure silicon. The thermal conductivity of the pristine diamond / silicon composite was measured to be 278 W·m. -1 ·K -1 This demonstrates that the silicon carbide-coated diamond particles prepared using the present invention have a significant advantage in improving the thermal conductivity of composite materials.

[0051] The above embodiments are preferred implementations of the present invention. In addition, the present invention can be implemented in other ways. Any obvious substitutions without departing from the concept of the present technical solution are within the protection scope of the present invention.

[0052] Finally, it should be emphasized that, in order to make it easier for those skilled in the art to understand the improvements of the present invention compared with the prior art, some descriptions of the present invention have been simplified, and for clarity, some other elements have been omitted from this application. Those skilled in the art should realize that these omitted elements can also constitute the content of the present invention.

Claims

1. A method for low temperature preparation of silicon carbide thin film on a diamond surface, characterized by, Includes the following steps: S1. Place diamond particles in a reaction vessel and introduce trimethylaluminum through an inert gas; S2. Under the condition of continuous introduction of trimethylaluminum, the temperature is raised to 600-700℃ and held for 0.1-4 hours, and the diamond particles are tumbled in the reaction vessel. S3. Stop the supply of trimethylaluminum and directly introduce a gaseous silicon source or introduce a liquid silicon source through an inert gas; S4. Further raise the temperature to 700-1000℃ and maintain the temperature for 0.5-4 hours; S5. Cool to room temperature to form a silicon carbide film on the diamond surface; In step S4, the thickness of the silicon carbide film is controlled by adjusting the heat preservation time, thereby forming a nano- or micro-scale silicon carbide film on the diamond surface.

2. The method of claim 1, wherein the method is characterized by: In step S3, the gaseous silicon source is silane, and the liquid silicon source is methyltrichlorosilane.

3. The method for preparing a silicon carbide thin film on a diamond surface at a low temperature according to claim 1, characterized in that: In step S4, the reaction temperature is 800-1000℃.

4. The method for preparing a silicon carbide thin film on a diamond surface at a low temperature according to claim 1, wherein: In steps S1 and S2, the mass concentration of trimethylaluminum does not exceed 20%.

5. The method for preparing a silicon carbide thin film on a diamond surface at a low temperature according to claim 1, wherein: In steps S2 and S4, the temperature is increased at a rate of ≤15℃ / min.

6. The method for preparing silicon carbide thin films at low temperature on diamond surfaces according to claim 1, characterized in that: In steps S1 and S3, hydrogen gas is introduced at the same time as an inert gas or a gaseous silicon source.

7. The method for preparing silicon carbide thin films at low temperature on diamond surfaces according to claim 1, characterized in that: In step S1, the diamond has a particle size of 40-600 μm.

8. A silicon carbide-coated diamond particle, characterized in that: It is prepared by the method described in any one of claims 1-7.

9. The application of the silicon carbide-coated diamond particles according to claim 8 in the preparation of diamond / silicon composite materials.

Citation Information

Patent Citations

  • Preparation method of silicon carbide coated diamond composite material, and diamond / aluminum composite material

    CN111732100A

  • Crystalline aluminum carbide thin film, semiconductor substrate having the aluminum carbide thin film formed thereon and method of fabricating the same

    US20120193640A1