A heat-resistant lithium-ion battery separator and preparation method thereof

By synthesizing amphoteric monomers and modified polyaryl ether nitrile and cross-linking with functional polysiloxane, the problem of easy overheating and insufficient flame retardant performance of lithium-ion battery separators at extreme temperatures has been solved, and the separator has achieved heat resistance, flame retardancy Fuel and high ionic conductivity improve battery safety and performance.

CN118448811BActive Publication Date: 2024-10-18HUNAN BOSHENG NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410908654.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-18
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

It is difficult for existing lithium-ion battery separators to meet the requirements of heat resistance, flame retardancy, and high ion conductivity at the same time, resulting in batteries that are prone to overheating, short circuiting, or low charge and discharge efficiency at extreme temperatures.

Method used

The amphoteric monomer was synthesized by reacting 2-diethylaminoethanethiol and 1,3-propane sultone, and combined with tetramethyltetraenylcyclotetrasiloxane and bis(4-chlorophenyl)phosphorus, 2, 6-Dichlorobenzonitrile and hexafluorobisphenol A react to form modified polyaryl ether nitrile and cross-link with functionalized polysiloxane to form a heat-resistant lithium-ion battery separator.

Benefits of technology

It achieves good heat resistance, flame retardancy and high ionic conductivity of the battery separator, reducing the risk of thermal runaway and battery performance bottlenecks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a heat-resistant lithium-ion battery separator and a preparation method thereof, and relates to the technical field of battery separators. When preparing the heat-resistant lithium-ion battery separator, the present invention reacts 2-diethylaminoethanethiol and 1,3-propane sultone to synthesize amphoteric monomers, reacts the amphoteric monomers with tetramethyltetraenylcyclotetrasiloxane to generate amphoteric cyclotetrasiloxane, and reacts octamethylcyclotetrasiloxane, tetramethyltetraenylcyclotetrasiloxane and amphoteric cyclotetrasiloxane to generate functionalized polysiloxane; reacts bis(4-chlorophenyl)phosphine, 2,6-dichlorobenzonitrile, and hexafluorobisphenol A to generate modified polyarylethernitrile; cross-links the modified polyarylethernitrile and functional polysiloxane to prepare a heat-resistant lithium-ion battery separator. The heat-resistant lithium-ion battery separator prepared by the present invention has high ionic conductivity, heat resistance and flame retardancy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery separators, in particular to a heat-resistant lithium-ion battery separator and a preparation method thereof. Background Art

[0002] Battery separator, as one of the core components of lithium-ion batteries, has a direct impact on the safety, stability and service life of the battery. An ideal battery separator should have properties such as heat resistance, flame retardancy and high ionic conductivity to ensure the stability of physical and chemical properties under extreme temperature conditions, prevent thermal runaway caused by battery overheating, and ensure safe and reliable operation of the battery.

[0003] However, existing battery separator technologies often find it difficult to meet these requirements at the same time. Some separators are prone to melting or shrinking at high temperatures, resulting in internal short circuits in the battery and increasing the risk of thermal runaway. In addition, the flame retardant properties of some separator materials are insufficient and cannot effectively slow the spread of fire. Although some separators have good temperature resistance, they are insufficient in ionic conductivity, which affects the charging and discharging efficiency of the battery, thereby reducing the power density and energy utilization of the battery. Therefore, the development of a new type of battery separator material that can withstand extreme temperatures, has good flame retardant properties, and maintains high ionic conductivity is of great significance for improving battery performance and safety. The heat-resistant lithium-ion battery separator prepared by the present invention has good ionic conductivity, heat resistance and flame retardancy. Summary of the invention

[0004] The object of the present invention is to provide a heat-resistant lithium-ion battery separator and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A heat-resistant lithium-ion battery separator. The heat-resistant lithium-ion battery separator is prepared by reacting 2-diethylaminoethanethiol and 1,3-propane sultone to synthesize an amphoteric monomer, reacting the amphoteric monomer and tetramethyltetraenylcyclotetrasiloxane to generate an amphoteric cyclotetrasiloxane, reacting octamethylcyclotetrasiloxane, tetramethyltetraenylcyclotetrasiloxane and an amphoteric cyclotetrasiloxane to generate a functionalized polysiloxane; reacting bis(4-chlorophenyl)phosphine, 2,6-dichlorobenzonitrile and hexafluorobisphenol A to generate a modified polyarylethernitrile; and cross-linking the modified polyarylethernitrile and the functional polysiloxane to prepare a heat-resistant lithium-ion battery separator.

[0007] A method for preparing a heat-resistant lithium-ion battery separator comprises the following steps:

[0008] Tetramethyltetravinylcyclotetrasiloxane, amphoteric monomer and tetrahydrofuran are uniformly mixed in a molar ratio of 1:1.1-1.3:20-30, 2,2-dimethoxy-2-phenylacetophenone in an amount of 0.1-0.3 times the mass of tetramethyltetravinylcyclotetrasiloxane is added, ultrasonication is performed at 20-40kHz for 20-30min, ultraviolet light is irradiated at room temperature, and tetrahydrofuran is removed by rotary evaporation under reduced pressure to obtain amphoteric cyclotetrasiloxane;

[0009] Octamethylcyclotetrasiloxane, amphoteric cyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are uniformly mixed in a mass ratio of 1:1.2-1.5:1.2-1.5, heated to 80-90°C under nitrogen protection, stirred for 30-40min at a stirring speed of 400-500r / min, and continued to heat to 110-120°C, and 0.02-0.03% of the mass of octamethylcyclotetrasiloxane was added with a 25wt% tetramethylammonium hydroxide aqueous solution, and then 0.3-0.4% of the mass of octamethylcyclotetrasiloxane was added with trimethylchlorosilane, and continued to stir for 3-4h, heated to 150°C, reacted for 3-4h, reduced pressure to 2-2.5Kpa, and continued to react for 3-4h to obtain functionalized polysiloxane;

[0010] Add bis(4-chlorophenyl)phosphine, dichlorobenzonitrile, hexafluorobisphenol A and potassium carbonate to a mixed solution of N-methylpyrrolidone and toluene in a molar ratio of 1:1.2-1.3:2:1-1.2, react at 130-140° C. for 2-3 hours, use a water separator to release toluene and generated water, continue to heat to 160-170° C., react for 2-3 hours, filter and wash with pure water for 3-4 times, and vacuum dry at 90-100° C. for 10-12 hours with a vacuum degree of 0.08 MPa to obtain a modified polyarylethernitrile;

[0011] Weigh 1-2 parts of functionalized polysiloxane, 2-3 parts of modified polyarylether nitrile, 0.03-0.05 parts of cesium carbonate, and 100-120 parts of N,N-dimethylformamide in parts by mass, stir the functionalized polysiloxane, modified polyarylether nitrile, cesium carbonate and N,N-dimethylformamide for 1-2 minutes at a stirring speed of 500-600r / min, cast them on a glass plate, and use a four-sided applicator to uniformly push out a 150μm thick wet film, let it stand at 70-80°C for 1-2 hours, then immerse it in isopropanol for 30-40 minutes, then transfer and immerse it in pure water, immerse it twice, and each immersion time is 10-12 hours to obtain a heat-resistant lithium-ion battery separator.

[0012] As an optimization, the ultraviolet light irradiation time in step (1) is 30-40 minutes, the ultraviolet light power is 500W, and the light source distance is 25cm.

[0013] As an optimization, the preparation method of the amphoteric monomer in step (1) is to uniformly mix 2-diethylaminoethanethiol, 1,3-propane sultone and N-methylpyrrolidone in a mass ratio of 1:0.6-0.7:10-15, heat to 120°C and stir for 22-24h, stirring speed 200-300r / min, filter and wash with methanol 5-6 times, vacuum dry at 50°C for 10-12h, vacuum degree of 0.08Mpa, to obtain the amphoteric monomer.

[0014] As an optimization, the N-methylpyrrolidone toluene mixed solution in step (3) is a mixture of N-methylpyrrolidone and toluene, wherein the volume ratio of N-methylpyrrolidone to toluene is 3:1-1.2; and the mass volume ratio of bis(4-chlorophenyl)phosphine to N-methylpyrrolidone toluene mixed solution is 1:20-30.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0016] When preparing a heat-resistant lithium-ion battery separator, the present invention comprises the following steps: reacting 2-diethylaminoethanethiol and 1,3-propane sultone to synthesize an amphoteric monomer; reacting the amphoteric monomer and tetramethyltetraenylcyclotetrasiloxane to generate an amphoteric cyclotetrasiloxane; reacting octamethylcyclotetrasiloxane, tetramethyltetraenylcyclotetrasiloxane and an amphoteric cyclotetrasiloxane to generate a functionalized polysiloxane; reacting bis(4-chlorophenyl)phosphine, 2,6-dichlorobenzonitrile and hexafluorobisphenol A to generate a modified polyarylethernitrile; and cross-linking the modified polyarylethernitrile and the functional polysiloxane to prepare the heat-resistant lithium-ion battery separator.

[0017] Firstly, 2-diethylaminoethanethiol and 1,3-propane sultone are reacted to synthesize amphoteric monomers, the amphoteric monomers and tetramethyltetraenylcyclotetrasiloxane are reacted to generate amphoteric cyclotetrasiloxane, octamethylcyclotetrasiloxane, tetramethyltetraenylcyclotetrasiloxane and amphoteric cyclotetrasiloxane are reacted to generate functionalized polysiloxane, 2-diethylaminoethanethiol and 1,3-propane sultone are reacted to obtain amphoteric monomers containing sulfonic acid groups and nitrogen cations, and the amphoteric monomers are subjected to a thiol-double bond click chemistry reaction to obtain amphoteric monomers. Cyclotetrasiloxane participates in the polymerization of the siloxane main chain. The sulfonic acid anion and quaternary ammonium cation structure contained in the siloxane main chain help promote the dissociation of polysulfides, limit the diffusion of polysulfides and accelerate the transmission of lithium ions, thereby improving the ionic conductivity of the battery separator. The ring-opening polymerization involving tetramethyltetraenylcyclotetrasiloxane makes the siloxane main chain have double bonds, which is convenient for subsequent addition reactions. The siloxane main chain contains a large number of silicon-oxygen bonds, which makes the battery separator have good heat resistance and flame retardancy.

[0018] Secondly, bis(4-chlorophenyl)phosphine, 2,6-dichlorobenzonitrile and hexafluorobisphenol A are reacted to generate fluorine-containing and phosphorus-containing polyarylethernitrile; polyarylethernitrile is a type of polymer with an electron-withdrawing group cyanide on the side chain, and its main chain is composed of an aromatic ring and an ether bond. The rigid benzene ring structure on the main chain gives it excellent mechanical properties, dimensional stability and heat resistance. In addition, polyarylethernitrile has a drip-free self-extinguishing property, a high limiting oxygen index, strong chemical stability, and excellent electrical insulation. The trifluoromethyl group on the side chain can effectively reduce the dielectric constant of the polyarylethernitrile itself, improve heat resistance and flame retardancy, and because the main chain also contains a flame-retardant phosphorus element containing a phosphorus-hydrogen structure, the flame retardancy of the battery separator is further improved.

[0019] Finally, the fluorine-containing and phosphorus-containing polyarylethernitrile and functionalized polysiloxane are cross-linked to form a heat-resistant lithium-ion battery separator. The phosphorus-hydrogen structure on the main chain of the polyarylethernitrile and the double bond structure on the main chain of the siloxane can undergo a phosphine hydrogenation reaction under the action of a catalyst, thereby forming a cross-linked network structure and enhancing the mechanical properties of the battery separator. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] A method for preparing a heat-resistant lithium-ion battery separator, the method comprising the following preparation steps:

[0023] (1) 2-Diethylaminoethanethiol, 1,3-propanesultone and N-methylpyrrolidone were mixed uniformly in a mass ratio of 1:0.6:10, heated to 120°C and stirred for 22 hours at a stirring speed of 300 r / min, filtered and washed with methanol for 6 times, and vacuum dried at 50°C for 12 hours at a vacuum degree of 0.08 MPa to obtain amphoteric monomers;

[0024] (2) Tetramethyltetravinylcyclotetrasiloxane, amphoteric monomer and tetrahydrofuran were mixed uniformly in a molar ratio of 1:1.1:20, 2,2-dimethoxy-2-phenylacetophenone (0.1 times the mass of tetramethyltetravinylcyclotetrasiloxane) was added, ultrasonication was carried out at 20kHz for 30min, ultraviolet light was irradiated at room temperature for 40min, the ultraviolet light power was 500w, the light source distance was 25cm, and tetrahydrofuran was removed by vacuum rotary evaporation to obtain amphoteric cyclotetrasiloxane;

[0025] (3) Octamethylcyclotetrasiloxane, amphoteric cyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane were mixed uniformly in a mass ratio of 1:1.2:1.2, heated to 80°C under nitrogen protection, stirred for 40 min at a stirring speed of 500 r / min, and then heated to 120°C, 0.02% of the mass of octamethylcyclotetrasiloxane in a 25wt% aqueous solution of tetramethylammonium hydroxide was added, and then 0.3% of the mass of octamethylcyclotetrasiloxane in trimethylchlorosilane was added, and the mixture was stirred for 4 h. The mixture was heated to 150°C, reacted for 4 h, and the pressure was reduced to 2.5 KPa, and the reaction was continued for 4 h to obtain a functionalized polysiloxane;

[0026] (4) Add bis(4-chlorophenyl)phosphine, dichlorobenzonitrile, hexafluorobisphenol A and potassium carbonate to a mixed solution of N-methylpyrrolidone and toluene in a molar ratio of 1:1.2:2:1, wherein the volume ratio of N-methylpyrrolidone to toluene is 3:1, and the mass volume ratio of bis(4-chlorophenyl)phosphine to N-methylpyrrolidone and toluene is 1:30, react at 140°C for 3 hours, use a water separator to release toluene and generated water, continue to heat to 170°C, react for 3 hours, filter and wash with pure water for 3 times, and vacuum dry at 100°C for 12 hours with a vacuum degree of 0.08 MPa to obtain a modified polyarylethernitrile;

[0027] (5) Weigh 1 part of functionalized polysiloxane, 2 parts of modified polyarylether nitrile, 0.03 parts of cesium carbonate, and 100 parts of N,N-dimethylformamide by mass; stir the functionalized polysiloxane, modified polyarylether nitrile, cesium carbonate, and N,N-dimethylformamide for 2 min at a stirring speed of 600 r / min, cast them on a glass plate, and use a four-sided coater to uniformly roll out a 150 μm thick wet film. Let it stand at 80°C for 2 h, then immerse it in isopropanol for 40 min, then transfer it to pure water and immerse it twice, each immersion time for 12 h, to obtain a heat-resistant lithium-ion battery separator.

[0028] Example 2

[0029] A method for preparing a heat-resistant lithium-ion battery separator, the method comprising the following preparation steps:

[0030] (1) 2-diethylaminoethanethiol, 1,3-propane sultone and N-methylpyrrolidone were mixed uniformly in a mass ratio of 1:0.6-0.7:10-15, heated to 120°C and stirred for 22-24 hours at a stirring speed of 200-300 r / min, filtered and washed with methanol for 5-6 times, and vacuum dried at 50°C for 10-12 hours at a vacuum degree of 0.08 MPa to obtain amphoteric monomers;

[0031] (2) Tetramethyltetravinylcyclotetrasiloxane, amphoteric monomer and tetrahydrofuran were mixed uniformly in a molar ratio of 1:1.2:25, 2,2-dimethoxy-2-phenylacetophenone (0.2 times the mass of tetramethyltetravinylcyclotetrasiloxane) was added, ultrasonication was carried out at 30kHz for 25 minutes, ultraviolet light was irradiated at room temperature for 35 minutes, the ultraviolet light power was 500w, the light source distance was 25cm, and tetrahydrofuran was removed by vacuum rotary evaporation to obtain amphoteric cyclotetrasiloxane;

[0032] (3) Octamethylcyclotetrasiloxane, amphoteric cyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane were mixed uniformly in a mass ratio of 1:1.3:1.4, heated to 85°C under nitrogen protection, stirred for 35 min at a stirring speed of 450 r / min, and then heated to 115°C, 0.025% of the mass of octamethylcyclotetrasiloxane in a 25wt% aqueous solution of tetramethylammonium hydroxide was added, and then 0.35% of the mass of octamethylcyclotetrasiloxane in trimethylchlorosilane was added, and the mixture was stirred for 3.5 h. The mixture was heated to 150°C, reacted for 3.5 h, and the pressure was reduced to 2.3 KPa, and the reaction was continued for 3.5 h to obtain a functionalized polysiloxane;

[0033] (4) Add bis(4-chlorophenyl)phosphine, dichlorobenzonitrile, hexafluorobisphenol A and potassium carbonate to a mixed solution of N-methylpyrrolidone and toluene in a molar ratio of 1:1.25:2:1.11, wherein the volume ratio of N-methylpyrrolidone to toluene is 3:1, and the mass volume ratio of the mixed solution of bis(4-chlorophenyl)phosphine, N-methylpyrrolidone and toluene is 1:25, react at 135°C for 2.5 hours, use a water separator to release toluene and generated water, continue to heat to 165°C, react for 2.5 hours, filter and wash with pure water for 3 times, and vacuum dry at 95°C for 11 hours with a vacuum degree of 0.08 MPa to obtain a modified polyarylethernitrile;

[0034] (5) Weigh 1 part of functionalized polysiloxane, 2 parts of modified polyarylether nitrile, 0.04 parts of cesium carbonate, and 110 parts of N,N-dimethylformamide by mass; stir the functionalized polysiloxane, modified polyarylether nitrile, cesium carbonate, and N,N-dimethylformamide for 1.5 min at a stirring speed of 550 r / min, cast them on a glass plate, and use a four-sided coater to uniformly roll out a 150 μm thick wet film. Let it stand at 75°C for 1.5 h, then immerse it in isopropanol for 35 min, then transfer it to pure water and immerse it twice, each immersion time for 11 h, to obtain a heat-resistant lithium-ion battery separator.

[0035] Example 3

[0036] A method for preparing a heat-resistant lithium-ion battery separator, the method comprising the following preparation steps:

[0037] (1) 2-diethylaminoethanethiol, 1,3-propanesultone and N-methylpyrrolidone were mixed uniformly in a mass ratio of 1:0.7:15, heated to 120°C and stirred for 22 hours at a stirring speed of 200 r / min, filtered and washed with methanol, and vacuum dried at 50°C for 10 hours at a vacuum degree of 0.08 MPa to obtain amphoteric monomers;

[0038] (2) Tetramethyltetravinylcyclotetrasiloxane, amphoteric monomer and tetrahydrofuran were mixed uniformly in a molar ratio of 1:1.3:30, 2,2-dimethoxy-2-phenylacetophenone (0.3 times the mass of tetramethyltetravinylcyclotetrasiloxane) was added, ultrasonication was carried out at 20kHz for 20 minutes, ultraviolet light was irradiated at room temperature for 30 minutes, the lamp source distance was 25cm, the ultraviolet light power was 500w, and tetrahydrofuran was removed by vacuum rotary evaporation to obtain amphoteric cyclotetrasiloxane;

[0039] (3) Octamethylcyclotetrasiloxane, amphoteric cyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane were mixed uniformly in a mass ratio of 1:1.5:1.5, heated to 80°C under nitrogen protection, stirred for 30 min at a stirring speed of 400 r / min, and then heated to 110°C, 0.03% of the mass of octamethylcyclotetrasiloxane in a 25wt% tetramethylammonium hydroxide aqueous solution was added, and then 0.4% of the mass of octamethylcyclotetrasiloxane in trimethylchlorosilane was added and stirred for 3 h, and then heated to 150°C, reacted for 3 h, reduced pressure to 2 KPa, and continued to react for 3 h to obtain functionalized polysiloxane;

[0040] (4) Add bis(4-chlorophenyl)phosphine, dichlorobenzonitrile, hexafluorobisphenol A and potassium carbonate to a mixed solution of N-methylpyrrolidone and toluene in a molar ratio of 1:1.3:2:1.2, wherein the volume ratio of N-methylpyrrolidone to toluene is 3:1.2, and the mass volume ratio of bis(4-chlorophenyl)phosphine to N-methylpyrrolidone and toluene is 1:30, react at 130°C for 2h, release toluene and generated water using a water separator, continue to heat to 160°C, react for 2h, filter and wash with pure water for 3 times, and vacuum dry at 90°C for 10h with a vacuum degree of 0.08Mpa to obtain a modified polyarylethernitrile;

[0041] (5) Weigh 2 parts of functionalized polysiloxane, 3 parts of modified polyarylether nitrile, 0.05 parts of cesium carbonate, and 120 parts of N,N-dimethylformamide by mass; stir the functionalized polysiloxane, modified polyarylether nitrile, cesium carbonate, and N,N-dimethylformamide for 1 min at a stirring speed of 500 r / min, cast them on a glass plate, and use a four-sided coater to uniformly roll out a 150 μm thick wet film. Let it stand at 70°C for 1 h, then immerse it in isopropanol for 30 min, then transfer it to pure water and immerse it twice, each immersion time for 10 h, to obtain a heat-resistant lithium-ion battery separator.

[0042] Comparative Example 1

[0043] The difference between the preparation method of the heat-resistant lithium-ion battery separator of Comparative Example 1 and that of Example 2 is that there are no steps (1) and (2), and step (3) is modified to uniformly mix octamethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane in a mass ratio of 1:1.4, heat to 85°C under nitrogen protection, stir for 35 min at a stirring speed of 450 r / min, continue to heat to 115°C, add 25 wt% tetramethylammonium hydroxide aqueous solution with a mass ratio of 0.025% of octamethylcyclotetrasiloxane, then add trimethylchlorosilane with a mass ratio of 0.35% of octamethylcyclotetrasiloxane, continue to stir for 3.5 h, heat to 150°C, react for 3.5 h, reduce the pressure to 2.3 KPa, and continue to react for 3.5 h to obtain functionalized polysiloxane.

[0044] Comparative Example 2

[0045] The difference between the preparation method of the heat-resistant lithium-ion battery separator of Comparative Example 2 and Example 2 is that step (5) is modified to add dichlorobenzonitrile, hexafluorobisphenol A and potassium carbonate to the N-methylpyrrolidone toluene mixture in a molar ratio of 1.25:2:1.11, wherein the volume ratio of N-methylpyrrolidone to toluene is 3:1, and the mass volume ratio of bis(4-chlorophenyl)phosphine to the N-methylpyrrolidone toluene mixture is 1:25, react at 135°C for 2.5h, use a water separator to release toluene and generated water, continue to heat to 165°C, react for 2.5h, filter and wash with pure water 3 times, and vacuum dry at 95°C for 11h with a vacuum degree of 0.08Mpa to obtain modified polyarylethernitrile.

[0046] Comparative Example 3

[0047] The difference between the preparation method of the heat-resistant lithium-ion battery separator of Comparative Example 3 and Example 2 is that step (5) is modified to add bis(4-chlorophenyl)phosphine, dichlorobenzonitrile and potassium carbonate to the N-methylpyrrolidone toluene mixture in a molar ratio of 1:1.25:1.11, wherein the volume ratio of N-methylpyrrolidone to toluene is 3:1, and the mass volume ratio of bis(4-chlorophenyl)phosphine and N-methylpyrrolidone toluene mixture is 1:25, react at 135°C for 2.5h, use a water separator to release toluene and generated water, continue to heat to 165°C, react for 2.5h, filter and wash with pure water three times, and vacuum dry at 95°C for 11h with a vacuum degree of 0.08Mpa to obtain modified polyarylethernitrile.

[0048] Test Example 1

[0049] Flame retardant performance test

[0050] Test method: The battery separators prepared in the examples and comparative examples were tested for limiting oxygen index using a JF-3 instrument. The results are shown in Table 1.

[0051] Table 1

[0052]

[0053] From the comparison of the experimental data of Examples 1-3 and Comparative Examples 1-3 in Table 1, it can be found that the heat-resistant lithium-ion battery separator prepared by the present invention has good flame retardant properties.

[0054] By comparison, the limiting oxygen index of Example 1-3 is greater than that of Comparative Example 2-3, indicating that 2-diethylaminoethanethiol and 1,3-propane sultone are reacted to synthesize amphoteric monomers, the amphoteric monomers and tetramethyltetraenylcyclotetrasiloxane are reacted to generate amphoteric cyclotetrasiloxane, and octamethylcyclotetrasiloxane, tetramethyltetraenylcyclotetrasiloxane and amphoteric cyclotetrasiloxane are reacted to generate functionalized polysiloxane; the siloxane main chain contains a large number of silicon-oxygen bonds, so that the battery separator has good flame retardant properties; secondly, bis(4-chlorophenyl)phosphine, 2,6-dichlorobenzonitrile and hexafluorobisphenol A are reacted to generate fluorine-containing and phosphorus-containing polyarylethernitrile; the polyarylethernitrile has a self-extinguishing property without dripping, a high limiting oxygen index, and the trifluoromethyl group of the side chain can simultaneously improve the flame retardancy. Since the main chain also contains a flame-retardant phosphorus element containing a phosphorus-hydrogen structure, the flame retardancy of the battery separator is further improved.

[0055] Test Example 2

[0056] Thermal shrinkage performance test

[0057] Test method: The battery separators prepared in each embodiment and comparative example were cut into disc samples with a diameter of 16 mm, and heat-treated at 170°C and 200°C for 0.5 h, respectively, to calculate the thermal shrinkage (η) of the separator at the corresponding temperature. The calculation formula for the thermal shrinkage is η(%)=(S0-S) / S0×100%; where η is the thermal shrinkage of the separator, S0 is the initial area of ​​the separator, and S is the final area of ​​the separator after heat treatment. The results are shown in Table 2.

[0058] Table 2

[0059]

[0060] From the comparison of the experimental data of Examples 1-3 and Comparative Examples 1-3 in Table 2, it can be found that the heat-resistant lithium-ion battery separator prepared by the present invention has good heat resistance.

[0061] By comparison, the thermal shrinkage rates of Examples 1-3 and are less than that of Comparative Examples 1-3, indicating that bis(4-chlorophenyl)phosphine, 2,6-dichlorobenzonitrile and hexafluorobisphenol A are reacted to generate fluorine-containing and phosphorus-containing polyarylethernitrile; polyarylethernitrile is a type of polymer having an electron-withdrawing group cyanide on the side chain, and its main chain is composed of an aromatic ring and an ether bond. The rigid benzene ring structure on the main chain gives it excellent mechanical properties, dimensional stability and heat resistance. In addition, polyarylethernitrile has a self-extinguishing property without dripping, a high limiting oxygen index, strong chemical stability, and excellent electrical insulation. The trifluoromethyl group on the side chain can effectively improve heat resistance.

[0062] Test Example 3

[0063] Ionic conductivity test

[0064] Test method: The battery separators prepared in each embodiment and comparative example were cut into disc samples with a diameter of 16 mm, and the ionic conductivity of the battery separators prepared in each embodiment and comparative example was calculated by electrochemical impedance spectroscopy using a CHI760E electrochemical workstation. Two stainless steel discs with a diameter of 15.8 mm were used as electrodes, and a simple simulated battery was assembled in the order of stainless steel disc / diaphragm soaked in electrolyte for 12 hours / stainless steel disc. The scanning frequency range was 0.1 Hz to 1 MHz. After measuring its impedance spectrum, its thickness was measured multiple times to take the average value and calculate the ionic conductivity (λ) of the diaphragm at the corresponding temperature; the electrolyte was a mixed solution of ethylene carbonate and dimethyl carbonate containing 1M lithium hexafluorophosphate, and the volume ratio of ethylene carbonate and dimethyl carbonate in the mixed solution of ethylene carbonate and dimethyl carbonate was 1:1. The electrolyte was purchased from Duoduo Reagent Co., Ltd.; the calculation formula of ionic conductivity was: λ= A×dRb, where λ is the ionic conductivity of the diaphragm; A is the area of ​​the stainless steel electrode; d is the thickness of the diaphragm; and Rb is the bulk resistance. The results are shown in Table 3.

[0065] Table 3

[0066]

[0067] From the comparison of the experimental data of Examples 1-3 and Comparative Examples 1-4 in Table 3, it can be found that the heat-resistant lithium-ion battery separator prepared by the present invention has good ion conductivity.

[0068] The ionic conductivity of Examples 1-3 is greater than that of Comparative Example 1, indicating that 2-diethylaminoethanethiol and 1,3-propane sultone are reacted to synthesize amphoteric monomers, the amphoteric monomers and tetramethyltetraenylcyclotetrasiloxane are reacted to generate amphoteric cyclotetrasiloxane, octamethylcyclotetrasiloxane, tetramethyltetraenylcyclotetrasiloxane and amphoteric cyclotetrasiloxane are reacted to generate functionalized polysiloxane, 2-diethylaminoethanethiol and 1,3-propane sultone are reacted to obtain amphoteric monomers containing sulfonic acid groups and nitrogen cations, the amphoteric monomers and tetramethyltetraenylcyclotetrasiloxane are reacted through a thiol-double bond click chemistry reaction to obtain amphoteric cyclotetrasiloxane to participate in the ring-opening polymerization of siloxane, and the sulfonic acid anions and quaternary ammonium cation structures contained in the main chain of the polysiloxane help to promote the dissociation of polysulfides, limit the diffusion of polysulfides and accelerate the transmission of lithium ions, thereby improving the ionic conductivity of the battery separator.

[0069] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a heat-resistant lithium-ion battery separator, characterized in that: The method comprises the following preparation steps: (1) 2-diethylaminoethanethiol, 1,3-propane sultone and N-methylpyrrolidone were mixed uniformly in a mass ratio of 1:0.6-0.7:10-15, heated to 120°C and stirred for 22-24 hours at a stirring speed of 200-300 r / min, filtered and washed with methanol for 5-6 times, and vacuum dried at 50°C for 10-12 hours at a vacuum degree of 0.08 MPa to obtain amphoteric monomers; (2) Tetramethyltetravinylcyclotetrasiloxane, amphoteric monomer and tetrahydrofuran are uniformly mixed in a molar ratio of 1:1.1-1.3:20-30, 2,2-dimethoxy-2-phenylacetophenone in an amount of 0.1-0.3 times the mass of tetramethyltetravinylcyclotetrasiloxane is added, ultrasonication is performed at 20-40kHz for 20-30min, ultraviolet light is irradiated at room temperature, and tetrahydrofuran is removed by vacuum rotary evaporation to obtain amphoteric cyclotetrasiloxane; (3) Octamethylcyclotetrasiloxane, amphoteric cyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are mixed uniformly in a mass ratio of 1:1.2-1.5:1.2-1.5, heated to 80-90°C under nitrogen protection, stirred for 30-40 min at a stirring speed of 400-500 r / min, and then heated to 110-120°C, 0.02-0.03% of the mass of octamethylcyclotetrasiloxane in a 25wt% tetramethylammonium hydroxide aqueous solution is added, and then 0.3-0.4% of the mass of octamethylcyclotetrasiloxane in trimethylchlorosilane is added, and the mixture is stirred for 3-4h, heated to 150°C, reacted for 3-4h, and decompressed to 2-2.5Kpa, and reacted for 3-4h to obtain a functionalized polysiloxane; (4) Add bis(4-chlorophenyl)phosphine, dichlorobenzonitrile, hexafluorobisphenol A and potassium carbonate to a mixed solution of N-methylpyrrolidone and toluene in a molar ratio of 1:1.2-1.3:2:1-1.2, react at 130-140°C for 2-3 hours, use a water separator to release toluene and generated water, continue to heat to 160-170°C, react for 2-3 hours, filter and wash with pure water for 3-4 times, and vacuum dry at 90-100°C for 10-12 hours with a vacuum degree of 0.08 MPa to obtain a modified polyarylethernitrile; (5) Weigh 1-2 parts of functionalized polysiloxane, 2-3 parts of modified polyarylether nitrile, 0.03-0.05 parts of cesium carbonate, and 100-120 parts of N,N-dimethylformamide, by mass, stir the functionalized polysiloxane, modified polyarylether nitrile, cesium carbonate and N,N-dimethylformamide for 1-2 minutes at a stirring speed of 500-600 r / min, cast them on a glass plate, and use a four-sided coater to uniformly roll out a 150 μm thick wet film. Let it stand at 70-80°C for 1-2 hours, then immerse it in isopropanol for 30-40 minutes, then transfer it and immerse it in pure water, immerse it twice, and immerse it for 10-12 hours each time to obtain a heat-resistant lithium-ion battery separator.

2. The method for preparing a heat-resistant lithium-ion battery separator according to claim 1, characterized in that: In step (1), the ultraviolet light irradiation time is 30-40 minutes, the ultraviolet light power is 500w, and the light source distance is 25cm.

3. The method for preparing a heat-resistant lithium-ion battery separator according to claim 2, characterized in that: The N-methylpyrrolidone toluene mixed solution in step (3) is prepared by mixing N-methylpyrrolidone and toluene, wherein the volume ratio of N-methylpyrrolidone to toluene is 3:1-1.2; and the mass volume ratio of bis(4-chlorophenyl)phosphine to N-methylpyrrolidone toluene mixed solution is 1:20-30.

4. A heat-resistant lithium-ion battery separator prepared according to the method for preparing a heat-resistant lithium-ion battery separator according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Ultrathin efficient graphene composite film-based lithium carrier and application thereof in lithium metal battery

    CN116936751A

  • Thermally conductive composition and method for preparing the same

    US20070241303A1