A method for testing the crystallization tendency of silicate glass
Through Raman spectral analysis of silicate glass, the crystallization tendency is directly determined, which solves the problems of cumbersome preparation and detection process and high energy consumption in the existing technology, and achieves rapid and low-cost crystallization tendency detection, reducing waste produce.
Patent Information
- Application Number
- CN202410577263.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-05-10
AI Technical Summary
In the prior art, it is necessary to prepare microcrystalline glass first and then perform XRD detection to determine its crystal phase type. The process consumes high energy, is expensive, is cumbersome, has a long experimental cycle, and the sample produces a lot of waste.
By detecting the Raman spectrum of silicate glass, the spectral segment of 600-1300cm-1 was intercepted, and 5 peak sites were selected for pretreatment and peak fitting. The formula S=1×A1+2×A2+3× A3+4×A4 determines the crystallization tendency of silicate glass, and directly analyzes it without heating or adding a nucleating agent.
It greatly reduces the experiment time and cost, reduces waste generation, provides a simple, environmentally friendly method to detect the tendency of glass crystallization, and the detection results are consistent with traditional methods.
Smart Images

Figure CN118443651B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of experimental detection, and in particular to a method for testing the crystallization tendency of silicate glass. Background Art
[0002] Glass-ceramics is a type of solid composite material that is prepared by targeted crystallization of base glass and contains both glass phase and crystal phase. As a new type of inorganic non-metallic material with superior performance, its application areas mainly include architectural decoration, municipal construction, military defense, aerospace, optical devices, electronics industry, daily necessities and chemical engineering.
[0003] The production of glass-ceramics is a new type of polycrystalline silicate material that is crystallized by adding reagents (catalysts or nucleating agents) and undergoing heat treatment. Glass-ceramics is a dense, non-porous, and uniform mixture of a crystalline phase and a residual glass phase. Usually, the size of the crystals can range from nanometers to micrometers, and the number of crystals can reach 50%-90%.
[0004] Glass is composed of a silicon-oxygen network. The basic structure of the silicon-oxygen network is a disordered silicon-oxygen tetrahedron. In a silicon-oxygen tetrahedron, the silicon atom is the center and the oxygen atom is the vertex. In a crystal, two tetrahedral structures share one oxygen atom to form an ordered structure. This connection is called bridging. In this case, the Si-O-Si bond is called a bridging oxygen bond. When the oxygen atom is connected to only one tetrahedral structure, it presents a negatively charged Si-O - state, defining it as a non-bridging oxygen bond.
[0005] There are many types of silicate crystal phases that can be precipitated in microcrystalline glass, including feldspar phase, olivine phase, pyroxene phase, amphibole phase, mica phase, etc. The specific crystal phase that is precipitated needs to be determined by testing after obtaining microcrystalline glass. The common feature between them and glass is that there are also silicon-oxygen tetrahedral structures with different connection modes in the crystal phase structure. Unlike the glass network, the silicon-oxygen tetrahedral structure in the crystal phase is orderly.
[0006] Currently, after the microcrystalline glass is prepared, it needs to be subjected to XRD testing to determine its specific crystal phase type. The whole process has high energy consumption, high cost, complicated steps, long experimental cycle, and a lot of waste generated by experimental samples. Summary of the invention
[0007] Therefore, the technical problem to be solved by the present invention is to overcome the defect in the prior art that microcrystalline glass needs to be prepared first and then subjected to XRD detection to determine the crystalline phase in the microcrystalline glass, thereby providing a method for testing the crystallization tendency of silicate glass.
[0008] The present invention provides a method for testing the crystallization tendency of silicate glass, wherein the specific testing steps include:
[0009] a. Detect the Raman spectrum of the treated silicate glass;
[0010] b. Intercept the Raman shift from the Raman spectrum to 600-1300cm -1 Spectrum, select 5 peaks, m0 corresponds to Raman shift of 600-800cm -1 , m1 corresponds to a Raman shift of 805-900 cm -1 , m2 corresponds to a Raman shift of 905-950cm -1 , m3 corresponds to a Raman shift of 955-1000cm -1 , m4 corresponds to a Raman shift of 1005-1300cm -1 , and then preprocessing;
[0011] c. Perform peak fitting processing to obtain the sub-peak area Q x , x is an integer from 0 to 4,
[0012] A x is the peak area Q x The ratio of all peak areas, x is an integer from 1 to 4;
[0013] d. Determine the crystallization tendency of silicate glass according to the formula,
[0014] The formula is: S = 1 × A 1 +2×A 2 +3×A 3 +4×A 4 ,
[0015] When 4.0>S≥3.1, the crystallization tendency of silicate glass is feldspar phase.
[0016] When 3.1>S≥2.6, the crystallization tendency of silicate glass is mica phase.
[0017] When 2.6>S≥2.1, the crystallization tendency of silicate glass is amphibole phase.
[0018] When 2.1>S≥1.5, the crystallization tendency of silicate glass is pyroxene phase.
[0019] When 1.5>S>0, the crystallization tendency of silicate glass is olivine phase.
[0020] In the present invention, the silicate glass is not heated, and no nucleating agent is added for nucleation crystallization treatment.
[0021] In the present invention, the specific range limiting step is to use the Truncate data tool to select 600-1300cm in the Raman spectrum -1 The data in .
[0022] According to the present invention, the silicate glass can be purchased commercially or prepared; when purchased commercially, the silicate glass includes but is not limited to one of aluminosilicate glass, borosilicate glass, and soda-lime silicate glass, and further includes but is not limited to one of sodium aluminosilicate glass, sodium borosilicate glass, and calcium magnesium aluminosilicate glass; when prepared, typically but not limitingly, the specific preparation process includes: mixing raw materials such as Na2O, MgO, MgF2, Al2O3, SiO2, Fe2O3, K2O, CaO, TiO2, B2O3, etc., melting, pouring, and finally annealing to obtain silicate glass. In some optional embodiments, Na2O, MgO, Al2O3, SiO2, Fe2O3, CaO, and B2O3 are used as raw materials, and the total mass of the raw materials is used as a benchmark, wherein the content of MgO is 8.5wt%, the content of Al2O3 is 8.5wt%, the content of CaO is 16.9wt%, the content of SiO2 is 47wt%, the content of B2O3 is 7.7wt%, the content of Na2O is 5.9wt%, and the content of Fe2O3 is 5.5wt%; the parameters of melting and annealing are conventional in the field, for example, the mixed material can be melted at 1500-1600°C, the melting time is 3-5h, the annealing temperature can be 600-650°C, and the time can be 3-4h.
[0023] According to the present invention, in step a, the thickness of the silicate glass is 5-10 mm.
[0024] According to the present invention, in step a, the specific steps of the treatment include grinding and polishing.
[0025] In the present invention, grinding and polishing are conventional processing methods in the art. Typically, but not limiting, 1000-mesh sandpaper, 2000-mesh sandpaper and 3000-mesh sandpaper are used in sequence for the grinding, and the grinding is performed 3 times in total.
[0026] In the present invention, a laser Raman analyzer is used for detection.
[0027] According to the present invention, in step a, the wavelength of the laser of the laser Raman analyzer used is selected from one of 325nm, 473nm, 532nm and 633nm, and the power is 15-25mW.
[0028] According to the present invention, in step a, the temperature of the Raman spectrum detection is 20-25° C., and the detection exposure time is 3-5 s.
[0029] According to the present invention, in step a, the temperature fluctuation range of the detection process does not exceed 1°C.
[0030] According to the present invention, in step a, the number of scans for the detection is 5-8 times.
[0031] In the present invention, WiRE5.2 is used to analyze the data obtained by the laser Raman analyzer.
[0032] According to the present invention, the preprocessing includes baseline correction and normalization processing.
[0033] In the present invention, the specific baseline correction step is to use the Through chosen points on each spectrum method in the Subtract baseline tool to perform fluorescence background subtraction; the specific normalization processing step is to use the curve fit tool to perform five-peak fitting on the selected range, wherein the weighted model is Square root, and the five peaks are confined to corresponding positions.
[0034] In the present invention, the glass is composed of a silicon-oxygen network, the basic structure of which is a disordered silicon-oxygen tetrahedron. In a silicon-oxygen tetrahedron, the silicon atom is the center Si 1 , oxygen atom is the vertex O 1 1. O 1 2. O 1 3. O 1 4. As a silicon-oxygen tetrahedron 1 The oxygen atom O 1 1. It can also serve as a silicon-oxygen tetrahedron 2 The vertices of the silicon atom Si 2 connection, i.e. silicon-oxygen tetrahedron 1 and silicon-oxygen tetrahedron 2 Two tetrahedral structures share one oxygen atom O 1 1, at this time Si 1 -O-Si 2 The bond is called a bridging oxygen bond. 1 1. O 1 2. O 1 3. O 1 The 4 connection methods are independent of each other. When 4 oxygen atoms serve as two vertices of the silicon-oxygen tetrahedron, it is case one. When 3 oxygen atoms serve as two vertices of the silicon-oxygen tetrahedron, it is case two. When 2 oxygen atoms serve as two vertices of the silicon-oxygen tetrahedron, it is case three. When 1 oxygen atom serves as two vertices of the silicon-oxygen tetrahedron, it is case four. When 4 oxygen atoms serve as only one vertex of the silicon-oxygen tetrahedron, it is case five. It is based on these five cases that we select 5 points m0, m1, m2, m3 and m4.
[0035] According to the present invention, along the direction of Raman shift from small to large, five peak sites m0, m1, m2, m3 and m4 are selected to decompose the Raman characteristic peak into Q 0 , Q 1 , Q 2 , Q3 , Q 4 Peak area superposition form, m0 corresponds to Q 0 , and so on, one by one correspondence is derived to derive the data when the fitting line and the test line fit together, and the peak area Q is obtained. x , x is an integer from 0 to 4.
[0036] According to the present invention, the peak separation fitting process is Gaussian fitting.
[0037] According to the present invention, the A x The specific calculation formula is: x =Q x / (Q 0 +Q 1 +Q 2 +Q 3 +Q 4 )×100%, where x is an integer from 1 to 4.
[0038] The technical solution of the present invention has the following advantages:
[0039] 1. The present invention relates to a method for testing the crystallization tendency of silicate glass, wherein the specific testing steps include: a. detecting the Raman spectrum of the treated silicate glass; b. intercepting the Raman shift of 600-1300cm from the Raman spectrum; -1 Spectrum, select 5 peaks, m0 corresponds to Raman shift of 600-800cm -1 , m1 corresponds to a Raman shift of 805-900 cm -1 , m2 corresponds to a Raman shift of 905-950cm -1 , m3 corresponds to a Raman shift of 955-1000cm -1 , m4 corresponds to a Raman shift of 1005-1300cm -1 , and then preprocessing; c. Perform peak fitting processing to obtain the sub-peak area Q x , x is an integer from 0 to 4, A x is the peak area Q x The ratio of the total peak area to the total peak area, x is an integer of 1-4; d. Determine the crystallization tendency of the silicate glass according to the formula; the formula is: S = 1 × A 1 +2×A 2 +3×A 3 +4×A 4When 4.0>S≥3.1, the crystallization tendency of silicate glass is feldspar phase, when 3.1>S≥2.6, the crystallization tendency of silicate glass is mica phase, when 2.6>S≥2.1, the crystallization tendency of silicate glass is amphibole phase, when 2.1>S≥1.5, the crystallization tendency of silicate glass is pyroxene phase, when 1.5>S>0, the crystallization tendency of silicate glass is olivine phase. The testing method of the present invention can detect the crystallization tendency of glass, and there is no need to prepare microcrystalline glass and then determine the crystal phase of microcrystalline glass. It greatly reduces the experimental time, reduces the experimental cost, and reduces the waste generated by the experiment.
[0040] 2. The specific laser wavelength and power, specific exposure time and number of detection scans of the laser Raman analyzer of the present invention can further improve the signal-to-noise ratio of the Raman spectrum and bring more accurate fitting results. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 is a Raman spectrum of Example 1 of the present invention;
[0043] Figure 2 is the XRD pattern of Example 1 of the present invention;
[0044] Figure 3 is a Raman spectrum of Example 2 of the present invention;
[0045] Figure 4 is the XRD pattern of Example 2 of the present invention;
[0046] Figure 5 is a Raman spectrum of Example 3 of the present invention;
[0047] Figure 6 is the XRD pattern of Example 3 of the present invention;
[0048] Figure 7 is a Raman spectrum of Example 4 of the present invention;
[0049] Figure 8 is the XRD pattern of Example 4 of the present invention;
[0050] Fig. 9 is a Raman spectrum of Example 5 of the present invention;
[0051] Fig.10 is the XRD pattern of Example 5 of the present invention;
[0052] Fig.11 The present invention is a flow chart of a method for testing the crystallization tendency of silicate glass. DETAILED DESCRIPTION
[0053] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0054] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0055] Example 1
[0056] This embodiment provides a method for testing the crystallization tendency of silicate glass. The test flow chart is as follows: Fig.11 As shown, the specific steps are as follows:
[0057] The silicate glass preparation process is as follows: analytically pure Na2O, MgO, Al2O3, SiO2, Fe2O3, CaO and B2O3 are mixed as raw materials, and the total weight of the raw materials is used as a benchmark, wherein the content of MgO is 8.5wt%, the content of Al2O3 is 8.5wt%, the content of CaO is 16.9wt%, the content of SiO2 is 47wt%, the content of B2O3 is 7.7wt%, the content of Na2O is 5.9wt%, and the content of Fe2O3 is 5.5wt%, the mixed materials are melted at 1500°C for 3h, then cast, and finally annealed at 600°C for 3h to obtain the silicate glass; the thickness of the silicate glass is 5mm, and the silicate glass is ground and polished with 1000-mesh sandpaper, 2000-mesh sandpaper and 3000-mesh sandpaper in turn to obtain the treated silicate glass.
[0058] a. The treated silicate glass was tested by a laser Raman analyzer with a wavelength of 532nm, a power of 20mW, a detection temperature of 20°C, a temperature fluctuation range of 1°C, an exposure time of 3s, and a detection scan number of 5 times to obtain a Raman spectrum;
[0059] b. Use the Truncate data tool to select 600-1300cm in the Raman spectrum. -1For the data in , select 5 peaks, and m0 corresponds to a Raman shift of 700 cm -1 , m1 corresponds to a Raman shift of 888 cm -1 , m2 corresponds to a Raman shift of 926 cm -1 , m3 corresponds to a Raman shift of 977 cm -1 , m4 corresponds to a Raman shift of 1022 cm -1 The specific baseline correction step is to use the Through chosen points on each spectrum method in the Subtractbaseline tool to perform fluorescence background subtraction; the specific normalization step is to use the curve fit tool to perform five-peak fitting on the selected range, where the weighted model is Square root, and the five peaks are limited to the corresponding positions;
[0060] c. Perform peak-splitting Gaussian fitting on the Raman characteristic peaks in the intercepted spectrum to obtain the peak area value Q 0 , Q 1 , Q 2 , Q 3 , Q 4 like Figure 1 As shown in Table 1; A 1 , A 2 , A 3 , A 4 The values are shown in Table 1;
[0061] d. According to S = 1 × A 1 +2×A 2 +3×A 3 +4×A 4 , calculated S = 3.17.
[0062] Table 1
[0063]
[0064] Q 0 It is 0 because there are no four oxygen atoms in silicate glass that serve as two vertices of silicon-oxygen tetrahedron.
[0065] S>3.1, the crystallization tendency of silicate glass is feldspar phase.
[0066] The traditional preparation and testing method is to grind the glass sample to obtain a powder that passes through a 200-mesh sieve, and perform DSC testing on the powder from room temperature to 1200°C, wherein the heating rate is 5°C / min, and obtain the DSC curve. According to the positions of the endothermic peak and the exothermic peak in the DSC curve, the nucleation temperature and the crystallization temperature are determined to be 720°C and 1000°C, respectively. The glass sample is placed in a muffle furnace for nucleation heat treatment at 720°C for 3 hours, and then the temperature is raised to 1000°C for crystallization heat treatment for 3 hours to obtain a microcrystalline glass sample, which is then crushed and ground to pass through a 325-mesh sieve, and XRD is performed to detect the crystalline phase precipitated in the microcrystalline glass.
[0067] The above experiments were compared with traditional preparation and detection methods, such as Figure 2 As shown: the result shown by XRD is also a feldspar phase, and the present invention is consistent with the XRD result.
[0068] Example 2
[0069] The present embodiment provides a method for testing the crystallization tendency of silicate glass, and the specific steps are as follows: the silicate glass preparation process is: using analytical pure Na2O, MgF2, MgO, Al2O3, SiO2, K2O, and B2O3 as raw materials for mixing, based on the total mass of the raw materials, wherein the content of MgF2 is 10wt%, the content of Al2O3 is 10.7wt%, the content of MgO is 5.2wt%, the content of SiO2 is 50wt%, the content of B2O3 is 10wt%, the content of Na2O is 4.2wt%, and the content of K2O is 9.9wt%, the mixed materials are melted at 1500° C. for 3 hours, then cast, and finally annealed at 600° C. for 3 hours to obtain silicate glass; the thickness of the silicate glass is 5 mm, and the silicate glass is ground and polished using 1000 mesh sandpaper, 2000 mesh sandpaper, and 3000 mesh sandpaper in sequence to obtain the treated silicate glass.
[0070] a. The treated silicate glass was tested by a laser Raman analyzer with a wavelength of 532nm, a power of 20mW, a detection temperature of 22°C, a temperature fluctuation range of 1°C, an exposure time of 4s, and a number of scans for 7 times to obtain a Raman spectrum;
[0071] b. Use the Truncate data tool to select 600-1300cm in the Raman spectrum. -1 From the data in , 5 peaks are selected, and the Raman shift corresponding to m0 is 752cm -1 , m1 corresponds to a Raman shift of 850 cm -1 , m2 corresponds to a Raman shift of 935 cm -1 , m3 corresponds to a Raman shift of 998 cm -1, m4 corresponds to a Raman shift of 1080 cm -1 The specific baseline correction step is to use the Through chosen points on each spectrum method in the Subtractbaseline tool to perform fluorescence background subtraction; the specific normalization step is to use the curve fit tool to perform five-peak fitting on the selected range, where the weighted model is Square root, and the five peaks are limited to the corresponding positions;
[0072] c. Perform peak-splitting Gaussian fitting on the Raman characteristic peaks in the intercepted spectrum to obtain the peak area value Q 0 , Q 1 , Q 2 , Q 3 , Q 4 like Figure 3 As shown in Table 2; A 1 , A 2 , A 3 , A 4 The values are shown in Table 2;
[0073] d. According to S = 1 × A 1 +2×A 2 +3×A 3 +4×A 4 , calculated S = 2.99.
[0074] Table 2
[0075]
[0076] Q 1 Because the area values of the other sub-peaks are too different, Figure 3 However, from the data in Table 2, we can see that Q 1 It is not 0.
[0077] 3.1>S≥2.6, the crystallization tendency of silicate glass is mica phase.
[0078] Conventional preparation and detection method: The treated silicate glass is obtained according to the operation of Example 2, and then the glass sample is crushed and ground to obtain a powder that passes through a 200-mesh sieve. The powder is subjected to DSC detection from room temperature to 1200°C, wherein the heating rate is 10°C / min, and the DSC curve is obtained. According to the positions of the endothermic peak and the exothermic peak in the DSC curve, the nucleation temperature and the crystallization temperature are determined to be 710°C and 980°C, respectively. The glass sample is placed in a muffle furnace for nucleation heat treatment at 710°C for 3h, and then the temperature is raised to 980°C for crystallization heat treatment for 3h to obtain a microcrystalline glass sample, and the microcrystalline glass sample is crushed and ground to pass through a 325-mesh sieve, and XRD is performed to detect the crystalline phase precipitated in the microcrystalline glass.
[0079] The above experiments were compared with traditional preparation and detection methods, such as Figure 4 As shown: the result shown by XRD is also mica phase, and the present invention is consistent with the XRD result.
[0080] Example 3
[0081] This embodiment provides a method for testing the crystallization tendency of silicate glass, and the specific steps are as follows:
[0082] The silicate glass preparation process is as follows: analytically pure Na2O, MgO, Al2O3, SiO2, TiO2, CaO, Fe2O3, and K2O are mixed as raw materials, and the total mass of the raw materials is used as a benchmark, wherein the content of Al2O3 is 20wt%, the content of MgO is 12wt%, the content of SiO2 is 42wt%, the content of CaO is 6wt%, the content of TiO2 is 8wt%, the content of Fe2O3 is 8wt%, the content of Na2O is 2wt%, and the content of K2O is 2wt%, the mixed materials are melted at 1500°C for 3h, and then cast, and finally annealed at 600°C for 3h to obtain the silicate glass; the thickness of the silicate glass is 5mm, and the silicate glass is ground and polished with 1000-mesh sandpaper, 2000-mesh sandpaper, and 3000-mesh sandpaper in turn to obtain the treated silicate glass.
[0083] a. The treated silicate glass was tested by a laser Raman analyzer with a wavelength of 473 nm, a power of 25 mW, a detection temperature of 21 ° C, a temperature fluctuation range of 1 ° C, an exposure time of 3 s, and a detection scan number of 8 times to obtain a Raman spectrum;
[0084] b. Use the Truncate data tool to select 600-1300cm in the Raman spectrum. -1 From the data in , 5 peaks are selected, and the Raman shift corresponding to m0 is 698cm -1 , m1 corresponds to a Raman shift of 885 cm -1 , m2 corresponds to a Raman shift of 942 cm -1 , m3 corresponds to a Raman shift of 998 cm -1 , m4 corresponds to a Raman shift of 1047 cm -1The specific baseline correction step is to use the Through chosen points on each spectrum method in the Subtractbaseline tool to perform fluorescence background subtraction; the specific normalization step is to use the curve fit tool to perform five-peak fitting on the selected range, where the weighted model is Square root, and the five peaks are limited to the corresponding positions;
[0085] c. Perform peak-splitting Gaussian fitting on the Raman characteristic peaks in the intercepted spectrum to obtain the peak area value Q 0 , Q 1 , Q 2 , Q 3 , Q 4 like Figure 5 As shown in Table 3; A 1 , A 2 , A 3 , A 4 The values are shown in Table 3;
[0086] d. According to S = 1 × A 1 +2×A 2 +3×A 3 +4×A 4 , calculated S = 2.52.
[0087] Table 3
[0088]
[0089] 2.6>S≥2.1, the crystallization tendency of silicate glass is amphibole phase.
[0090] Conventional preparation and detection method: The treated silicate glass is obtained according to the operation of Example 3, and then the glass sample is crushed and ground to obtain a powder that passes through a 200-mesh sieve. The powder is subjected to DSC detection from room temperature to 1200°C, wherein the heating rate is 10°C / min, and the DSC curve is obtained. According to the positions of the endothermic peak and the exothermic peak in the DSC curve, the nucleation temperature and the crystallization temperature are determined to be 700°C and 950°C, respectively. The glass sample is placed in a muffle furnace for nucleation heat treatment at 700°C for 3h, and then the temperature is raised to 950°C for crystallization heat treatment for 3h to obtain a microcrystalline glass sample. The microcrystalline glass sample is crushed and ground to pass through a 325-mesh sieve, and XRD is performed to detect the crystalline phase precipitated in the microcrystalline glass.
[0091] The above experiments were compared with traditional preparation and detection methods, such as Figure 6 As shown: the result shown by XRD is also an amphibole phase, and the present invention is consistent with the XRD result.
[0092] Example 4
[0093] This embodiment provides a method for testing the crystallization tendency of silicate glass, and the specific steps are as follows:
[0094] The silicate glass preparation process is as follows: analytically pure Na2O, MgO, CaO, Al2O3, SiO2, Fe2O3, K2O and B2O3 are mixed as raw materials, and the total weight of the raw materials is taken as a benchmark, wherein the content of Al2O3 is 11wt%, the content of MgO is 9wt%, the content of CaO is 15wt%, the content of SiO2 is 49wt%, the content of Fe2O3 is 8wt%, the content of B2O3 is 2wt%, the content of Na2O is 4wt%, and the content of K2O is 2wt%, the mixed materials are melted at 1500°C for 3h, and then cast, and finally annealed at 600°C for 3h to obtain the silicate glass; the thickness of the silicate glass is 5mm, and the silicate glass is ground and polished with 1000-mesh sandpaper, 2000-mesh sandpaper and 3000-mesh sandpaper in turn to obtain the treated silicate glass.
[0095] a. The treated silicate glass was tested by a laser Raman analyzer with a wavelength of 633 nm, a power of 21 mW, a detection temperature of 22 ° C, a temperature fluctuation range of 1 ° C, an exposure time of 4 s, and a detection scan number of 6 times to obtain a Raman spectrum;
[0096] b. Use the Truncate data tool to select 600-1300cm in the Raman spectrum. -1 The data in , 5 peaks are selected, and the Raman shift corresponding to m0 is 723cm -1 , m1 corresponds to a Raman shift of 885 cm -1 , m2 corresponds to a Raman shift of 949 cm -1 , m3 corresponds to a Raman shift of 999 cm -1 , m4 corresponds to a Raman shift of 1033 cm -1 The specific baseline correction step is to use the Through chosen points on each spectrum method in the Subtractbaseline tool to perform fluorescence background subtraction; the specific normalization step is to use the curve fit tool to perform five-peak fitting on the selected range, where the weighted model is Square root, and the five peaks are limited to the corresponding positions;
[0097] c. Perform peak-splitting Gaussian fitting on the Raman characteristic peaks in the intercepted spectrum to obtain the peak area value Q 0 , Q 1 , Q 2 , Q 3 , Q 4 like Figure 7 As shown in Table 4; A 1 , A 2 , A 3 , A 4 The values of are shown in Table 4;
[0098] d. According to S = 1 × A 1 +2×A 2 +3×A 3 +4×A 4 , calculated S = 2.07.
[0099] Table 4
[0100]
[0101] 2.1>S≥1.5, the crystallization tendency of silicate glass is pyroxene phase.
[0102] Conventional preparation and detection method: The treated silicate glass is obtained according to the operation of Example 4, and then the glass sample is crushed and ground to obtain a powder that passes through a 200-mesh sieve. The powder is subjected to DSC detection from room temperature to 1200°C, wherein the heating rate is 15°C / min, and the DSC curve is obtained. According to the positions of the endothermic peak and the exothermic peak in the DSC curve, the nucleation temperature and the crystallization temperature are determined to be 690°C and 930°C, respectively. The glass sample is placed in a muffle furnace for nucleation heat treatment at 690°C for 3h, and then the temperature is raised to 930°C for crystallization heat treatment for 3h to obtain a microcrystalline glass sample, and the microcrystalline glass sample is crushed and ground to pass through a 325-mesh sieve, and XRD is performed to detect the crystalline phase precipitated in the microcrystalline glass.
[0103] The above experiments were compared with traditional preparation and detection methods, such as Figure 8 As shown: the result shown by XRD is also a pyroxene phase, and the present invention is consistent with the XRD result.
[0104] Example 5
[0105] This embodiment provides a method for testing the crystallization tendency of silicate glass, and the specific steps are as follows:
[0106] The silicate glass preparation process is as follows: analytically pure Na2O, MgO, CaO, Al2O3, SiO2, Fe2O3, K2O and B2O3 are mixed as raw materials, and the total weight of the raw materials is taken as a benchmark, wherein the content of Al2O3 is 15wt%, the content of MgO is 20wt%, the content of SiO2 is 45wt%, the content of CaO is 9.6wt%, the content of Fe2O3 is 2wt%, the content of B2O3 is 2.2wt%, the content of Na2O is 4.8wt%, and the content of K2O is 1.4wt%, the mixed materials are melted at 1500°C for 3h, then cast, and finally annealed at 600°C for 3h to obtain the silicate glass; the thickness of the silicate glass is 5mm, and the silicate glass is ground and polished with 1000-mesh sandpaper, 2000-mesh sandpaper and 3000-mesh sandpaper in turn to obtain the treated silicate glass.
[0107] a. The treated silicate glass was tested by a laser Raman analyzer with a wavelength of 325 nm, a power of 15 mW, a detection temperature of 23 ° C, a temperature fluctuation range of 0.5 ° C, an exposure time of 3 s, and a detection scan number of 7 times to obtain a Raman spectrum;
[0108] b. Use the Truncate data tool to select 600-1300cm in the Raman spectrum. -1 From the data in , 5 peaks are selected, and the Raman shift corresponding to m0 is 727 cm -1 , m1 corresponds to a Raman shift of 815 cm -1 , m2 corresponds to a Raman shift of 905 cm -1 , m3 corresponds to a Raman shift of 957 cm -1 , m4 corresponds to a Raman shift of 1038 cm -1 The specific baseline correction step is to use the Through chosen points on each spectrum method in the Subtractbaseline tool to perform fluorescence background subtraction; the specific normalization step is to use the curve fit tool to perform five-peak fitting on the selected range, where the weighted model is Square root, and the five peaks are limited to the corresponding positions;
[0109] c. Perform peak-splitting Gaussian fitting on the Raman characteristic peaks in the intercepted spectrum to obtain the peak area value Q 0 , Q 1 , Q 2 , Q 3 , Q 4 like Fig. 9 As shown in Table 5; A 1 , A 2 , A3 , A 4 The values of are shown in Table 5;
[0110] d. According to S = 1 × A 1 +2×A 2 +3×A 3 +4×A 4 , calculate S=1.25.
[0111] Table 5
[0112]
[0113] 1.5>S≥0, the crystallization tendency of silicate glass is olivine phase.
[0114] Conventional preparation and detection method: The treated silicate glass is obtained according to the operation of Example 5, and then the glass sample is crushed and ground to obtain a powder that passes through a 200-mesh sieve. The powder is subjected to DSC detection from room temperature to 1200°C, wherein the heating rate is 10°C / min, and the DSC curve is obtained. According to the positions of the endothermic peak and the exothermic peak in the DSC curve, the nucleation temperature and the crystallization temperature are determined to be 660°C and 900°C, respectively. The glass sample is placed in a muffle furnace for nucleation heat treatment at 660°C for 3h, and then the temperature is raised to 900°C for crystallization heat treatment for 3h to obtain a microcrystalline glass sample, and the microcrystalline glass sample is crushed and ground to pass through a 325-mesh sieve for XRD detection of the crystalline phase precipitated in the microcrystalline glass.
[0115] The above experiments were compared with traditional preparation and detection methods, such as Fig.10 As shown: the result shown by XRD is also olivine phase, and the present invention is consistent with the XRD result.
[0116] It can be seen from the embodiments of the present invention that the technical solution of the present invention can obtain the crystallization tendency of the glass without heating the glass, adding a nucleating agent to cultivate the crystal phase and using DSC and XRD testing. The method is simple, environmentally friendly, has a short experimental cycle, and is harmless to the body of the experimenter.
[0117] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for testing the crystallization tendency of silicate glass, characterized in that: The specific test steps include: a. Using a laser Raman analyzer to detect the Raman spectrum of the treated silicate glass; The wavelength of the laser of the laser Raman analyzer is selected from one of 325nm, 473nm, 532nm and 633nm; b. Intercept the Raman shift from the Raman spectrum to 600-1300cm -1 Spectrum, select 5 peaks, m0 corresponds to Raman shift of 600-800cm -1 , m1 corresponds to a Raman shift of 805-900 cm -1 , m2 corresponds to a Raman shift of 905-950cm -1 , m3 corresponds to a Raman shift of 955-1000cm -1 , m4 corresponds to a Raman shift of 1005-1300cm -1 , and then preprocessing; c. Perform peak fitting processing to obtain the sub-peak area Q 0 , Q 1 , Q 2 , Q 3 , Q 4 , m0 corresponds to Q 0 , m1 corresponds to Q 1 , m2 corresponds to Q 2 、m3 corresponds to Q 3 、m4 corresponds to Q 4 , A x is the peak area Q x The ratio of all peak areas, A x The specific calculation formula is: x =Q x / (Q 0 +Q 1 +Q 2 +Q 3 +Q 4 )×100%, where x is an integer from 1 to 4; d. Determine the crystallization tendency of silicate glass according to the formula, The formula is: S=1×A 1 +2×A 2 +3×A 3 +4×A 4 , When 4.0>S≥3.1, the crystallization tendency of silicate glass is feldspar phase. When 3.1>S≥2.6, the crystallization tendency of silicate glass is mica phase. When 2.6>S≥2.1, the crystallization tendency of silicate glass is amphibole phase. When 2.1>S≥1.5, the crystallization tendency of silicate glass is pyroxene phase. When 1.5>S>0, the crystallization tendency of silicate glass is olivine phase.
2. The method according to claim 1, characterized in that In step b, the preprocessing includes baseline correction and normalization processing.
3. The method according to claim 1 or 2, characterized in that: In step c, the peak fitting process is Gaussian fitting.
4. The method according to claim 1, characterized in that: In step a, the power of the laser used in the laser Raman analyzer is 15-25 mW.
5. The method according to claim 1, characterized in that In step a, the detection temperature of the Raman spectrum is 20-25° C., and the detection exposure time is 3-5 s.
6. The method according to claim 1, characterized in that In step a, the temperature fluctuation range of the detection process does not exceed 1°C.
7. The method according to claim 1, characterized in that In step a, the detection is scanned 5-8 times.
8. The method according to claim 1, characterized in that In step a, the specific steps of the treatment include grinding and polishing.