A method for continuously producing ultra-fine fiber filaments
By combining the electrostatic field and the air flow field at the spinneret to form a melt jet, and using a static eliminator to neutralize the static charge of the fiber, the problem in the existing technology that ultrafine fiber filaments cannot be continuously prepared and stably wound is solved, and the It achieves efficient fiber bundling and drafting, improving fiber strength and unwinding speed.
Patent Information
- Application Number
- CN202410904138.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-08
AI Technical Summary
It is difficult to continuously prepare ultrafine fiber filaments with a diameter of less than 4 μm using existing technology, and cannot be wound up and unwound stably for a long time. The fiber strength is low, easy to break, and electrostatic adsorption leads to serious fiber adhesion and overlapping.
After heating and melting extrusion using a screw extruder, it is transported to the spinneret through a micro metering pump. The spinneret hole forms a melt jet under the action of the electrostatic field and air flow field. The rotating air flow is twisted and bundled, and neutralized using a static eliminator. The fiber surface is electrostatically charged, followed by oiling and hot roller drafting to achieve continuous winding of the fiber.
It has realized the continuous production of ultra-fine fiber filaments with a single filament diameter of 1~3μm, and can unwind normally, with an unwinding speed of more than 300m/min. The fiber strength is improved, the stability and continuity are greatly improved, and the electrostatic adsorption is avoided. adhesion problem.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical fiber manufacturing and relates to a continuous production method of ultra-fine fiber filaments. Background Art
[0002] In the textile industry, the fineness of a fiber is one of the important indicators for measuring its performance and application range. In my country's textile industry, fibers with a single filament fineness of less than 0.44 dtex are defined as ultrafine fibers.
[0003] Among the production methods of ultrafine fibers, direct spinning (i.e., the method of directly spinning polymer melt or solution made by polymerization) is the simplest, but it is difficult to spin fiber filaments below 0.55 dtex. The existing technology uses continuous polymerization direct spinning technology to achieve the industrial production of ultrafine fibers with a single fiber linear density of 0.15~0.50 dtex (diameter 4~7μm).
[0004] For example, patent CN202410081226.2 (a method for preparing porous ultra-fine denier nylon 6FDY by side-blowing) adopts a distributed arrangement of the melt pipe design in the melting section, that is, multiple branch pipes are evenly arranged, the melt pipe length is 9.5m, the residence time of the melt in the pipe is 10min, the pressure loss is 7~8MPa, and the flow rate and pressure of the melt are ensured to be consistent; a melt static mixer is installed at the elbow of the melt pipe; a buffer is installed at the melt outlet, and the temperature of the slow cooler is 255~265℃; the difference between the cold roller speed and the speed of the melt ejected from the spinneret forms the spinneret draft, and the draft multiple DR1 is set to 800~900; the hot roller draft DR2 is set to 1.05~1.07, and the hot roller temperature is set to 175~180℃. This patent enables the production of nylon 6 fiber with a dpf less than 0.3dtex (about 6μm), but the single fiber diameter is still relatively thick, much larger than 4μm.
[0005] Composite spinning technology is currently the most widely used and studied method for preparing ultrafine fibers. This method can reduce the diameter of the fiber to a certain extent through composite spinning of two or more polymers. For example, patent CN202010644575.2 (a sea island fiber with PET as the island component, its preparation method and ultrafine fibers formed therefrom), patent CN 202010644732.X (a sea island fiber with PP as the island component, its preparation method and ultrafine fibers formed therefrom) and patent CN 202010644747.6 (a sea island fiber with PA6 as the island component, its preparation method and ultrafine fibers formed therefrom) all use modified copolyester as the sea component, and PET, PP and PA6 as the island components of the sea island fiber. However, this method cannot directly and continuously prepare ultrafine fiber filaments, but requires the spun fibers to be re-opened after winding, and the sea part of the sea island fiber is dissolved by a solvent, leaving the island part. The preparation process is complicated, and the performance of the ultrafine fiber is easily damaged.
[0006] In order to solve the problem that the above-mentioned ultrafine fiber filaments cannot be continuously prepared, patent CN 114134580A discloses an electrostatic spinning ultrafine fiber bundling system and method, including a coaxially arranged spinning nozzle and a bundling disk, the spinning nozzle is arranged on the upper part of the bundling disk, the bundling disk is connected to the motor through a coupling, the motor rotates to drive the bundling disk to rotate, and a guide groove is also arranged on the outside of the bundling disk; an axis is arranged at the center of the bundling disk, and the insulating outer ring, the central conductive ring, the insulating inner ring and the axis are fixed by bonding or thermal bonding; the inner and outer edges of the central conductive ring are smooth arc fillets, and the inner edge of the insulating outer ring and the outer edge of the insulating inner ring are corresponding smooth inner fillets. A carbon brush body is arranged at the lower end of the bundling disk, the carbon brush body is fixed on the carbon brush bracket, and the graphite block in the carbon brush body is close to the bottom of the central conductive ring of the bundling disk under the action of the spring, and the graphite block is connected to the high-voltage electrostatic generator arranged outside through a wire. This patent can improve the stability and uniformity of electrospinning fiber bundling, but this patent mainly receives the fibers through a bundling disk and then reels them up. This process has a slow reeling speed and insufficient fiber orientation.
[0007] Patent CN 202310995651.8 discloses a melt electrospinning device and a method for preparing nanofiber filaments using the same. The melt electrospinning device includes a spinneret, the bottom of the spinneret is an inverted truncated cone structure, and the lower surface of the bottom is provided with a groove and a spinneret outlet distributed around the groove; the groove is a conical structure, the small end of the inverted truncated cone structure and the bottom surface of the conical structure are coplanar, and the spinneret is a capillary structure; the diameter of the spinneret outlet or the equivalent circular diameter is 0.06~0.8mm; the distance a between the spinneret outlet and the small end edge of the inverted truncated cone structure does not exceed 4mm, and the distance b between the spinneret outlet and the bottom edge of the conical structure does not exceed 4mm; when the aforementioned melt electrospinning device is used to prepare nanofiber filaments, the spinning pressure is 0.2~1MPa, and the feed rate of the micro multi-screw extruder is 0.2~0.8kg / h. This patent solves the problem of the stability of the melt jet formed by the nozzle, reduces the fiber breakage rate and stiffness, but only solves the problem of poor stability of floating silk caused by the dripping of melt from the nozzle during the spinning process from the perspective of nozzle structure design. It does not solve the problem of subsequent continuous winding and unwinding of the fiber bundle. It only performs simple winding, with a stabilization time of less than 40 minutes. The fiber strength is not high, and it is easy to break during the weaving process. There is a strong electrostatic effect between the fibers, and the fibers are seriously adsorbed and overlapped, making it impossible to unwind normally.
[0008] In summary, although the existing technology is able to prepare ultrafine fibers to a certain extent, fibers with a diameter less than 4 μm cannot be stably wound for a long time or unwound normally.
[0009] Therefore, it is of great significance to study a continuous production method of ultrafine fiber filaments to solve the problems existing in the prior art. Summary of the invention
[0010] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for continuously producing ultrafine fiber filaments.
[0011] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0012] A continuous production method for ultrafine fiber filaments, firstly, a polymer is heated and melted and extruded through a screw extruder, and then transported to a spinneret through a micrometering pump, and the melt extruded through the spinneret hole is sprayed downward under the action of an electrostatic field and an airflow field, and then the sprayed fiber filaments are twisted and bundled under the action of a rotating airflow, and the twisted and bundled fiber filaments are then passed through an internal hollow static eliminator to eliminate static charges on the surface of the fiber filaments caused by friction with the air, and then the fiber filaments after the surface static charges are eliminated are oiled and hot roller stretched in sequence, and finally the stretched filament bundles are wound to obtain ultrafine fiber filaments;
[0013] The single filament diameter of the ultrafine fiber filament is 1~3μm (0.02~0.08dtex), the continuous winding time is not less than 1h, and it can be unwound normally (that is, the fiber is not damaged or stretched during the unwinding process), and the unwinding speed is above 300m / min;
[0014] The air flow pressure during twisting and bundling is 0.3~0.9MPa, and the twisting air flow rate is 600~1200L / min.
[0015] When the airflow pressure is higher than 0.9MPa, the pressure is too high and the fibers are easily broken by the high-pressure gas; when the airflow pressure is lower than 0.3MPa, the pressure is too low and the fiber twisting is insufficient, and the fibers are intermittently dispersed and not held together. When the twisting airflow is greater than 1200L / min, the airflow on the fiber path is too large, the bundle of fibers shakes severely, the spinning stability is poor, and the fibers are prone to breakage; when the twisting airflow is less than 600L / min, the airflow is too small and the gas velocity in the airflow field below the spinneret is too small, and the fibers are easily accumulated in the rotating airflow generator and cannot be continuous.
[0016] As the preferred technical solution:
[0017] In the continuous production method of ultrafine fiber filaments as described above, the polymer is one or more of polypropylene, polyethylene, polyester, liquid crystal polyester, polylactic acid, polyamide, polyoxymethylene, polycarbonate, polyphenylene ether, polysulfone, polyetheretherketone, polyphenylene sulfide, polyimide and polyetherimide.
[0018] In the continuous production method of ultrafine fiber filaments as described above, the screw extruder is a single-screw extruder, the speed of the single-screw extruder is 5-20r / min, the diameter is 8-35mm, and the aspect ratio is 15-26:1.
[0019] In the continuous production method of ultrafine fiber filaments as described above, the processing temperature of the screw extruder is 180~360℃.
[0020] In the continuous production method of ultrafine fiber filaments as described above, the number of spinnerets of the spinneret is 100-300, the diameter of the spinnerets is 0.08-0.5 mm, and the spacing between adjacent spinnerets is 0.8-2 mm.
[0021] For the production of fiber filaments with a monofilament diameter of 1 to 3 μm, the extrusion amount of raw materials is small and the spinneret hole is small. The spinneret used in the present invention has a specification of 100 to 300 holes, a hole diameter of 0.08 to 0.5 mm, and a spacing of 0.8 to 2 mm between adjacent spinneret holes. Under this condition, the melt cannot continuously form a jet at the spinneret hole, and continuous spinning is impossible. Usually, high pressure extrusion is required, and the extrusion amount of the melt is large, resulting in the inability of the prior art to make the fiber diameter thinner at the same speed.
[0022] The continuous production method of ultrafine fiber filaments as described above has a single hole extrusion amount of ≤0.016G / min and an extrusion pressure of ≤1.5MPa. The method of the present invention controls the melt extrusion amount to perform micro-extrusion under the action of the electrostatic field and the airflow field, so that the pressure of the polymer melt at the spinneret hole is ≤1.5MPa, and forms a melt filament bundle through the synergistic action of the electrostatic field and the airflow field. The melt forms droplets at the spinneret hole under low pressure, and under the action of the electric field, charge accumulation is formed on the surface of the polymer melt, and the polymer melt is stretched along the direction of the electric field line. At the same time, the airflow field assists in drawing the filament bundle, so that the polymer melt can be continuously and stably filamented after exiting the spinneret hole.
[0023] In the continuous production method of ultrafine fiber filaments as described above, the electrostatic field is applied from bottom to top, and the electric field strength is 120~600kV / m; the airflow field is applied from top to bottom to pull the fiber downward, the gas flow rate of the airflow field is 0.4~5m / s, and the airflow temperature is 20~150℃.
[0024] The electric field is formed by setting a positive electrode plate under the nozzle. The upper nozzle is grounded, that is, at zero potential. The direction of the electric field is from bottom to top. The melt is affected by the electric field at the nozzle, the surface charge is polarized, and it is attracted by the positive charge below to form a melt jet downward. Therefore, the direction of the electric field is opposite to the direction of the airflow field.
[0025] In the method for continuously producing ultrafine fiber filaments as described above, the static eliminator includes a hollow cylindrical shell, a plasma generator and a fan;
[0026] The hollow cylindrical shell is provided with a plurality of radial through holes, and a plasma generator is arranged in the through holes near the inner wall of the hollow cylindrical shell to generate positive ions or negative ions;
[0027] The fan is arranged on the outside of the hollow cylindrical shell and is used to generate wind force to blow the positive ions or negative ions generated by the plasma generator to the surface of the fiber filaments to neutralize the static charge on the fiber surface.
[0028] Due to the particularity of fiber fineness, the specific surface area of ultrafine fibers is relatively large, so they will carry charges when in contact with air and guide rollers, thereby generating an electrostatic effect and static electricity accumulation, resulting in higher adsorption capacity and activity, making it easy to adhere to the guide roller and wind around, making it difficult to wind up; at the same time, the same charges between single fibers repel each other, which is not conducive to fiber bundling.
[0029] As the fiber moves downward, it passes through the cavity inside the hollow cylindrical shell, and the air is ionized into a large number of positive ions or negative ions by a plasma generator. Wind then blows a large number of negative ions or positive ions onto the fiber surface to neutralize static electricity, thereby eliminating static electricity on the surface of the ultrafine fiber.
[0030] As described above, in a continuous production method of ultrafine fiber filaments, hot roller drawing includes three stages of hot drawing, the first stage hot drawing temperature is 60~150℃, and the drawing multiple is 1.1~2 times; the second stage hot drawing temperature is 75~200℃, and the drawing multiple is 1.2~2 times; the third stage hot drawing temperature is 90~300℃, and the drawing multiple is 1.2~2 times.
[0031] Principle of the invention:
[0032] After the fiber forms a jet, it needs to be bundled and wound. The existing technology usually uses a suction gun to assist in oiling and bundling the fiber. However, for the fiber with a smaller monofilament diameter prepared by the present invention, the existing technology cannot perform oiling and bundling. The reasons are: 1. The fiber diameter is thin and the strength is low, so the suction gun cannot collect it; 2. The fiber surface is charged, the fiber is dispersed, and the adhesion is poor. At the same time, the collection of charged fiber surface poses a threat to human safety; 3. The dispersed fiber monofilament has a thin diameter and low strength. When passing through the oil nozzle during the oiling process, the liquid adhesion of the oil will easily break the fiber. The existing spinning technology cannot directly oil and bundle it. In addition, the friction between the fiber and the roller surface is prone to cause static electricity accumulation, causing the ultrafine fiber to adsorb the roller surface of the guide roller. The existing technology cannot continuously reel and unwind the fiber with a monofilament diameter of 1~3μm for a long time.
[0033] In view of the above problems, the present invention proposes an innovative spinning process, which effectively solves the key problems in the spinning, winding and unwinding processes of ultrafine fibers. Specifically, in the spinning process, multiple ultrafine fibers are bundled and embraced by air twisting, and multiple ultrafine fibers are introduced into an air generator. With the help of air flow, the fibers are fully in contact with the air and rotate rapidly to form a tightly interwoven rotating fiber flow bundle. With the continuous rotation and interweaving of the fibers, entanglement is formed between single fibers, and finally a low-degree spiral fiber bundle is formed. In order to solve the problem that ultrafine fibers adhere to the surface of the guide roller due to electrostatic adsorption during the winding process, the present invention uses an electrostatic eliminator to pre-treat the fiber filaments after twisting and bundling to eliminate the static charge on the fiber surface. Because the present invention bundles and holds multiple ultrafine fibers together by air twisting, and eliminates the static charge generated by the friction between the fibers and the air during the electrospinning process and the bundling process, after the multiple ultrafine fibers are held together, the overall strength of the fiber bundle is improved, and subsequent spinning processes such as oiling, drawing, and winding can be carried out continuously. The industrial winding head can be used for continuous winding for more than 1 hour, and the continuous stability is greatly improved. At the same time, after the static electricity is eliminated, the fibers are fully held together by oiling, and the filament bundles will not adhere to each other due to static electricity and cannot be unwound, so normal unwinding is achieved, and the unwinding speed is more than 300m / min.
[0034] Beneficial effects:
[0035] The method for continuous production of ultrafine fiber filaments of the present invention solves the problem in the prior art that ultrafine fibers with a monofilament diameter of less than 4 μm cannot be effectively oiled, bundled and rolled, and can achieve continuous production of ultrafine fiber filaments with a monofilament diameter of 1 to 3 μm. It has broad application prospects and potential advantages, and will bring new opportunities for the production of ultrafine fibers and the development of related fields. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0037] The test methods involved in the performance indicators in the embodiments and comparative examples of the present invention are as follows:
[0038] Breaking strength and breaking elongation: The ultrafine fiber filaments were measured according to GB / T 14344-2008 standard, where the stretching speed was 500 mm / min.
[0039] Fiber diameter: Observe under a scanning electron microscope and measure the average diameter of 10 fibers in the same photo.
[0040] Linear density: ultrafine fiber filaments are measured according to GB / T 4743-1995 standard, where the skein length is 200m and weighed using method 1 of 8.3.1.
[0041] Example 1
[0042] A method for continuously producing ultrafine fiber filaments, the specific steps are as follows:
[0043] (1) Polypropylene (manufacturer: Sinopec, brand: T30S) was melt-extruded at 280°C through a single screw extruder at a rotation speed of 8 r / min, and then transported to a spinneret through a micro metering pump; wherein, the diameter of the single screw extruder was 12 mm, and the aspect ratio of the single screw extruder was 18:1;
[0044] (2) After the melt transported to the spinneret is extruded through the spinneret hole, it is sprayed downward under the action of the electrostatic field and airflow field applied from bottom to top; wherein, the number of spinneret holes of the spinneret is 150, the diameter of the spinneret hole is 0.2 mm, and the spacing between adjacent spinneret holes is 0.8 mm; the single hole extrusion amount of the spinneret is 0.01 G / min, and the extrusion pressure is 1.3 MPa; the electric field strength of the electrostatic field is 300 kV / m, the gas flow rate of the airflow field is 0.8 m / s, and the airflow temperature is 20 °C;
[0045] (3) The fiber filaments ejected through the electrostatic field and the airflow field are twisted and bundled under the action of the rotating airflow. The twisted and bundled fiber filaments are then passed through the internal hollow static eliminator to eliminate the negative charge generated on the surface of the fiber filaments due to friction with the air; wherein, the airflow pressure during twisting and bundling is 0.3MPa, and the twisting airflow is 1000L / min;
[0046] The static eliminator includes a hollow cylindrical shell, a plasma generator and a fan;
[0047] The inner wall of the hollow cylindrical shell is provided with 32 through holes evenly distributed in the radial direction, and a plasma generator is respectively arranged in each through hole near the inner wall of the hollow cylindrical shell to generate positive ions;
[0048] The fan is arranged outside the hollow cylindrical shell and is used to generate wind force to blow the positive ions generated by the plasma generator to the surface of the fiber filaments;
[0049] (4) The fiber filaments after eliminating the surface static charge are sequentially oiled and three-stage hot roller drawing, and finally the drawn filament bundles are wound to obtain ultrafine fiber filaments; wherein the first stage hot drawing temperature is 60°C and the drawing ratio is 1.5 times; the second stage hot drawing temperature is 80°C and the drawing ratio is 2 times; the third stage hot drawing temperature is 100°C and the drawing ratio is 2 times.
[0050] The final ultrafine fiber filament has an average single filament diameter of 2 μm, a continuous winding time of 2 h, and can be unwound normally at an unwinding speed of 300 m / min; the ultrafine fiber filament has a linear density of 10 dtex, a breaking strength of 1.4 cN / dtex, and an elongation at break of 22%.
[0051] Comparative Example 1
[0052] A method for continuous production of fiber filaments is basically the same as that of Example 1, except that: step (4) is not performed, and step (3) is to bundle the fiber filaments ejected through the electrostatic field and the airflow field through a bundling disk, and then pass the bundled fiber filaments through an internal hollow static eliminator to eliminate the static charge generated on the surface of the fiber filaments due to friction with the air, and finally the filament bundle after the static charge is eliminated is wound to obtain fiber filaments.
[0053] The average single-filament diameter of the fiber filament finally obtained is 6 μm; the linear density of the fiber filament is 250 dtex, the breaking strength is 0.4 cN / dtex, and the breaking elongation is 47%.
[0054] By comparing Comparative Example 1 with Example 1, it can be seen that the fiber filaments prepared in Comparative Example 1 have a larger linear density, reduced breaking strength, high breaking elongation, and poor fiber uniformity. This is because the fiber filaments produced in Comparative Example 1 are only bundled by a bunching disk, and are not subsequently stretched by a hot roller, resulting in low crystallinity and poor strength of the fiber filaments, and the prepared fiber filaments have a larger linear density; in addition, the fiber filaments that have not been stretched and shaped have low fiber strength, and are easily pulled off the bunching disk if the speed is too fast during winding, while being too slow will cause the fiber filaments to stack.
[0055] In the above-mentioned continuous production method of fiber filaments, if the filament bundle after eliminating static charge is first subjected to three-stage hot roller drawing as in step (4) of Example 1 (the process parameters of the three-stage hot roller drawing are the same as those of Example 1), since the force applied to each fiber on the bunching disk is inconsistent when bundling is performed using a bunching disk, some fibers in the bundle will break during the drawing process, and some fibers will not be fully drawn, resulting in poor drawing stability of the fibers and failure to be smoothly wound up.
[0056] Comparative Example 2
[0057] A method for producing ultrafine fiber filaments is basically the same as that of Example 1, except that in step (3), after twisting and bundling, no static eliminator is used to eliminate the static charge on the surface of the fiber filaments caused by friction with the air, and step (4) is directly performed.
[0058] Since no static eliminator is used to eliminate the static charge on the fiber surface after twisting and bundling, the fibers with static charge on the surface cannot be bundled and pulled using a suction gun, making subsequent processing difficult.
[0059] By comparing Comparative Example 2 with Example 1, it can be seen that it is difficult to achieve stable and continuous production of fibers in Comparative Example 2. This is because during the spinning process, the fiber filaments are subjected to charge accumulation in the electric field and charge accumulation caused by high-speed friction with the air. These charge accumulations make the fiber surface charged. Due to electrostatic adsorption, the fibers are more likely to adhere to the surfaces of the equipment in contact with them, such as the guide disk and winding roller in the spinning process. Especially when the fiber diameter is smaller, the electrostatic adsorption effect will become more significant, further aggravating the adhesion problem between the fiber and the surface of the contact object, and ultimately resulting in the inability to stably and continuously produce the fibers.
[0060] Example 2
[0061] A method for continuously producing ultrafine fiber filaments, the specific steps are as follows:
[0062] (1) Polyester (manufacturer: Jiangsu Shenghong Group Co., Ltd., brand: semi-matte PET, viscosity: 0.6 dL / g) was melt-extruded at 290°C through a single screw extruder at a rotation speed of 5 r / min, and then transported to a spinneret through a micro metering pump; wherein, the diameter of the single screw extruder was 20 mm, and the aspect ratio of the single screw extruder was 24:1;
[0063] (2) After the melt transported to the spinneret is extruded through the spinneret hole, it is sprayed downward under the action of the electrostatic field and airflow field applied from bottom to top; wherein, the number of spinneret holes of the spinneret is 150, the diameter of the spinneret hole is 0.5 mm, and the distance between adjacent spinneret holes is 2 mm; the single hole extrusion amount of the spinneret is 0.012 G / min, and the extrusion pressure is 1 MPa; the electric field strength of the electrostatic field is 180 kV / m, the gas flow rate of the airflow field is 4 m / s, and the airflow temperature is 80 °C;
[0064] (3) The fiber filaments ejected through the electrostatic field and the airflow field are twisted and bundled under the action of the rotating airflow. The twisted and bundled fiber filaments are then passed through the internal hollow static eliminator to eliminate the negative charge generated on the surface of the fiber filaments due to friction with the air; wherein, the airflow pressure during twisting and bundling is 0.7MPa, and the twisting airflow is 800L / min;
[0065] The static eliminator includes a hollow cylindrical shell, a plasma generator and a fan;
[0066] The inner wall of the hollow cylindrical shell is provided with 16 through holes evenly distributed in the radial direction, and a plasma generator is respectively arranged in each through hole near the inner wall of the hollow cylindrical shell to generate positive ions;
[0067] The fan is arranged outside the hollow cylindrical shell and is used to generate wind force to blow the positive ions generated by the plasma generator to the surface of the fiber filaments;
[0068] (4) The fiber filaments after eliminating the surface static charge are sequentially oiled and three-stage hot roller stretched, and finally the stretched filament bundles are wound to obtain ultrafine fiber filaments; wherein the first stage hot stretching temperature is 90°C, and the stretching ratio is 1.3 times; the second stage hot stretching temperature is 95°C, and the stretching ratio is 1.5 times; the third stage hot stretching temperature is 150°C, and the stretching ratio is 1.2 times.
[0069] The final ultrafine fiber filament has an average single filament diameter of 3 μm, a continuous winding time of 3 hours, and can be unwound normally at an unwinding speed of 500 m / min; the ultrafine fiber filament has a linear density of 13 dtex, a breaking strength of 2.5 cN / dtex, and an elongation at break of 18%.
[0070] Example 3
[0071] A method for continuously producing ultrafine fiber filaments, the specific steps are as follows:
[0072] (1) Polylactic acid (manufacturer: NatureWorks, USA, brand: 3251D) was melt-extruded at 220°C through a single screw extruder at a rotation speed of 20 r / min, and then transported to a spinneret through a micro metering pump; wherein, the diameter of the single screw extruder was 8 mm, and the aspect ratio of the single screw extruder was 16:1;
[0073] (2) After the melt transported to the spinneret is extruded through the spinneret hole, it is sprayed downward under the action of the electrostatic field and airflow field applied from bottom to top; wherein, the number of spinneret holes of the spinneret is 300, the diameter of the spinneret hole is 0.08 mm, and the spacing between adjacent spinneret holes is 1.3 mm; the single hole extrusion amount of the spinneret is 0.012 G / min, and the extrusion pressure is 0.5 MPa; the electric field strength of the electrostatic field is 500 kV / m, the gas flow rate of the airflow field is 3 m / s, and the airflow temperature is 70 °C;
[0074] (3) The fiber filaments ejected through the electrostatic field and the airflow field are twisted and bundled under the action of the rotating airflow. The twisted and bundled fiber filaments are then passed through the internal hollow static eliminator to eliminate the negative charge on the surface of the fiber filaments caused by friction with the air; wherein, the airflow pressure during twisting and bundling is 0.5MPa, and the twisting airflow is 600L / min;
[0075] The static eliminator includes a hollow cylindrical shell, a plasma generator and a fan;
[0076] The inner wall of the hollow cylindrical shell is provided with 8 through holes evenly distributed in the radial direction, and a plasma generator is respectively arranged in each through hole near the inner wall of the hollow cylindrical shell to generate positive ions;
[0077] The fan is arranged outside the hollow cylindrical shell and is used to generate wind force to blow the positive ions generated by the plasma generator to the surface of the fiber filaments;
[0078] (4) The fiber filaments after eliminating the surface static charge are sequentially oiled and three-stage hot roller drawing, and finally the drawn filament bundles are wound to obtain ultrafine fiber filaments; wherein the first stage hot drawing temperature is 70°C, and the drawing ratio is 1.2 times; the second stage hot drawing temperature is 75°C, and the drawing ratio is 1.2 times; the third stage hot drawing temperature is 90°C, and the drawing ratio is 1.2 times.
[0079] The final ultrafine fiber filament has an average single filament diameter of 1 μm, a continuous winding time of 5 hours, and can be unwound normally with an unwinding speed of 400 m / min; the ultrafine fiber filament has a linear density of 27 dtex, a breaking strength of 2.2 cN / dtex, and an elongation at break of 13%.
[0080] Example 4
[0081] A method for continuously producing ultrafine fiber filaments, the specific steps are as follows:
[0082] (1) Polyamide (manufacturer: Shanghai Cathay Biotechnology Co., Ltd., brand: E-1273) was melt-extruded at 285°C through a single screw extruder with a rotation speed of 12 r / min, and then transported to a spinneret through a micro metering pump; wherein, the diameter of the single screw extruder was 15 mm, and the aspect ratio of the single screw extruder was 18:1;
[0083] (2) After the melt transported to the spinneret is extruded through the spinneret hole, it is sprayed downward under the action of the electrostatic field and airflow field applied from bottom to top; wherein, the number of spinneret holes of the spinneret is 200, the diameter of the spinneret hole is 0.2 mm, and the distance between adjacent spinneret holes is 1.8 mm; the single hole extrusion amount of the spinneret is 0.013 G / min, and the extrusion pressure is 1.5 MPa; the electric field strength of the electrostatic field is 120 kV / m, the gas flow rate of the airflow field is 2.5 m / s, and the airflow temperature is 60 °C;
[0084] (3) The fiber filaments ejected through the electrostatic field and the airflow field are twisted and bundled under the action of the rotating airflow. The twisted and bundled fiber filaments are then passed through the internal hollow static eliminator to eliminate the negative charge generated on the surface of the fiber filaments due to friction with the air; wherein, the airflow pressure during twisting and bundling is 0.6MPa, and the twisting airflow is 700L / min;
[0085] The static eliminator includes a hollow cylindrical shell, a plasma generator and a fan;
[0086] The inner wall of the hollow cylindrical shell is provided with 64 through holes evenly distributed in the radial direction, and a plasma generator is respectively arranged in each through hole near the inner wall of the hollow cylindrical shell to generate positive ions;
[0087] The fan is arranged outside the hollow cylindrical shell and is used to generate wind force to blow the positive ions generated by the plasma generator to the surface of the fiber filaments;
[0088] (4) The fiber filaments after eliminating the surface static charge are sequentially oiled and three-stage hot roller drawing, and finally the drawn filament bundles are wound to obtain ultrafine fiber filaments; wherein the first stage hot drawing temperature is 70°C, and the drawing ratio is 1.2 times; the second stage hot drawing temperature is 80°C, and the drawing ratio is 1.2 times; the third stage hot drawing temperature is 90°C, and the drawing ratio is 1.3 times.
[0089] The final ultrafine fiber filament has an average single filament diameter of 3 μm, a continuous winding time of 1 hour, and can be unwound normally at an unwinding speed of 400 m / min; the ultrafine fiber filament has a linear density of 20 dtex, a breaking strength of 2.5 cN / dtex, and an elongation at break of 18%.
[0090] Example 5
[0091] A method for continuously producing ultrafine fiber filaments, the specific steps are as follows:
[0092] (1) Polylactic acid (manufacturer: Anhui Fengyuan Group Co., Ltd., brand: FY201, melt index: 6.0 g / 10 min) was melt-extruded at 210°C through a single screw extruder at a rotation speed of 16 r / min, and then transported to a spinneret through a micro metering pump; wherein, the diameter of the single screw extruder was 10 mm, and the aspect ratio of the single screw extruder was 22:1;
[0093] (2) After the melt transported to the spinneret is extruded through the spinneret hole, it is sprayed downward under the action of the electrostatic field and airflow field applied from bottom to top; wherein, the number of spinneret holes of the spinneret is 150, the diameter of the spinneret hole is 0.1 mm, and the spacing between adjacent spinneret holes is 2 mm; the single hole extrusion amount of the spinneret is 0.016 G / min, and the extrusion pressure is 0.3 MPa; the electric field strength of the electrostatic field is 600 kV / m, the gas flow rate of the airflow field is 5 m / s, and the airflow temperature is 70 °C;
[0094] (3) The fiber filaments ejected through the electrostatic field and the airflow field are twisted and bundled under the action of the rotating airflow. The twisted and bundled fiber filaments are then passed through the internal hollow static eliminator to eliminate the negative charge generated on the surface of the fiber filaments due to friction with the air; wherein, the airflow pressure during twisting and bundling is 0.9MPa, and the twisting airflow is 1200L / min;
[0095] The static eliminator includes a hollow cylindrical shell, a plasma generator and a fan;
[0096] The inner wall of the hollow cylindrical shell is provided with 24 through holes evenly distributed in the radial direction, and a plasma generator is respectively arranged in each through hole near the inner wall of the hollow cylindrical shell to generate positive ions;
[0097] The fan is arranged outside the hollow cylindrical shell and is used to generate wind force to blow the positive ions generated by the plasma generator to the surface of the fiber filaments;
[0098] (4) The fiber filaments after eliminating the surface static charge are sequentially oiled and three-stage hot roller drawing, and finally the drawn filament bundles are wound to obtain ultrafine fiber filaments; wherein the first stage hot drawing temperature is 80°C, and the drawing ratio is 1.1 times; the second stage hot drawing temperature is 85°C, and the drawing ratio is 1.2 times; the third stage hot drawing temperature is 90°C, and the drawing ratio is 1.2 times.
[0099] The final ultrafine fiber filament has an average single filament diameter of 2 μm, a continuous winding time of 5 hours, and can be unwound normally with an unwinding speed of 600 m / min; the ultrafine fiber filament has a linear density of 18 dtex, a breaking strength of 2.3 cN / dtex, and an elongation at break of 15%.
Claims
1. A method for continuous production of ultrafine fiber filaments, characterized in that: First, the polymer is heated and melted by a screw extruder and then transported to a spinneret through a micrometering pump. The melt extruded through the spinneret hole is sprayed downward under the action of an electrostatic field and an airflow field. Then, the ejected fiber filaments are twisted and bundled under the action of a rotating airflow. The twisted and bundled fiber filaments are then passed through an internal hollow static eliminator to eliminate the static charge on the surface caused by friction with the air. After that, the fiber filaments after eliminating the static charge on the surface are oiled and stretched with a hot roller in turn. Finally, the stretched filament bundles are wound to obtain ultrafine fiber filaments. The electrostatic field is applied from bottom to top, with an electric field strength of 120~600kV / m; the gas flow field is applied from top to bottom, with a gas flow rate of 0.4~5m / s and a gas flow temperature of 20~150℃; The single filament diameter of the ultrafine fiber filament is 1~3μm, the continuous winding time is not less than 1h, and it can be unwound normally, and the unwinding speed is above 300m / min; The number of spinneret holes is 100~300, the hole diameter is 0.08~0.5mm, and the distance between adjacent spinneret holes is 0.8~2mm; the single hole extrusion volume of the spinneret is ≤0.016G / min, and the extrusion pressure is ≤1.5MPa; the air flow pressure during twisting and bundling is 0.3~0.9MPa, and the twisting air flow is 600~1200L / min.
2. The method for continuous production of ultrafine fiber filaments according to claim 1, characterized in that: The polymer is one or more of polypropylene, polyethylene, polyester, liquid crystal polyester, polylactic acid, polyamide, polyoxymethylene, polycarbonate, polyphenylene ether, polysulfone, polyetheretherketone, polyphenylene sulfide, polyimide and polyetherimide.
3. The method for continuous production of ultrafine fiber filaments according to claim 1, characterized in that: The screw extruder is a single screw extruder with a rotation speed of 5-20 r / min, a diameter of 8-35 mm, and an aspect ratio of 15-26:
1.
4. The method for continuous production of ultrafine fiber filaments according to claim 3, characterized in that: The processing temperature of the screw extruder is 180~360℃.
5. The method for continuous production of ultrafine fiber filaments according to claim 1, characterized in that: The static eliminator includes a hollow cylindrical shell, a plasma generator and a fan; The hollow cylindrical shell is provided with a plurality of radial through holes, and a plasma generator is arranged in the through holes near the inner wall of the hollow cylindrical shell to generate positive ions or negative ions; The fan is arranged on the outside of the hollow cylindrical shell and is used to generate wind force to blow the positive ions or negative ions generated by the plasma generator to the surface of the fiber filaments.
6. The method for continuous production of ultrafine fiber filaments according to claim 1, characterized in that: Hot roller stretching includes three levels of hot stretching. The first level hot stretching temperature is 60~150℃, and the stretching multiple is 1.1~2 times; the second level hot stretching temperature is 75~200℃, and the stretching multiple is 1.2~2 times; the third level hot stretching temperature is 90~300℃, and the stretching multiple is 1.2~2 times.
Citation Information
Patent Citations
A sea-island fiber with PET as the island component, its preparation method, and the resulting microfiber.
CN111621875B
Sea-island fiber with PP as island component, preparation method of sea-island fiber and superfine fiber formed by sea-island fiber
CN111676544A
A sea-island fiber with PA6 as the island component, its preparation method, and the resulting microfiber.
CN111733480B
Melting electrostatic spinning device and method for preparing nanofiber filaments through melting electrostatic spinning device
CN116716668A
Preparation method for producing porous superfine denier chinlon 6 FDY (Fully Drawn Yarn) by cross air blowing
CN117987938A