A method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery
By using iron-based graphene and rare earth lanthanum-doped composite lithium cobalt oxide positive electrode material in lithium-ion battery cathode sheets, a two-component dispersant and binder of modified lignin and modified PVDF-HFP copolymer, The structural instability and electrical performance problems of lithium cobalt oxide positive electrode sheets in lithium-ion batteries are solved, and higher battery performance and service life are achieved.
Patent Information
- Application Number
- CN202410705763.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-03
AI Technical Summary
The existing lithium cobalt oxide positive electrode sheet for lithium-ion batteries reacts with the electrolyte during long-term charging and discharging, resulting in irreversible attenuation and unstable structure, resulting in reduced battery capacity, poor pressure performance and increased surface defects, affecting the migration rate and energy of lithium ion density.
Using iron-based graphene and rare earth lanthanum composite lithium cobalt oxide positive electrode material, combined with two-component dispersant and binder of modified lignin and modified PVDF-HFP copolymer, improve structural stability through microwave pulse treatment and dispersion, reduce interface resistance, enhance electron mobility and electrical cycle stability.
It significantly improves the battery performance and service life of lithium-ion batteries, enhances the transmission performance and high voltage resistance of lithium-ion batteries, solves the problems of agglomeration and instability, and extends the battery's cycle stability and capacity retention rate.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery. Background Art
[0002] In recent years, in order to improve energy efficiency and promote the development of new energy, lithium-ion battery related components have been studied in depth. Among them, the positive electrode sheet for lithium-ion batteries is one of the important components of lithium-ion batteries, which plays a key role in the electrical performance and service life of lithium-ion batteries.
[0003] At present, most of the positive electrode sheets for lithium-ion batteries are made of positive electrode slurry coated with aluminum foil current collector and then compacted; the positive electrode slurry generally includes components such as positive electrode material, conductive agent, binder, dispersant, etc.; among them, the earlier commercialized positive electrode material for lithium-ion batteries is lithium cobalt oxide, which has a higher material density and electrode compaction performance, and its main working principle is the insertion and extraction process of lithium ions and the reduction or oxidation process of cobalt ions. In the prior art, lithium cobalt oxide reacts with the electrolyte during long-term charging and discharging, causing its battery capacity to irreversibly decay during use and having a poor service life; at the same time, its unstable structure also leads to poor high-voltage performance. In addition, the positive electrode slurry prepared with lithium cobalt oxide has agglomeration and instability, resulting in unevenness in the positive electrode sheet prepared therefrom, increasing the surface defects of the positive electrode sheet, thereby reducing the lithium ion migration rate, energy density and other performance of the lithium-ion battery.
[0004] Therefore, it is of great significance to solve the above problems and prepare a lithium cobalt oxide positive electrode sheet for lithium ion batteries with excellent performance. Summary of the invention
[0005] The object of the present invention is to provide a process for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery comprises the following steps:
[0008] Step 1: Preparation of positive electrode materials: S1: Grind and blend iron-based graphene, cobalt oxide and lithium carbonate, and heat treat them at 950-1000°C for 8-10 hours to obtain composite lithium cobalt oxide; S2: Disperse the composite lithium cobalt oxide in a lanthanum chloride aqueous solution, stir at room temperature for 24 hours, wash and dry; Heat treat the obtained material at 500-600°C for 6 hours, and after cooling, microwave pulse at a power of 800-900W for 2-5 seconds to obtain a positive electrode material;
[0009] Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add the dispersant to the solvent and disperse it evenly; add the conductive agent, positive electrode material, and binder in sequence, homogenize, and obtain the positive electrode slurry; S2: Wash the aluminum foil current collector with ethanol; then apply the positive electrode slurry on its surface, compact and dry to obtain the lithium cobalt oxide positive electrode sheet.
[0010] In a further embodiment, the solid content of the positive electrode slurry is 40-60wt%; the raw materials of the positive electrode slurry include the following components: by weight, 93-95 parts of positive electrode material, 2-3 parts of conductive agent, 2.4-3.5 parts of binder, and 0.5-0.6 parts of dispersant.
[0011] In a further embodiment, the dispersant comprises modified lignin and sodium polyacrylate in a mass ratio of 0.3-0.4:0.2-0.3.
[0012] In a further embodiment, the preparation method of the modified lignin is:
[0013] (1) adding alkali lignin to deionized water to obtain a solution with a solid content of 25-30 wt%; adding sodium hydroxide to adjust the pH to 10-12, adding sodium sulfite and formaldehyde; reacting under high pressure and sealed conditions at 160-200°C for 3-5 hours, washing and drying to obtain sulfonic acid lignin;
[0014] (2) Add N-vinyl pyrrolidone, glycerol allyl ether, and N-(1-(5-fluoropyridin-2-yl) vinyl) acetamide to deionized water in sequence, add an aqueous solution of ammonium persulfate dropwise, and react at 75-80°C for 4-6 hours; add sulfonic acid lignin, raise the temperature to 90-100°C, react for 4-5 hours, wash, and dry to obtain modified lignin.
[0015] In a further embodiment, the raw material of the sulfonic acid lignin includes the following components: by weight, 10 parts of alkali lignin, 4 to 4.2 parts of sodium sulfite, and 1 to 1.2 parts of formaldehyde;
[0016] The modified lignin comprises the following raw materials: by weight, 11 to 12 parts of N-vinyl pyrrolidone, 8 to 10 parts of glycerol allyl ether, 3 to 4 parts of N-(1-(5-fluoropyridin-2-yl) vinyl)acetamide, 0.1 to 0.2 parts of ammonium persulfate, and 14 to 16 parts of sulfonic acid lignin.
[0017] In a further embodiment, the binder comprises polyvinylidene fluoride and modified PVDF-HFP copolymer in a mass ratio of 1.5-2.5:0.9-1.
[0018] In a further embodiment, the preparation method of the modified PVDF-HFP copolymer is as follows: (1) adding the PVDF-HFP copolymer to N-methylpyrrolidone and stirring evenly to obtain a solution A having a solid content of 10-15 wt%; (2) adding sodium styrene sulfonate and N-(1-(5-fluoropyridin-2-yl)vinyl)acetamide to dichlorothionyl and stirring evenly to obtain a solution B; (3) mixing solution A and solution B, adding cuprous chloride and pentamethyldiethylenetriamine under a nitrogen atmosphere, reacting at 120-125° C. for 24 hours, washing and drying to obtain a modified PVDF-HFP copolymer;
[0019] In the raw materials of the modified PVDF-HFP copolymer, the mass ratio of the PVDF-HFP copolymer, sodium styrene sulfonate, and N-(1-(5-fluoropyridin-2-yl)vinyl)acetamide is 10:0.8-1.5:1.2-1.5.
[0020] In a further embodiment, in the composite lithium cobaltate, the molar ratio of cobalt in cobalt oxide to lithium in lithium carbonate is 1.8:1.05-1.1; and the amount of the iron-based graphene introduced accounts for 1.5-2.5wt% of the total mass of cobalt oxide and lithium carbonate.
[0021] In a further embodiment, the ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g: 2-3 mL; the concentration of the lanthanum trichloride aqueous solution is 0.4-0.45 mol / L.
[0022] In a further scheme, the preparation method of the iron-based graphene is: ultrasonically disperse graphene oxide in deionized water, add ferric chloride, sodium molybdate, and L-cysteine, and stir for 1 to 2 hours to obtain a mixed solution; transfer it to a reactor, heat it at 220 to 240°C for 24 hours, wash and dry to obtain iron-based graphene; wherein the mass ratio of graphene oxide, ferric chloride, sodium molybdate and L-cysteine is 10:1.5~2:0.5~0.7:3~4.
[0023] The beneficial effects of the present application are as follows: First, by doping iron-based graphene and rare earth lanthanum into lithium cobalt oxide to obtain a positive electrode material, the structural stability of the positive electrode material is effectively increased and the battery performance is improved; second, by using a two-component dispersant containing modified lignin, the dispersibility is improved while the interface resistance is effectively reduced to improve the battery performance; third, by using a two-component binder containing a modified PVDF-HFP copolymer, the adhesion of the positive electrode slurry on the current collector during the charge and discharge process is effectively guaranteed, and the synergistic dispersant effectively improves the electron mobility and electrical cycle stability of the positive electrode sheet.
[0024] In the scheme, iron ions can partially replace cobalt in the positive electrode material and be doped with graphene to adjust the lattice in the composite lithium cobalt oxide, resulting in local deformation of the lattice spacing, thereby increasing the size of the lithium ion diffusion channel and improving the lithium ion transmission performance; and the molybdenum ions contained and the lanthanum ions doped later are doped in the lattice structure, which improves the stability of the lattice structure and avoids the corrosion of the electrolyte on the lattice surface, thereby effectively improving the high voltage resistance and electrical cycle stability. Among them, the positive electrode material is finally subjected to microwave pulse treatment. This process further reduces the defects of the positive electrode material and improves the electrical cycle capacity retention rate after the electrode sheet is applied to the battery.
[0025] In the scheme, compared with the common use of a single sodium polyacrylate as a dispersant, modified lignin is added to the compound with it, and the electrostatic repulsion and steric hindrance formed between the two are used to produce a synergistic effect, which effectively solves the agglomeration and instability existing in the positive electrode slurry; at the same time, it also solves the problem of low peeling strength of the positive electrode slurry and rapid reduction of peeling performance during cyclic charging; thereby improving the battery rate and cycle stability of lithium-ion batteries.
[0026] Among them, the modified lignin is first sulfonated based on alkali lignin, and then compounded with a prepolymer of N-vinyl pyrrolidone, glycerol allyl ether, and N-(1-(5-fluoropyridin-2-yl) vinyl) acetamide. The aromatic ring structures contained in it, such as benzene ring and pyridine, improve the influence of thermal stress during the charge and discharge cycle; and the pyridine ring and fluorine atom contained in it have lone pairs of electrons, which can coordinate with cobalt ions and inhibit the side reactions between cobalt and electrolyte that affect battery performance; at the same time, the pyrrolidone, hydroxyl, and sulfonic acid groups contained in it can generate hydrogen bonds with the surface of the positive electrode material, electrostatically interact, improve the dispersion and ion mobility.
[0027] In the scheme, the binder uses a composition of polyvinylidene fluoride and modified PVDF-HFP copolymer; wherein, some of the chain segments of the introduced modified PVDF-HFP copolymer are similar to some of the chain segments in the binder, and have better affinity, which reduces the interface resistance and improves the electrical performance. On the other hand, the modified PVDF-HFP copolymer is a comb-like structure, which cooperates with the dispersant to form better adhesion, and the groups contained on its surface have good electron mobility and good interface affinity in the positive electrode slurry, which can effectively reduce the surface resistance. In addition, compared with single polyvinylidene fluoride, the combination of the two further increases the stability of the positive electrode during the electrical cycle, improves the powder removal, thereby improving the capacity retention rate after the electrical cycle and increasing the service life of the lithium-ion battery. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] It should be noted that the purchase manufacturers of all raw materials involved in the present invention are exemplified without any special restrictions: in the following embodiments, parts are parts by mass; the solvent in the positive electrode slurry is N-methylpyrrolidone; the conductive agent is acetylene black; polyvinylidene fluoride is polyvinylidene fluoride 5130, and the brand is American Solvay; the product number of PVDF-HFP copolymer is PA14975, and the brand is Wengjiang reagent; polyvinyl pyrrolidone is povidone K30, and the brand is BASF; the sodium polyacrylate model is JH-90, and the brand is Jianghai brand; the alkali lignin brand is Shanghai Nuotai; the product number of graphene oxide is M33420, and the brand is Myrel, and the product number of graphene is A343980, and the brand is Alpha; the CAS number of N-(1-(5-fluoropyridin-2-yl) vinyl) acetamide is 905587-18-0; the CAS number of glycerol allyl ether is 123-34-2.
[0030] Preparation of modified lignin: (1) Add 10 parts of alkali lignin to deionized water to obtain a solution with a solid content of 25 wt%; add sodium hydroxide to adjust the pH to 11.2, add 4.2 parts of sodium sulfite and 1.2 parts of formaldehyde; react at 180°C under high pressure and in a closed manner for 4 hours, wash and dry to obtain sulfonate lignin; (2) Add 12 parts of N-vinyl pyrrolidone, 8 parts of glycerol allyl ether, and 4 parts of N-(1-(5-fluoropyridin-2-yl) vinyl) acetamide to deionized water in sequence, add an aqueous solution of ammonium persulfate (0.2 parts of ammonium persulfate) dropwise, and react at 80°C for 5 hours; add 15 parts of sulfonate lignin, heat to 100°C and react for 4 hours, wash and dry to obtain modified lignin.
[0031] Preparation of PVDF-HFP copolymer: (1) Weigh PVDF-HFP copolymer, sodium styrene sulfonate, and N-(1-(5-fluoropyridin-2-yl)vinyl)acetamide in a mass ratio of 10:1.2:1.3; add the PVDF-HFP copolymer to N-methylpyrrolidone and stir evenly to obtain a solution A with a solid content of 10 wt%; (2) add sodium styrene sulfonate and N-(1-(5-fluoropyridin-2-yl)vinyl)acetamide to thionyl chloride and stir evenly to obtain a solution B with a solid content of 15 wt%; (3) mix solution A and solution B. Mix, add cuprous chloride (accounting for 1wt% of the total mass of PVDF-HFP copolymer, sodium styrene sulfonate, and N-(1-(5-fluoropyridin-2-yl)vinyl)acetamide) and pentamethyldiethylenetriamine (accounting for 1wt% of the total mass of PVDF-HFP copolymer, sodium styrene sulfonate, and N-(1-(5-fluoropyridin-2-yl)vinyl)acetamide) under nitrogen atmosphere, react at 120° C. for 24 hours, wash and dry to obtain a modified PVDF-HFP copolymer;
[0032] Preparation of iron-based graphene: ultrasonically disperse graphene oxide in deionized water, add ferric chloride, sodium molybdate and L-cysteine, stir for 2 hours to obtain a mixed solution; transfer it to a reactor, heat it at 240°C for 24 hours, wash and dry to obtain iron-based graphene; wherein the mass ratio of graphene oxide, ferric chloride, sodium molybdate and L-cysteine is 10:1.8:0.6:4.
[0033] Embodiment 1: A method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery, comprising the following steps:
[0034] Step 1: Preparation of positive electrode materials: S1: Grind and blend iron-based graphene, cobalt oxide, and lithium carbonate, and heat-treat at 950° C. for 10 hours to obtain composite lithium cobalt oxide; in the composite lithium cobalt oxide, the molar ratio of cobalt in cobalt oxide to lithium in lithium carbonate is 1.8:1.08; the amount of the iron-based graphene introduced accounts for 1.5wt% of the total mass of cobalt oxide and lithium carbonate;
[0035] S2: Disperse the composite lithium cobaltate in a 0.4 mol / L lanthanum trichloride aqueous solution, the ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g:2.5 mL, stir at room temperature for 24 hours, wash and dry; heat treat the obtained material at 600°C for 6 hours, and after cooling, microwave pulse for 5 seconds at a power of 800 W to obtain a positive electrode material;
[0036] Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add 0.5 parts of dispersant (modified lignin and sodium polyacrylate in a mass ratio of 0.3:0.2) into the solvent and disperse evenly; add 2 parts of conductive agent, 95 parts of positive electrode material, 2.5 parts of binder (1.5:1 polyvinylidene fluoride and modified PVDF-HFP copolymer) in sequence, homogenize, and obtain a positive electrode slurry with a solid content of 50wt%; S2: Wash the aluminum foil current collector with ethanol; then apply the positive electrode slurry on its surface, compact and dry to obtain a lithium cobalt oxide positive electrode sheet.
[0037] Embodiment 2: A method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery, comprising the following steps:
[0038] Step 1: Preparation of positive electrode materials: S1: Grind and blend iron-based graphene, cobalt oxide, and lithium carbonate, and heat-treat them at 950° C. for 10 hours to obtain composite lithium cobalt oxide; in the composite lithium cobalt oxide, the molar ratio of cobalt in cobalt oxide to lithium in lithium carbonate is 1.8:1.08; the amount of the iron-based graphene introduced accounts for 2.5wt% of the total mass of cobalt oxide and lithium carbonate;
[0039] S2: Disperse the composite lithium cobaltate in a 0.4 mol / L lanthanum trichloride aqueous solution, the ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g:2.5 mL, stir at room temperature for 24 hours, wash and dry; heat treat the obtained material at 600°C for 6 hours, and after cooling, microwave pulse for 2 seconds at a power of 900 W to obtain a positive electrode material;
[0040] Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add 0.6 parts of dispersant (modified lignin and sodium polyacrylate in a mass ratio of 0.3:0.3) into the solvent and disperse evenly; add 3 parts of conductive agent, 93 parts of positive electrode material, 3.4 parts of binder (2.4:1 polyvinylidene fluoride and modified PVDF-HFP copolymer) in sequence, homogenize, and obtain a positive electrode slurry with a solid content of 50wt%; S2: Wash the aluminum foil current collector with ethanol; then apply the positive electrode slurry on its surface, compact and dry to obtain a lithium cobalt oxide positive electrode sheet.
[0041] Embodiment 3: A method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery, comprising the following steps:
[0042] Step 1: Preparation of positive electrode material: S1: Grind and blend iron-based graphene, cobalt oxide and lithium carbonate, and heat-treat at 950° C. for 10 hours to obtain composite lithium cobaltate; in the composite lithium cobaltate, the molar ratio of cobalt in cobalt oxide to lithium in lithium carbonate is 1.8:1.08; the amount of the iron-based graphene introduced accounts for 2wt% of the total mass of cobalt oxide and lithium carbonate;
[0043] S2: Disperse the composite lithium cobaltate in a 0.4 mol / L lanthanum trichloride aqueous solution, the ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g:2.5 mL, stir at room temperature for 24 hours, wash and dry; heat treat the obtained material at 600°C for 6 hours, and after cooling, microwave pulse for 4 seconds at a power of 900 W to obtain a positive electrode material;
[0044] Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add 0.6 parts of dispersant (modified lignin and sodium polyacrylate in a mass ratio of 0.4:0.2) into the solvent and disperse evenly; add 2.5 parts of conductive agent, 94 parts of positive electrode material, and 2.9 parts of binder (polyvinylidene fluoride and modified PVDF-HFP copolymer in a ratio of 2:0.9) in sequence, homogenize, and obtain a positive electrode slurry with a solid content of 50wt%; S2: Wash the aluminum foil current collector with ethanol; then apply the positive electrode slurry on its surface, compact and dry it to obtain a lithium cobalt oxide positive electrode sheet.
[0045] Comparative Example 1: Graphene is used instead of iron-based graphene, and the rest is the same as Example 3; the details are as follows:
[0046] Step 1: Preparation of positive electrode materials: S1: Grind and blend graphene, cobalt oxide, and lithium carbonate, and heat-treat them at 950° C. for 10 hours to obtain composite lithium cobalt oxide; in the composite lithium cobalt oxide, the molar ratio of cobalt in cobalt oxide to lithium in lithium carbonate is 1.8:1.08; the amount of graphene introduced accounts for 2wt% of the total mass of cobalt oxide and lithium carbonate;
[0047] S2: Disperse the composite lithium cobaltate in a 0.4 mol / L lanthanum trichloride aqueous solution, the ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g:2.5 mL, stir at room temperature for 24 hours, wash and dry; heat treat the obtained material at 600°C for 6 hours, and after cooling, microwave pulse for 4 seconds at a power of 900 W to obtain a positive electrode material;
[0048] Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add 0.6 parts of dispersant (modified lignin and sodium polyacrylate in a mass ratio of 0.4:0.2) into the solvent and disperse evenly; add 2.5 parts of conductive agent, 94 parts of positive electrode material, and 2.9 parts of binder (polyvinylidene fluoride and modified PVDF-HFP copolymer in a ratio of 2:0.9) in sequence, homogenize, and obtain a positive electrode slurry with a solid content of 50wt%; S2: Wash the aluminum foil current collector with ethanol; then apply the positive electrode slurry on its surface, compact and dry it to obtain a lithium cobalt oxide positive electrode sheet.
[0049] Comparative Example 2: The positive electrode material is not subjected to microwave pulse treatment, and the rest is the same as Example 3; the details are as follows:
[0050] Step 1: Preparation of positive electrode material: S1: Grind and blend iron-based graphene, cobalt oxide and lithium carbonate, and heat-treat at 950° C. for 10 hours to obtain composite lithium cobaltate; in the composite lithium cobaltate, the molar ratio of cobalt in cobalt oxide to lithium in lithium carbonate is 1.8:1.08; the amount of the iron-based graphene introduced accounts for 2wt% of the total mass of cobalt oxide and lithium carbonate;
[0051] S2: Disperse the composite lithium cobaltate in a 0.4 mol / L lanthanum trichloride aqueous solution, the ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g:2.5 mL, stir at room temperature for 24 hours, wash and dry; heat treat the obtained material at 600°C for 6 hours, and cool to obtain a positive electrode material;
[0052] Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add 0.6 parts of dispersant (modified lignin and sodium polyacrylate in a mass ratio of 0.4:0.2) into the solvent and disperse evenly; add 2.5 parts of conductive agent, 94 parts of positive electrode material, and 2.9 parts of binder (polyvinylidene fluoride and modified PVDF-HFP copolymer in a ratio of 2:0.9) in sequence, homogenize, and obtain a positive electrode slurry with a solid content of 50wt%; S2: Wash the aluminum foil current collector with ethanol; then apply the positive electrode slurry on its surface, compact and dry it to obtain a lithium cobalt oxide positive electrode sheet.
[0053] Comparative Example 3: Polyvinyl pyrrolidone was used instead of modified lignin, and the rest was the same as Example 3; the details are as follows:
[0054] Step 1: Preparation of positive electrode material: S1: Grind and blend iron-based graphene, cobalt oxide and lithium carbonate, and heat-treat at 950° C. for 10 hours to obtain composite lithium cobaltate; in the composite lithium cobaltate, the molar ratio of cobalt in cobalt oxide to lithium in lithium carbonate is 1.8:1.08; the amount of the iron-based graphene introduced accounts for 2wt% of the total mass of cobalt oxide and lithium carbonate;
[0055] S2: Disperse the composite lithium cobaltate in a 0.4 mol / L lanthanum trichloride aqueous solution, the ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g:2.5 mL, stir at room temperature for 24 hours, wash and dry; heat treat the obtained material at 600°C for 6 hours, and after cooling, microwave pulse for 4 seconds at a power of 900 W to obtain a positive electrode material;
[0056] Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add 0.6 parts of dispersant (polyvinyl pyrrolidone and sodium polyacrylate in a mass ratio of 0.4:0.2) into the solvent and disperse evenly; add 2.5 parts of conductive agent, 94 parts of positive electrode material, and 2.9 parts of binder (2:0.9 polyvinylidene fluoride and modified PVDF-HFP copolymer) in sequence, homogenize, and obtain a positive electrode slurry with a solid content of 50wt%; S2: Wash the aluminum foil current collector with ethanol; then apply the positive electrode slurry on its surface, compact and dry it to obtain a lithium cobalt oxide positive electrode sheet.
[0057] Comparative Example 4: Polyvinylidene fluoride is used as the binder alone, and the rest is the same as Example 3; the details are as follows:
[0058] Step 1: Preparation of positive electrode material: S1: Grind and blend iron-based graphene, cobalt oxide and lithium carbonate, and heat-treat at 950° C. for 10 hours to obtain composite lithium cobaltate; in the composite lithium cobaltate, the molar ratio of cobalt in cobalt oxide to lithium in lithium carbonate is 1.8:1.08; the amount of the iron-based graphene introduced accounts for 2wt% of the total mass of cobalt oxide and lithium carbonate;
[0059] S2: Disperse the composite lithium cobaltate in a 0.4 mol / L lanthanum trichloride aqueous solution, the ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g:2.5 mL, stir at room temperature for 24 hours, wash and dry; heat treat the obtained material at 600°C for 6 hours, and after cooling, microwave pulse for 4 seconds at a power of 900 W to obtain a positive electrode material;
[0060] Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add 0.6 parts of dispersant (modified lignin and sodium polyacrylate in a mass ratio of 0.4:0.2) into the solvent and disperse evenly; add 2.5 parts of conductive agent, 94 parts of positive electrode material, and 2.9 parts of polyvinylidene fluoride in sequence, homogenize, and obtain a positive electrode slurry with a solid content of 50wt%; S2: Wash the aluminum foil current collector with ethanol; then apply the positive electrode slurry on its surface, compact and dry to obtain a lithium cobalt oxide positive electrode sheet.
[0061] Performance test: The embodiment and the comparative example were used to prepare a lithium cobalt oxide positive electrode sheet (with a loading of 4.5 mg / cm 2 ) was assembled with a polypropylene separator, metal lithium as the negative electrode, and 1 mol / L lithium hexafluorophosphate electrolyte (the solvent was ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a volume ratio of 1:1:1) to form a button cell, and an electrochemical test was performed to test its capacity retention rate and discharge capacity after 200 cycles at a voltage range of 4.6V; the obtained data are shown in the following table:
[0062]
[0063] Conclusion: The data in the above table show that the present application has prepared a lithium cobalt oxide positive electrode sheet with excellent electrical performance and cycle stability. From the performance of comparative examples 1 to 4, it can be found that metal-based graphene has better improvement on the electrical performance of the positive electrode sheet than ordinary graphene; the use of microwave pulse treatment can reduce the defects of the positive electrode material and further improve the electrical cycle performance of the lithium cobalt oxide positive electrode sheet; and the setting of a two-component dispersant containing modified lignin and a two-component binder containing a modified PVDF-HFP copolymer can effectively improve the stability and electrical performance of the lithium cobalt oxide positive electrode sheet, and effectively improve its service life in lithium batteries.
[0064] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery, characterized in that: The following steps are involved: Step 1: Preparation of positive electrode material: S1: Grind and blend iron-based graphene, cobalt oxide and lithium carbonate, and heat treat them at 950-1000°C for 8-10 hours to obtain composite lithium cobalt oxide; S2: Disperse the composite lithium cobalt oxide in a lanthanum chloride aqueous solution, stir at room temperature for 24 hours, wash and dry; Heat treat the obtained material at 500-600°C for 6 hours, and after cooling, microwave pulse at a power of 800-900W for 2-5 seconds to obtain a positive electrode material; Step 2: Preparation of lithium cobalt oxide positive electrode sheet: S1: Add dispersant to solvent and disperse evenly; add conductive agent, positive electrode material and binder in sequence, homogenize and obtain positive electrode slurry; S2: Wash aluminum foil current collector with ethanol; then apply positive electrode slurry on its surface, compact and dry to obtain lithium cobalt oxide positive electrode sheet; The dispersant comprises modified lignin and sodium polyacrylate in a mass ratio of 0.3-0.4:0.2-0.3; The modified lignin comprises the following raw materials: by weight, 11 to 12 parts of N-vinyl pyrrolidone, 8 to 10 parts of glycerol allyl ether, 3 to 4 parts of N-(1-(5-fluoropyridin-2-yl) vinyl) acetamide, 0.1 to 0.2 parts of ammonium persulfate, and 14 to 16 parts of sulfonic acid lignin; The binder comprises polyvinylidene fluoride and modified PVDF-HFP copolymer in a mass ratio of 1.5-2.5:0.9-1; In the raw materials of the modified PVDF-HFP copolymer, the mass ratio of PVDF-HFP copolymer, sodium styrene sulfonate, and N-(1-(5-fluoropyridin-2-yl)vinyl)acetamide is 10:0.8-1.5:1.2-1.5; The preparation method of the iron-based graphene is as follows: ultrasonically dispersing graphene oxide in deionized water, adding ferric chloride, sodium molybdate and L-cysteine, stirring for 1 to 2 hours to obtain a mixed solution; transferring the mixed solution to a reactor, heating at 220 to 240° C. for 24 hours, washing and drying to obtain iron-based graphene; wherein the mass ratio of graphene oxide, ferric chloride, sodium molybdate and L-cysteine is 10:1.5 to 2:0.5 to 0.7:3 to 4.
2. The method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery according to claim 1, characterized in that: The solid content of the positive electrode slurry is 40-60wt%; the raw materials of the positive electrode slurry include the following components: by weight, 93-95 parts of positive electrode material, 2-3 parts of conductive agent, 2.4-3.5 parts of binder, and 0.5-0.6 parts of dispersant.
3. The method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery according to claim 1, characterized in that: The preparation method of the modified lignin is: (1) adding alkali lignin to deionized water to obtain a solution with a solid content of 25 to 30 wt%; adding sodium hydroxide to adjust the pH to 10 to 12, adding sodium sulfite and formaldehyde; reacting under high pressure and sealed conditions at 160 to 200° C. for 3 to 5 hours, washing, and drying to obtain sulfonic acid lignin; (2) N-vinyl pyrrolidone, glycerol allyl ether, and N-(1-(5-fluoropyridin-2-yl) vinyl) acetamide are added to deionized water in sequence, and an aqueous ammonium persulfate solution is added dropwise, and the mixture is reacted at 75 to 80° C. for 4 to 6 hours; sulfonic acid lignin is added, the temperature is raised to 90 to 100° C., the mixture is reacted for 4 to 5 hours, and the mixture is washed and dried to obtain modified lignin.
4. The method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery according to claim 3, characterized in that: The raw materials of the sulfonic acid lignin include the following components: by weight, 10 parts of alkali lignin, 4 to 4.2 parts of sodium sulfite, and 1 to 1.2 parts of formaldehyde.
5. The method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery according to claim 1, characterized in that: The preparation method of the modified PVDF-HFP copolymer is as follows: (1) adding the PVDF-HFP copolymer to N-methylpyrrolidone and stirring evenly to obtain a solution A with a solid content of 10 to 15 wt%; (2) adding sodium styrene sulfonate and N-(1-(5-fluoropyridin-2-yl)vinyl)acetamide to dichlorothionyl and stirring evenly to obtain a solution B; (3) mixing the solution A and the solution B, adding cuprous chloride and pentamethyldiethylenetriamine under a nitrogen atmosphere, reacting at 120 to 125° C. for 24 hours, washing and drying to obtain the modified PVDF-HFP copolymer.
6. The method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery according to claim 1, characterized in that: In the composite lithium cobaltate, the molar ratio of cobalt in cobalt tetroxide to lithium in lithium carbonate is 1.8:1.05-1.1; the introduced amount of the iron-based graphene accounts for 1.5-2.5wt% of the total mass of cobalt tetroxide and lithium carbonate.
7. The method for preparing a lithium cobalt oxide positive electrode sheet for a lithium ion battery according to claim 1, characterized in that: The ratio of the composite lithium cobaltate to the lanthanum trichloride aqueous solution is 1 g: 2-3 mL; the concentration of the lanthanum trichloride aqueous solution is 0.4-0.45 mol / L.