A composite activated carbon desulfurizer and its preparation method and application

By modifying activated carbon and actoliite and loading iron, zinc, bismuth and other components to form a composite desulfurizer, the problem of insufficient recycle and penetration of activated carbon desulfurizer in the prior art is solved, and the problem of insufficient recycle of activated carbon desulfurizer in the prior art is achieved. Efficient removal of organic and inorganic sulfur improves desulfurization accuracy and recycling performance.

CN118454685BActive Publication Date: 2024-11-05JIANGSU ZHUHAI ACTIVATED CARBON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410910352.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-05
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

In the prior art, activated carbon desulfurization agents have shortcomings in the number of cycles and penetration of sulfur capacity, and it is difficult to efficiently remove organic and inorganic sulfur common in the industry, and the desulfurization accuracy and recycling performance need to be further improved.

Method used

By using the preparation method of composite activated carbon desulfurization agent, by modifying activated carbon and citrolith materials, and loading active components such as iron, zinc and bismuth in turn to form a composite carrier with high adsorption capacity, improving desulfurization performance and recycling life.

Benefits of technology

It realizes high-precision removal of organic and inorganic sulfur, and can maintain a high desulfurization effect after 50 cycles, improving treatment efficiency and recycling performance, and reducing usage costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a composite activated carbon desulfurizer and a preparation method and application thereof. The preparation of the desulfurizer includes the steps of preparing activated carbon, modifying activated carbon, preparing modified rectorite, preparing a composite carrier, loading iron, loading zinc, loading bismuth, etc. The composite activated carbon desulfurizer provided by the present invention uses activated carbon and rectorite as main carriers, and sequentially impregnates and loads active components such as iron, zinc, and bismuth. The composite activated carbon desulfurizer provided by the present invention can be obtained by simple impregnation loading, has excellent desulfurization performance and cycle life, has controllable cost, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of desulfurization, and specifically relates to a composite activated carbon desulfurizer and a preparation method and application thereof. Background Art

[0002] Hydrogen sulfide is a toxic and harmful colorless acidic gas with the smell of rotten eggs. Hydrogen sulfide is formed in a wide range of ways and is mainly found in natural gas, coke oven gas and petroleum cracking gas. According to the causes of its formation, the sources of hydrogen sulfide in nature can be divided into three categories: (1) biological origin, including biodegradation and microbial sulfate reduction; biological hydrogen sulfide is generated by anaerobic or facultative microbial assimilation and reduction metabolism of sulfur-containing organic compounds or by sulfate-reducing bacteria's dissimilatory reduction metabolism of sulfate; (2) thermochemical origin, including thermal cracking and thermochemical reduction of sulfate; hydrogen sulfide generated by thermal cracking is formed by the breakage of sulfur-containing heterocyclic rings in sulfur-containing organic compounds under the action of heat; (3) volcanic eruption origin. The sulfur abundance in the earth's interior is much higher than that in the crust. Magma activity melts rocks deep in the crust and produces volatile components containing hydrogen sulfide. The presence of hydrogen sulfide is harmful to human health on the one hand, and corrosive to equipment, pipes, etc. on the other.

[0003] In addition, as the trend of heavy petroleum becomes more and more obvious, the removal of organic sulfur has become more and more important. Common organic sulfur includes mercaptans, thiophenols and disulfides. In industrial production, how to effectively remove organic sulfur and inorganic sulfur is very important. At present, the desulfurization methods implemented in industry include wet desulfurization (i.e., liquid absorption), dry desulfurization (i.e., powder absorbent or catalyst, etc.), and semi-dry desulfurization; according to the object of desulfurization, desulfurization includes the removal of organic sulfur and the removal of inorganic sulfur. In the prior art, dry desulfurization has been widely used; among them, dry desulfurization includes chemical reaction desulfurization and physical adsorption desulfurization. The chemical reaction method removes sulfides by chemical reaction, and its desulfurization has the characteristics of high desulfurization accuracy and large sulfur capacity; physical adsorption desulfurization mainly removes sulfides by adsorption of the polarity of the adsorbent. The desulfurization by polar adsorption has certain requirements on the polarity of sulfides, and sulfides with low polarity cannot be adsorbed and removed.

[0004] Activated carbon is a type of material widely used in the field of desulfurization. According to the different raw materials, activated carbon can be divided into coal-based activated carbon, wood-based activated carbon, synthetic activated carbon and other types of activated carbon; among them, the preparation sources of wood-based activated carbon include coconut shells, apricot shells, fruit shells, bamboo, etc. In the prior art, the earlier patent results of the applicant's patent name "An activated carbon-based catalyst and its preparation method and application" and the document number "CN117019128B" disclose a desulfurizer prepared by using activated carbon, which can be recycled 20 times and can remove carbonyl sulfide. The number of recycling times needs to be further improved, and the penetration sulfur capacity needs to be further improved; similarly, the patent document CN106925229B provides an iron-zinc-based composite lignin activated carbon desulfurizer, which is composed of lignin activated carbon, iron-zinc solution, iron salt solution, surfactant, alkaline solution, etc., but its sulfur capacity needs to be further improved. Obviously, efficient and cost-controllable desulfurizers still need to be developed and studied. Based on the above considerations, the present invention is proposed. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a composite activated carbon desulfurizer and a preparation method and application thereof, which has high desulfurization accuracy, high penetration sulfur capacity, and can be efficiently recycled 50 times.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A method for preparing a composite activated carbon desulfurizer comprises the following steps:

[0008] (1) Preparation of activated carbon;

[0009] (2) Modification of activated carbon: adding the activated carbon obtained in step (1) into a nitric acid solution, followed by heating and stirring for reaction; after the reaction is completed, washing and drying are performed to obtain modified activated carbon;

[0010] (3) Preparation of modified rectorite: first, the rectorite is washed with dilute hydrochloric acid, then mixed with sodium hydroxide and subjected to high temperature treatment. After the treatment is completed, pre-modified rectorite is obtained; then, the obtained pre-modified rectorite is ground and sieved, added to water, stirred and dispersed evenly, and then silicon dioxide is added, the pH value of the system is adjusted, stirred, centrifuged, washed, and dried, and the modified rectorite is obtained;

[0011] (4) Preparation of a composite carrier: the modified activated carbon obtained in step (2) and the modified rectorite obtained in step (3) are sequentially added into water, stirred, centrifuged and dried to obtain a composite carrier;

[0012] (5) Iron loading: adding the composite support obtained in step (4) to a ferric nitrate solution, shaking and impregnating, and then drying and calcining to obtain a primary loaded catalyst;

[0013] (6) Zinc loading: adding the primary loaded catalyst obtained in step (5) to a zinc nitrate solution, shaking and impregnating, and then drying and calcining to obtain a secondary loaded catalyst;

[0014] (7) Bismuth loading: The secondary loaded catalyst obtained in step (6) is added to the bismuth nitrate solution, shaken and impregnated, then dried and extruded, and finally calcined to obtain a desulfurization agent product.

[0015] Furthermore, in step (1), the preparation of activated carbon includes the following steps: mixing bamboo powder with alkali and carbonizing the mixture, washing and filtering the mixture after cooling, boiling the mixture in hydrochloric acid, washing the mixture until neutral, and drying the mixture to obtain activated carbon;

[0016] The ratio of bamboo powder to alkali is 1:2-3, and the alkali is selected from one or more of sodium hydroxide and potassium hydroxide; the carbonization treatment temperature is 880-895°C, and the carbonization treatment time is 0.5-4h.

[0017] Furthermore, in step (2), the concentration of the nitric acid solution is 25-50 wt %, the temperature of the heating and stirring reaction is 65-85° C., and the time of the heating and stirring reaction is 6-18 h.

[0018] Furthermore, in step (3), the concentration of dilute hydrochloric acid is 5-15wt%, the mass ratio of rectorite to sodium hydroxide is 1:0.2-0.5, the high temperature treatment temperature is 800-810°C, and the treatment time is 0.5-4h;

[0019] The sieve mesh number is 80-150 mesh, the mass ratio of pre-modified rectorite, water and silica is 4-10:100:0.05-0.2, the system pH value is 8-8.4, and the stirring time after adjusting the system pH value is 8-24h.

[0020] Furthermore, in step (4), the mass ratio of modified activated carbon, modified rectorite and water is 1:0.5~2:20~50; the stirring time is 0.5~4h, and the stirring temperature is 25~35°C.

[0021] Furthermore, in step (5), the concentration of the ferric nitrate solution is 0.8-1.2 mol / L, the mass ratio of the composite carrier to the ferric nitrate solution is 1:4-6.5; the calcination temperature is 500-525°C, and the calcination treatment time is 0.5-4h.

[0022] Furthermore, in step (6), the concentration of the zinc nitrate solution is 0.4-0.8 mol / L, the mass ratio of the primary loaded catalyst to the zinc nitrate solution is 1:3-5; the calcination temperature is 500-525°C, and the calcination treatment time is 0.5-4h.

[0023] Furthermore, in step (7), the concentration of the bismuth nitrate solution is 0.3-0.8 mol / L, the mass ratio of the secondary supported catalyst to the bismuth nitrate solution is 1:1-2.5; the calcination temperature is 500-525°C, and the calcination treatment time is 0.5-4h.

[0024] In addition, the present invention also hopes to protect the desulfurizing agent prepared by the above method.

[0025] Furthermore, it is also desired to protect the use of the desulfurizing agent prepared above in desulfurization.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The composite activated carbon desulfurizer provided by the present invention uses activated carbon and rectorite as main carriers, and is sequentially impregnated and loaded with active components such as iron, zinc, and bismuth. It can be obtained by simple impregnation loading and has excellent desulfurization performance and cycle life.

[0028] In the carrier preparation process of the present invention, the activated carbon is made of common bamboo powder and treated with nitric acid. The purpose of this treatment is twofold: one is to facilitate the subsequent composite use with the modified rectorite, and the other is to introduce oxygen-containing groups to improve the adsorption capacity of organic sulfur (forming hydrogen bonds, etc.); the rectorite is sequentially washed with dilute hydrochloric acid, treated with sodium hydroxide at high temperature, and loaded with silicon dioxide. Specifically, the dilute hydrochloric acid washing is mainly to wash away impurities on the surface of the rectorite, which plays a role in preliminary cleaning of the pores; the sodium hydroxide high temperature treatment is to enrich the pores of the rectorite, which plays a role in further activating the pores. Simply mixing and compounding the activated carbon and the rectorite has the disadvantage of relatively poor stability in recycling use, so, The present application also carries out a loading treatment of nano-silicon dioxide on the rectorite. The purpose of this treatment method is: on the one hand, based on the rich hydroxyl groups of silicon dioxide, the adsorption activity of the surface of the rectorite is improved, which is convenient for the efficient loading of the subsequent active components; on the other hand, based on the rich pore structure of the modified rectorite, nano-silicon dioxide is loaded on its surface and in the pores. Since nano-silicon dioxide is rich in hydroxyl groups, and the surface of the activated carbon treated with nitric acid is rich in oxygen-containing groups (such as hydroxyl groups, carboxyl groups, etc.), the two can be combined in the form of hydrogen bonds, ensuring the firmness and durability of the carrier binding, so that the rectorite modified by nano-silicon dioxide can be well combined with the activated carbon to obtain a composite carrier, which increases the service life of the carrier. In addition, there is another reason for selecting silicon dioxide to modify the rectorite, that is, it can also be used as a carrier, which can further increase the load of the active component and ensure the desulfurization effect.

[0029] The composite activated carbon desulfurizer provided by the present invention uses common iron and zinc as desulfurization active components, and selects and uses bismuth as an auxiliary active component, which can further improve the desulfurization effect of the organic sulfur and inorganic sulfur of the desulfurizer, improve the processing efficiency while increasing the processing volume, and improve the recycling performance. The reason for the improvement of this effect is most likely that bismuth improves the number and distribution of acid centers in the desulfurizer.

[0030] In conclusion, the desulfurizer provided by the present invention can remove both inorganic sulfur and organic sulfur such as methyl mercaptan; while achieving high-precision desulfurization, it ensures the performance after up to 50 cycles. DETAILED DESCRIPTION

[0031] Embodiments of the present invention are described in detail below. All embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0032] In various embodiments of the present invention, the silicon dioxide is nano silicon dioxide with a particle size of about 40-50 nm.

[0033] The bamboo raw material comes from Liyang area of ​​Jiangsu Province, and the growth cycle is about 4 years. The bamboo powder obtained in the present invention is obtained by crushing and drying the bamboo raw material; the rectorite is purchased from Hubei Mingliu Rectorite Co., Ltd.

[0034] Other processing methods not described, such as washing, screening, grinding, drying, etc., are conventional technical methods of those skilled in the art; other chemical raw materials are commercially available.

[0035] Embodiment 1: A method for preparing a composite activated carbon desulfurizer comprises the following steps:

[0036] (1) Preparation of activated carbon: Bamboo powder and potassium hydroxide were mixed in a mass ratio of 1:2.5 and carbonized at 890°C for 1.5 h. After cooling, the mixture was washed and filtered, then boiled in hydrochloric acid, washed until neutral, and dried to obtain activated carbon.

[0037] (2) Modification of activated carbon: The activated carbon prepared in step (1) was added to a 45 wt% nitric acid solution, and then heated and stirred at 80°C for 12 h. After the reaction, the modified activated carbon was washed and dried to obtain the modified activated carbon.

[0038] (3) Preparation of modified rectorite: first, the rectorite was washed with 8wt% dilute hydrochloric acid, then mixed with sodium hydroxide in a mass ratio of 1:0.35, and treated at a high temperature of 805°C for 1h. After the treatment, pre-modified rectorite was obtained; then, the obtained pre-modified rectorite was ground and sieved through 100 mesh and added into water, stirred and dispersed evenly, and then nano-silicon dioxide was added. The pH value of the system was adjusted to 8.2, stirred for 12h, and then centrifuged, washed, and dried to obtain modified rectorite; wherein the mass ratio of pre-modified rectorite, water, and silicon dioxide was 5:100:0.08;

[0039] (4) Preparation of a composite carrier: The modified activated carbon obtained in step (2) and the modified rectorite obtained in step (3) are sequentially added into water, stirred at 30° C. for 2.5 h, centrifuged, and dried to obtain a composite carrier; the mass ratio of the modified activated carbon, the modified rectorite, and water is 1:0.8:40;

[0040] (5) Iron loading: The composite support obtained in step (4) was added to a 1 mol / L ferric nitrate solution at a mass ratio of 1:5.5, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2 h) to obtain a primary loaded catalyst;

[0041] (6) Zinc loading: The primary loaded catalyst obtained in step (5) was added to a 0.6 mol / L zinc nitrate solution at a mass ratio of 1:4.5, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2h) to obtain a secondary loaded catalyst;

[0042] (7) Bismuth loading: The secondary loaded catalyst obtained in step (6) was added to a 0.5 mol / L bismuth nitrate solution at a mass ratio of 1:3.5, and the mixture was shaken and impregnated. The mixture was then dried and extruded into strips, and finally calcined (510° C., 2 h) to obtain a desulfurizer product.

[0043] Embodiment 2: A method for preparing a composite activated carbon desulfurizer, comprising the following steps:

[0044] (1) Preparation of activated carbon: Bamboo powder and potassium hydroxide were mixed in a mass ratio of 1:2.4 and carbonized at 895°C for 1 h. After cooling, the mixture was washed and filtered, then boiled in hydrochloric acid, washed until neutral, and dried to obtain activated carbon.

[0045] (2) Modification of activated carbon: The activated carbon prepared in step (1) was added to a 45 wt% nitric acid solution, and then heated and stirred at 80°C for 14 h. After the reaction, the modified activated carbon was washed and dried to obtain the modified activated carbon.

[0046] (3) Preparation of modified rectorite: first, the rectorite was washed with 9wt% dilute hydrochloric acid, then mixed with sodium hydroxide in a mass ratio of 1:0.32, and treated at a high temperature of 810°C for 1h. After the treatment, pre-modified rectorite was obtained; then, the obtained pre-modified rectorite was ground and sieved through 100 mesh and added into water, stirred and dispersed evenly, and then nano-silicon dioxide was added. The pH value of the system was adjusted to 8.3, stirred for 12h, and then centrifuged, washed, and dried to obtain modified rectorite; wherein the mass ratio of pre-modified rectorite, water, and silicon dioxide was 5:100:0.09;

[0047] (4) Preparation of a composite carrier: The modified activated carbon obtained in step (2) and the modified rectorite obtained in step (3) are added to water in sequence, stirred at 35° C. for 2 h, centrifuged, and dried to obtain a composite carrier; the mass ratio of the modified activated carbon, the modified rectorite, and water is 1:1:40;

[0048] (5) Iron loading: The composite support obtained in step (4) was added to a 1 mol / L ferric nitrate solution at a mass ratio of 1:6, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2h) to obtain a primary loaded catalyst;

[0049] (6) Zinc loading: The primary loaded catalyst obtained in step (5) was added to a 0.6 mol / L zinc nitrate solution at a mass ratio of 1:5, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2h) to obtain a secondary loaded catalyst;

[0050] (7) Bismuth loading: The secondary loaded catalyst obtained in step (6) was added to a 0.5 mol / L bismuth nitrate solution at a mass ratio of 1:3, and the mixture was shaken and impregnated. The mixture was then dried and extruded into strips, and finally calcined (510° C., 2 h) to obtain a desulfurizer product.

[0051] Embodiment 3: A method for preparing a composite activated carbon desulfurizer, comprising the following steps:

[0052] (1) Preparation of activated carbon: Bamboo powder and potassium hydroxide were mixed in a mass ratio of 1:2.6 and carbonized at 885°C for 1 h. After cooling, the mixture was washed and filtered, then boiled in hydrochloric acid, washed until neutral, and dried to obtain activated carbon.

[0053] (2) Modification of activated carbon: The activated carbon prepared in step (1) was added to a 45 wt% nitric acid solution, and then heated and stirred at 85°C for 12 h. After the reaction, the modified activated carbon was washed and dried to obtain the modified activated carbon.

[0054] (3) Preparation of modified rectorite: first, the rectorite was washed with 7wt% dilute hydrochloric acid, then mixed with sodium hydroxide in a mass ratio of 1:0.3, and treated at a high temperature of 805°C for 1.5h. After the treatment, pre-modified rectorite was obtained; then, the obtained pre-modified rectorite was ground and sieved through 100 mesh and added into water, stirred and dispersed evenly, and then nano-silicon dioxide was added. The pH value of the system was adjusted to 8.1, stirred for 16h, and then centrifuged, washed, and dried to obtain modified rectorite; wherein the mass ratio of pre-modified rectorite, water, and silicon dioxide was 5:100:0.07;

[0055] (4) Preparation of a composite carrier: The modified activated carbon obtained in step (2) and the modified rectorite obtained in step (3) are sequentially added into water, stirred at 30° C. for 2 h, centrifuged, and dried to obtain a composite carrier; the mass ratio of the modified activated carbon, the modified rectorite, and water is 1:1.1:40;

[0056] (5) Iron loading: The composite support obtained in step (4) was added to a 1 mol / L ferric nitrate solution at a mass ratio of 1:5.2, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2h) to obtain a primary loaded catalyst;

[0057] (6) Zinc loading: The primary loaded catalyst obtained in step (5) was added to a 0.6 mol / L zinc nitrate solution at a mass ratio of 1:4.6, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2h) to obtain a secondary loaded catalyst;

[0058] (7) Bismuth loading: The secondary loaded catalyst obtained in step (6) was added to a 0.5 mol / L bismuth nitrate solution at a mass ratio of 1:3.7, and then shaken and impregnated. After drying, the mixture was extruded into strips, and finally calcined (510° C., 2 h) to obtain a desulfurizer product.

[0059] Comparative Example 1: A method for preparing a composite activated carbon desulfurizer, comprising the following steps:

[0060] (1) Preparation of activated carbon: Bamboo powder and potassium hydroxide were mixed in a mass ratio of 1:2.5 and carbonized at 890°C for 1.5 h. After cooling, the mixture was washed and filtered, then boiled in hydrochloric acid, washed until neutral, and dried to obtain activated carbon.

[0061] (2) Preparation of modified rectorite: first, the rectorite was washed with 8wt% dilute hydrochloric acid, then mixed with sodium hydroxide in a mass ratio of 1:0.35, and treated at a high temperature of 805°C for 1h. After the treatment, pre-modified rectorite was obtained; then, the obtained pre-modified rectorite was ground and sieved through 100 mesh and added into water, stirred and dispersed evenly, and then nano-silicon dioxide was added, the pH value of the system was adjusted to 8.2, stirred for 12h, and then centrifuged, washed, and dried to obtain modified rectorite; wherein the mass ratio of pre-modified rectorite, water, and silicon dioxide was 5:100:0.08;

[0062] (3) Preparation of a composite carrier: The activated carbon obtained in step (1) and the modified rectorite obtained in step (2) are added to water in sequence, stirred at 30° C. for 2.5 h, centrifuged, and dried to obtain a composite carrier; the mass ratio of the modified activated carbon, the modified rectorite, and water is 1:0.8:40;

[0063] (4) Iron loading: The composite support obtained in step (3) was added to a 1 mol / L ferric nitrate solution at a mass ratio of 1:5.5, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2h) to obtain a primary loaded catalyst;

[0064] (5) Zinc loading: The primary loaded catalyst obtained in step (4) was added to a 0.6 mol / L zinc nitrate solution at a mass ratio of 1:4.5, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2h) to obtain a secondary loaded catalyst;

[0065] (6) Bismuth loading: The secondary loaded catalyst obtained in step (5) was added to a 0.5 mol / L bismuth nitrate solution at a mass ratio of 1:3.5, and then shaken and impregnated. After drying, the mixture was extruded into strips, and finally calcined (510° C., 2 h) to obtain a desulfurizer product.

[0066] The difference between Comparative Example 1 and Example 1 is that the activated carbon is not subjected to modification treatment.

[0067] Comparative Example 2: A method for preparing a composite activated carbon desulfurizer, comprising the following steps:

[0068] (1) Preparation of activated carbon: Bamboo powder and potassium hydroxide were mixed in a mass ratio of 1:2.5 and carbonized at 890°C for 1.5 h. After cooling, the mixture was washed and filtered, then boiled in hydrochloric acid, washed until neutral, and dried to obtain activated carbon.

[0069] (2) Modification of activated carbon: The activated carbon prepared in step (1) was added to a 45 wt% nitric acid solution, and then heated and stirred at 80°C for 12 h. After the reaction, the modified activated carbon was washed and dried to obtain the modified activated carbon.

[0070] (3) Preparation of modified rectorite: The rectorite was first washed with 8 wt % dilute hydrochloric acid, then mixed with sodium hydroxide in a mass ratio of 1:0.35, and treated at 805° C. for 1 h. After the treatment, pre-modified rectorite was obtained;

[0071] (4) Preparation of a composite carrier: The modified activated carbon obtained in step (2) and the pre-modified rectorite obtained in step (3) are added to water in sequence, stirred at 30° C. for 2.5 h, centrifuged, and dried to obtain a composite carrier; the mass ratio of the modified activated carbon, the modified rectorite, and water is 1:0.8:40;

[0072] (5) Iron loading: The composite support obtained in step (4) was added to a 1 mol / L ferric nitrate solution at a mass ratio of 1:5.5, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2 h) to obtain a primary loaded catalyst;

[0073] (6) Zinc loading: The primary loaded catalyst obtained in step (5) was added to a 0.6 mol / L zinc nitrate solution at a mass ratio of 1:4.5, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2h) to obtain a secondary loaded catalyst;

[0074] (7) Bismuth loading: The secondary loaded catalyst obtained in step (6) was added to a 0.5 mol / L bismuth nitrate solution at a mass ratio of 1:3.5, and the mixture was shaken and impregnated. The mixture was then dried and extruded into strips, and finally calcined (510° C., 2 h) to obtain a desulfurizer product.

[0075] The difference between Comparative Example 2 and Example 1 is that the rectorite is not subjected to modification treatment with silicon dioxide.

[0076] Comparative Example 3: A method for preparing a composite activated carbon desulfurizer, comprising the following steps:

[0077] (1) Preparation of activated carbon: Bamboo powder and potassium hydroxide were mixed in a mass ratio of 1:2.5 and carbonized at 890°C for 1.5 h. After cooling, the mixture was washed and filtered, then boiled in hydrochloric acid, washed until neutral, and dried to obtain activated carbon.

[0078] (2) Modification of activated carbon: The activated carbon prepared in step (1) was added to a 45 wt% nitric acid solution, and then heated and stirred at 80°C for 12 h. After the reaction, the modified activated carbon was washed and dried to obtain the modified activated carbon.

[0079] (3) Preparation of modified rectorite: first, the rectorite was washed with 8wt% dilute hydrochloric acid, then mixed with sodium hydroxide in a mass ratio of 1:0.35, and treated at a high temperature of 805°C for 1h. After the treatment, pre-modified rectorite was obtained; then, the obtained pre-modified rectorite was ground and sieved through 100 mesh and added into water, stirred and dispersed evenly, and then nano-silicon dioxide was added. The pH value of the system was adjusted to 8.2, stirred for 12h, and then centrifuged, washed, and dried to obtain modified rectorite; wherein the mass ratio of pre-modified rectorite, water, and silicon dioxide was 5:100:0.08;

[0080] (4) Preparation of a composite carrier: The modified activated carbon obtained in step (2) and the modified rectorite obtained in step (3) are sequentially added into water, stirred at 30° C. for 2.5 h, centrifuged, and dried to obtain a composite carrier; the mass ratio of the modified activated carbon, the modified rectorite, and water is 1:0.8:40;

[0081] (5) Iron loading: The composite support obtained in step (4) was added to a 1 mol / L ferric nitrate solution at a mass ratio of 1:5.5, and the mixture was shaken and impregnated, followed by drying and calcination (515°C, 2 h) to obtain a primary loaded catalyst;

[0082] (6) Zinc loading: The primary loaded catalyst obtained in step (5) was added to a 0.6 mol / L zinc nitrate solution at a mass ratio of 1:4.5, and then shaken and impregnated. After drying, the mixture was extruded and finally calcined (515°C, 2h) to obtain a desulfurizer product.

[0083] The difference between Comparative Example 3 and Example 1 is that bismuth is not loaded.

[0084] The desulfurization performance of the desulfurizers prepared in Example 1 and Comparative Examples 1 to 3 was tested. The specific method was as follows: 3 g of the desulfurizers prepared in Example 1 and Comparative Examples 1 to 3 were loaded into a fixed bed, and the temperature was raised to 200 ° C under normal pressure for 3500 h. -1 The mixed gas (hydrogen sulfide 1500ppm, methyl mercaptan 500ppm, hydrogen content 25%, water vapor content 8%, the balance is nitrogen) is introduced at an air velocity for desulfurization. The desulfurizer that has been deactivated by penetration is regenerated by water washing, and then ultrasonically vibrated in deionized water for 15 minutes, dried, and set aside; after recycling for 50 times, the desulfurization performance is tested again. The test results are shown in Tables 1 and 2. Among them, the desulfurization accuracy refers to the sulfur content of the desulfurized tail gas before the sulfur content penetrates during the desulfurization process; the penetration sulfur capacity refers to the capacity of the desulfurizer per unit volume to absorb sulfur while ensuring the process purification index; the sulfur content of the mixed gas after desulfurization is tested in accordance with GB / T28727-2012.

[0085]

[0086]

[0087] It can be seen from Table 1 and Table 2 that the desulfurizer obtained in the embodiment of the present invention has higher desulfurization accuracy and higher breakthrough sulfur capacity than that in Comparative Examples 1 to 3, and still has a higher breakthrough sulfur capacity retention rate after 50 cycles, indicating that the desulfurizer provided by the present invention can not only desulfurize efficiently, but also ensure better recycling, thereby indirectly reducing the cost of use.

[0088] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a composite activated carbon desulfurizer, characterized in that: The method comprises the following steps: (1) preparing activated carbon; (2) modifying the activated carbon: adding the activated carbon prepared in step (1) into a nitric acid solution, followed by heating and stirring for reaction; after the reaction is completed, washing and drying are performed to obtain modified activated carbon; (3) Preparation of modified rectorite: first, wash the rectorite with dilute hydrochloric acid, then mix it with sodium hydroxide and treat it at high temperature. After the treatment, pre-modified rectorite is obtained. Then, the obtained pre-modified rectorite is ground and sieved, added to water, stirred and dispersed evenly, and then silicon dioxide is added to adjust the pH value of the system. After stirring, centrifugation, washing and drying are performed to obtain modified rectorite. (4) Preparation of composite carrier: The modified activated carbon obtained in step (2) and the modified rectorite obtained in step (3) are added to water in sequence, stirred, centrifuged and dried to obtain a composite carrier. (5) Iron loading: The composite carrier obtained in step (4) is added to a ferric nitrate solution, and vibrated. The catalyst is impregnated by shaking, and then dried and calcined to obtain a primary loaded catalyst; (6) zinc loading: the primary loaded catalyst obtained in step (5) is added to a zinc nitrate solution, shaken and impregnated, and then dried and calcined to obtain a secondary loaded catalyst; (7) bismuth loading: the secondary loaded catalyst obtained in step (6) is added to a bismuth nitrate solution, shaken and impregnated, and then dried and extruded, and finally calcined to obtain a desulfurization agent product; wherein, in step (1), the preparation of activated carbon comprises the following steps: mixing bamboo powder with alkali and carbonizing it, washing and filtering it after cooling, then boiling it in hydrochloric acid, and finally washing it to neutral and drying it wherein the ratio of bamboo powder to alkali is 1:2-3, and the alkali is selected from one or more of sodium hydroxide and potassium hydroxide; the carbonization treatment temperature is 880-895°C, and the carbonization treatment time is 0.5-4h; wherein, in step (2), the concentration of nitric acid solution is 25-50wt%, the temperature of heating and stirring reaction is 65-85°C, and the heating and stirring reaction time is 6-18h; wherein, in step (3), the concentration of dilute hydrochloric acid is 5-15wt%, the mass ratio of rectorite to sodium hydroxide is 1:0.2-0.5, the high temperature treatment temperature is 800-810°C, and the treatment time is 0.5-4h; the sieve mesh is 80- 150 mesh, the mass ratio of pre-modified rectorite, water and silicon dioxide is 4-10:100:0.05-0.2, the pH value of the system is 8-8.4, and the stirring time after adjusting the pH value of the system is 8-24 hours; wherein, in step (4), the mass ratio of modified activated carbon, modified rectorite and water is 1:0.5-2:20-50; the stirring time is 0.5-4 hours, and the stirring temperature is 25-35°C; wherein, in step (5), the concentration of ferric nitrate solution is 0.8-1.2 mol / L, the mass ratio of the composite carrier to the ferric nitrate solution is 1:4-6.5; the calcination temperature is 500-525°C, and the calcination treatment time is 0.5-4 hours.

2. The method for preparing a composite activated carbon desulfurizer according to claim 1, characterized in that: In step (6), the concentration of the zinc nitrate solution is 0.4-0.8 mol / L, the mass ratio of the primary loaded catalyst to the zinc nitrate solution is 1:3-5; the calcination temperature is 500-525°C, and the calcination treatment time is 0.5-4h.

3. The method for preparing a composite activated carbon desulfurizer according to claim 1, characterized in that: In step (7), the concentration of the bismuth nitrate solution is 0.3-0.8 mol / L, the mass ratio of the secondary supported catalyst to the bismuth nitrate solution is 1:1-2.5; the calcination temperature is 500-525°C, and the calcination treatment time is 0.5-4h.

4. A desulfurizing agent prepared by the method according to any one of claims 1 to 3.