A high-activity defective bismuth vanadate nanosheet and its preparation method and application

Nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets were prepared through solvothermal reaction and hydrothermal method, and molybdenum disulfide was grown on them, which solved the problem of insufficient activity of bismuth vanadate photocatalyst and achieved efficient photocatalytic performance. promote.

CN118454719BActive Publication Date: 2024-10-29WUHAN POLYTECHNIC UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410549629.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-06
Publication Date
2024-10-29
Estimated Expiration
2044-05-06

AI Technical Summary

Technical Problem

The existing bismuth vanadate-based photocatalysts have low photogenerated carrier separation efficiency, weak redox ability and low solar energy utilization, which limits their application in environmental pollution control.

Method used

Bismuth trichloride, sodium orthovanadate dodecahydrate and a complexing agent are used to perform a solvothermal reaction to prepare nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets, and molybdenum disulfide is grown on them by a hydrothermal method. Formation of highly active defective bismuth vanadate nanosheets enhances its photoresponse range and catalytic activity.

Benefits of technology

The photocatalytic activity of bismuth vanadate is improved, the photoresponse range is expanded, the lifetime and redox ability of photogenerated carriers are improved, and the utilization efficiency of broad-spectrum sunlight is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004823873220000131
    Figure BDA0004823873220000131
  • Figure BDA0004823873220000141
    Figure BDA0004823873220000141
Patent Text Reader

Abstract

The invention discloses a high-activity defective bismuth vanadate nanosheet and its preparation method and application, and relates to the field of photocatalysis technology. When preparing the high-activity defective bismuth vanadate nanosheet, the invention first uses bismuth trichloride, sodium orthovanadate dodecahydrate and a complexing agent for solvent thermal reaction, and then anneals at high temperature in a nitrogen atmosphere to obtain nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheet; prepares nitrogen-doped carbon quantum dots from biomass raw materials by hydrothermal method; loads nitrogen-doped carbon quantum dots on nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheet; grows molybdenum disulfide crystals on nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheet by hydrothermal method to obtain high-activity defective bismuth vanadate nanosheet. The high-activity defective bismuth vanadate nanosheet prepared by the invention has a light response range from ultraviolet to near infrared, high photocatalytic reaction activity, high photogenerated carrier lifetime and ultra-thin thickness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalysis, and in particular to a high-activity defective bismuth vanadate nanosheet and a preparation method and application thereof. Background Art

[0002] In today's rapidly developing world, environmental pollution is becoming increasingly serious. To solve this problem, developing an ideal and reliable environmental pollution control technology has become an urgent problem to be solved. Photocatalytic technology, which can use sunlight to drive reactions to degrade pollutants at room temperature, has emerged. Photocatalytic environmental control technology is a technology that uses renewable solar energy to remove pollutants from the environment. Therefore, photocatalytic technology based on semiconductor materials has received widespread attention.

[0003] Bismuth vanadate has gradually become a research hotspot for photocatalytic materials due to its green and non-toxic properties, strong physicochemical stability and narrow bandgap of 2.4eV. However, the application of bismuth vanadate-based photocatalysts is restricted by its defects such as low separation efficiency of photogenerated carriers, weak redox ability and low solar energy utilization. Based on the above situation, the present invention proposes a high-activity defective bismuth vanadate nanosheet and its preparation method and application. The high-activity defective bismuth vanadate nanosheet prepared by the present invention has a light response range from ultraviolet to near-infrared light, a high photogenerated carrier lifetime, an ultra-thin thickness and a high photocatalytic reaction activity. Summary of the invention

[0004] The purpose of the present invention is to provide a high-activity defective bismuth vanadate nanosheet and a preparation method and application thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A high-activity defective bismuth vanadate nanosheet is prepared by firstly carrying out a solvothermal reaction with bismuth trichloride, sodium orthovanadate dodecahydrate and a complexing agent, and then annealing at high temperature in a nitrogen atmosphere to obtain a nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheet; preparing nitrogen-doped carbon quantum dot powder from biomass raw materials by a hydrothermal method; loading nitrogen-doped carbon quantum dots on nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheet to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheet; and growing molybdenum disulfide on nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheet by a hydrothermal method to obtain a high-activity defective bismuth vanadate nanosheet.

[0007] As an optimization, the complexing agent is lauryltrimethylammonium bromide.

[0008] As an optimization, the biomass raw material is one or more of corn stalks, sorghum stalks, rice stalks, peanut shells, coconut shells, and leaves.

[0009] As an optimization, a method for preparing highly active defective bismuth vanadate nanosheets comprises the following preparation steps:

[0010] (1) bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol are uniformly mixed, stirred at 25-30° C. and 600-800 r / min for 40-60 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride is added, stirred at 25-30° C. and 600-800 r / min for 5-10 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160° C. for 3-4 h, naturally cooled to 20-25° C., centrifuged at 8000-10000 r / min for 10-15 min, collected the precipitate, washed with anhydrous ethanol and deionized water for 5-6 times respectively, dried at 5-10 Pa and 50-60° C. for 10-12 h, and annealed at 340-360° C. in a nitrogen atmosphere at a heating rate of 5° C. / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0011] (2) mixing nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, carbon quantum dot suspension, and deionized water, stirring and refluxing at 85-95° C. and 300-500 r / min for 3-4 hours, cooling naturally to room temperature, and centrifuging at 6000-8000 r / min for 8-12 minutes, washing the collected precipitate with deionized water for 4-6 times, and vacuum drying at 50-60° C. and 5-10 Pa for 6-8 hours to obtain nitrogen-doped carbon quantum dot / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0012] (3) The nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, molybdenum precursor, sulfur precursor and deionized water are mixed uniformly, stirred and dispersed at 20-30° C. and 300-500 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 190-200° C. for 24 h, naturally cooled to room temperature, centrifuged at 6000-8000 r / min for 10-15 min, the collected precipitate is washed with deionized water and ethanol for 4-6 times respectively, and vacuum dried at 5-10 Pa and 50-60° C. for 6-8 h to obtain molybdenum disulfide / nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, that is, high-activity defect state bismuth vanadate nanosheets.

[0013] As an optimization, the preparation method of the carbon quantum dot suspension in step (2) is as follows:

[0014] (A) washing the biomass raw material with deionized water, drying it at 5-10 Pa and 60-80° C. for 8-10 h, and using a high-speed pulverizer to produce a biomass powder with a particle size of less than 2 mm;

[0015] (B) The biomass powder, lysine and deionized water were mixed uniformly in a mass ratio of 1: (0.25-0.3): (45-55), stirred and dispersed at 20-30° C. and 300-500 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 180-200° C. for 12 h, naturally cooled to room temperature, centrifuged at 8000-12000 r / min for 10-15 min, the supernatant was collected, filtered using a 0.22 μm filter membrane, and freeze-dried at -15° C. to obtain nitrogen-doped carbon quantum dot powder;

[0016] (C) The nitrogen-doped carbon quantum dot powder was dispersed in deionized water, and the mixture was stirred at 20-30° C. and 300-500 r / min for 20 min to prepare a 1 mg / ml carbon quantum dot suspension.

[0017] As an optimization, the molar ratio of bismuth trichloride, lauryltrimethylammonium bromide and ethylene glycol in step (1) is 1:(0.4-0.5):(50-60).

[0018] As an optimization, in step (2), the mass ratio of nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, carbon quantum dot suspension, and deionized water is 1:(10-12):(30-40).

[0019] As an optimization, in the step (3), the mass ratio of nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, molybdenum precursor, sulfur precursor, and deionized water is 1:(0.03-0.035):(0.3-0.35):(25-35).

[0020] As an optimization, the molybdenum precursor in step (3) is one of sodium molybdate and hexaammonium heptamolybdate tetrahydrate.

[0021] As an optimization, the sulfur precursor in step (3) is one of thiourea and thioacetamide.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] When preparing high-activity defective bismuth vanadate nanosheets, the present invention firstly uses bismuth trichloride, sodium orthovanadate dodecahydrate and lauryltrimethylammonium bromide to carry out solvent thermal reaction to prepare vanadium vacancy defective bismuth vanadate nanosheets, and then carries out high-temperature annealing in a nitrogen atmosphere to obtain nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets; uses a hydrothermal method to prepare nitrogen-doped carbon quantum dot powder from biomass raw materials; loads nitrogen-doped carbon quantum dots on nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets; and uses a hydrothermal method to grow molybdenum disulfide on nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets to obtain high-activity defective bismuth vanadate nanosheets.

[0024] First, bismuth trichloride and lauryl trimethylammonium bromide are mixed in ethylene glycol, and bismuth trichloride and lauryl trimethylammonium bromide form a complex precursor, so that the layers are separated, and then sodium orthovanadate dodecahydrate is added. Under solvent thermal conditions, vanadate reacts with metal bismuth ions in the precursor to form vanadium vacancy defect state bismuth vanadate nanosheets. Due to the complex layer separation effect of lauryl trimethylammonium bromide, the thickness of the prepared vanadium vacancy defect state bismuth vanadate nanosheet is only 1 to 2 nm. At the same time, due to the short reaction time and the high reaction temperature, the vanadium vacancy defect state bismuth vanadate nanosheet is only 1 to 2 nm thick. Many vanadium vacancy defects are formed on the vacancy defect state bismuth vanadate nanoflakes, and these vanadium vacancy defects provide a large number of active sites for catalytic reactions, thereby improving the photocatalytic activity. The vanadium vacancy defect state bismuth vanadate nanoflakes are then annealed at high temperature in a nitrogen atmosphere to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes. Nitrogen atoms replace oxygen atoms to form nitrogen doping and produce oxygen vacancies. At the same time, the incorporation of nitrogen atoms reduces the bandgap width of the vanadium vacancy defect state bismuth vanadate nanoflakes, and the light response range is red-shifted. The expanded light response range improves the photocatalytic activity.

[0025] Secondly, biomass raw materials and lysine are used to prepare nitrogen-doped carbon quantum dot powder by a hydrothermal method. In the present invention, the use of biomass raw materials reduces costs and provides a new high-value-added application mode for agricultural waste, reducing environmental protection pressure; then the nitrogen-doped carbon quantum dot powder is prepared into a carbon quantum dot suspension, and in a reflux reaction, the carbon quantum dots are loaded on nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes by forming a heterojunction structure with bismuth vanadate to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, and the carbon quantum dots are combined with bismuth vanadate to form a Z-type photocatalyst. Under the irradiation of sunlight, the vanadium The electrons of bismuth vanadate jump from the valence band to the conduction band, leaving photogenerated electron holes in the valence band, and the electrons are transferred to the carbon quantum dots, combining with the adsorbed oxygen to generate oxygen free radicals, inhibiting the recombination of electron-hole pairs and increasing the lifetime of photogenerated carriers. At the same time, carbon quantum dots have upconversion photoluminescence properties, that is, carbon quantum dots can absorb longer wavelength light and then emit shorter wavelength light to excite bismuth vanadate to form electron-hole pairs, giving nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect bismuth vanadate nanosheets a broad spectrum of light response range in ultraviolet light, visible light, and near-infrared light, which can more effectively utilize wide-spectrum sunlight to enhance photocatalytic activity.

[0026] Finally, molybdenum disulfide nanosheets were grown on nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect bismuth vanadate nanosheets suspended in a solution under hydrothermal conditions using molybdenum precursors and sulfur precursors. During the reaction, the excess sulfur precursors made the grown molybdenum disulfide nanosheets have many lattice defects, exposing more edge sulfur atom active sites, and having high photocatalytic activity. At the same time, molybdenum disulfide, carbon quantum dots, and bismuth vanadate formed a double Z-type semiconductor structure. Under sunlight, electrons of molybdenum disulfide jumped from the valence band to the conduction band, leaving a Electron holes, photogenerated electrons are transferred to the valence band of bismuth vanadate, and jump to the conduction band of bismuth vanadate under light, and then captured by carbon quantum dots and combined with adsorbed oxygen to form oxygen free radicals. The photogenerated electron holes remaining on molybdenum disulfide form hydroxyl free radicals with hydroxyl in the solution, or directly participate in redox reactions as reducing agents. The structure of the double Z-type semiconductor reduces the recombination probability of electron-hole pairs, and the thickness close to the single atomic layer reduces the distance of electron migration, improves the utilization rate of photogenerated electrons, and obtains higher photocatalytic activity. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0028] The preparation process of the carbon quantum dot suspension used in all subsequent examples and comparative examples is as follows:

[0029] (A) The biomass raw material was washed with deionized water, dried at 5 Pa and 60° C. for 10 h, and a high-speed pulverizer was used to produce a biomass powder with a particle size of less than 2 mm;

[0030] (B) The biomass powder, lysine and deionized water were mixed in a mass ratio of 1:0.25:50, stirred and dispersed at 25°C and 400 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 200°C for 12 h, naturally cooled to room temperature, centrifuged at 10000 r / min for 10 min, the supernatant was collected, filtered using a 0.22 μm filter membrane, and freeze-dried at -15°C to obtain nitrogen-doped carbon quantum dot powder;

[0031] (C) The nitrogen-doped carbon quantum dot powder was dispersed in deionized water and stirred at 25° C. and 400 rpm for 20 min to prepare a 1 mg / ml carbon quantum dot suspension.

[0032] Example 1

[0033] A method for preparing highly active defective bismuth vanadate nanosheets, the method comprising the following preparation steps:

[0034] (1) bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol were mixed uniformly in a molar ratio of 1:0.4:50, stirred at 25°C and 600 r / min for 40 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 25°C and 600 r / min for 5 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160°C for 3 h, naturally cooled to 20°C, centrifuged at 8000 r / min for 10 min, collected the precipitate, washed 5 times with anhydrous ethanol and deionized water respectively, dried at 5 Pa and 50°C for 10 h, and annealed at 340°C in a nitrogen atmosphere at a heating rate of 5°C / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0035] (2) mixing nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, carbon quantum dot suspension, and deionized water in a mass ratio of 1:10:30, stirring and refluxing at 85°C and 300 r / min for 3 h, cooling naturally to room temperature, and centrifuging at 6000 r / min for 12 min. The collected precipitate was washed 4 times with deionized water, and vacuum dried at 5 Pa and 50°C for 6 h to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0036] (3) Nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, sodium molybdate, thioacetamide, and deionized water were mixed uniformly in a mass ratio of 1:0.03:0.3:25, stirred and dispersed at 20°C and 300 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 190°C for 24 h, naturally cooled to room temperature, centrifuged at 6000 r / min for 10 min, and the collected precipitate was washed 4 times with deionized water and ethanol respectively, and vacuum dried at 5 Pa and 50°C for 6 h to obtain molybdenum disulfide / nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, that is, high-activity defect state bismuth vanadate nanosheets.

[0037] Example 2

[0038] A method for preparing highly active defective bismuth vanadate nanosheets, the method comprising the following preparation steps:

[0039] (1) bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol were mixed uniformly in a molar ratio of 1:0.45:55, stirred at 25°C and 700 r / min for 50 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 25°C and 700 r / min for 5 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160°C for 3 h, naturally cooled to 20°C, centrifuged at 9000 r / min for 12 min, collected the precipitate, washed 5 times with anhydrous ethanol and deionized water respectively, dried at 5 Pa and 55°C for 11 h, and annealed at 350°C in a nitrogen atmosphere at a heating rate of 5°C / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0040] (2) mixing nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, carbon quantum dot suspension, and deionized water in a mass ratio of 1:11:35, stirring and refluxing at 90° C. and 400 r / min for 3.5 h, cooling naturally to room temperature, and centrifuging at 7000 r / min for 10 min. The collected precipitate was washed 5 times with deionized water, and vacuum dried at 5 Pa and 55° C. for 7 h to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0041] (3) Nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, sodium molybdate, thioacetamide, and deionized water were mixed uniformly in a mass ratio of 1:0.032:0.33:30, stirred and dispersed at 25°C and 400 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 195°C for 24 h, naturally cooled to room temperature, centrifuged at 7000 r / min for 12 min, and the collected precipitate was washed 5 times with deionized water and ethanol respectively, and vacuum dried at 5 Pa and 55°C for 7 h to obtain molybdenum disulfide / nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, that is, high-activity defect state bismuth vanadate nanoflakes.

[0042] Example 3

[0043] A method for preparing highly active defective bismuth vanadate nanosheets, the method comprising the following preparation steps:

[0044] (1) bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol were mixed uniformly in a molar ratio of 1:0.5:60, stirred at 30°C and 800 r / min for 60 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 30°C and 800 r / min for 10 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160°C for 4 h, naturally cooled to 25°C, centrifuged at 10000 r / min for 15 min, collected the precipitate, washed with anhydrous ethanol and deionized water for 6 times respectively, dried at 10 Pa and 60°C for 12 h, and annealed at 360°C in a nitrogen atmosphere at a heating rate of 5°C / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0045] (2) mixing nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, carbon quantum dot suspension, and deionized water in a mass ratio of 1:12:40, stirring and reflux at 95° C. and 500 r / min for 4 h, cooling naturally to room temperature, and centrifuging at 8000 r / min for 8 min. The collected precipitate was washed 6 times with deionized water, and vacuum dried at 10 Pa and 60° C. for 8 h to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0046] (3) Nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, sodium molybdate, thioacetamide, and deionized water were mixed uniformly in a mass ratio of 1:0.035:0.35:35, stirred and dispersed at 30°C and 500 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 200°C for 24 h, naturally cooled to room temperature, centrifuged at 8000 r / min for 15 min, and the collected precipitate was washed with deionized water and ethanol for 6 times respectively, and vacuum dried at 10 Pa and 60°C for 8 h to obtain molybdenum disulfide / nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, that is, high-activity defect state bismuth vanadate nanoflakes.

[0047] Comparative Example 1

[0048] A method for preparing highly active defective bismuth vanadate nanosheets, the method comprising the following preparation steps:

[0049] (1) bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol were mixed uniformly in a molar ratio of 1:0.45:55, stirred at 25°C and 700 r / min for 50 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 25°C and 700 r / min for 5 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 120°C for 12 h, naturally cooled to 20°C, centrifuged at 9000 r / min for 12 min, collected the precipitate, washed with anhydrous ethanol and deionized water for 5 times respectively, dried at 5 Pa and 55°C for 11 h, and annealed at 350°C in a nitrogen atmosphere at a heating rate of 5°C / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0050] (2) mixing nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, carbon quantum dot suspension, and deionized water in a mass ratio of 1:11:35, stirring and refluxing at 90° C. and 400 r / min for 3.5 h, cooling naturally to room temperature, and centrifuging at 7000 r / min for 10 min. The collected precipitate was washed 5 times with deionized water, and vacuum dried at 5 Pa and 55° C. for 7 h to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0051] (3) Nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, sodium molybdate, thioacetamide, and deionized water were mixed uniformly in a mass ratio of 1:0.032:0.33:30, stirred and dispersed at 25°C and 400 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 195°C for 24 h, naturally cooled to room temperature, centrifuged at 7000 r / min for 12 min, and the collected precipitate was washed 5 times with deionized water and ethanol respectively, and vacuum dried at 5 Pa and 55°C for 7 h to obtain molybdenum disulfide / nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, that is, high-activity defect state bismuth vanadate nanoflakes.

[0052] Comparative Example 2

[0053] A method for preparing highly active defective bismuth vanadate nanosheets, the method comprising the following preparation steps:

[0054] (1) bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol were mixed uniformly in a molar ratio of 1:0.45:55, stirred at 25°C and 700 r / min for 50 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 25°C and 700 r / min for 5 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160°C for 3 h, naturally cooled to 20°C, centrifuged at 9000 r / min for 12 min, collected the precipitate, washed 5 times with anhydrous ethanol and deionized water respectively, and dried at 5 Pa and 55°C for 11 h to obtain vanadium vacancy defect state bismuth vanadate nanosheets;

[0055] (2) mixing vanadium vacancy defect state bismuth vanadate nanosheets, carbon quantum dot suspension, and deionized water in a mass ratio of 1:11:35, stirring and reflux at 90° C. and 400 r / min for 3.5 h, cooling naturally to room temperature, and centrifuging at 7000 r / min for 10 min. The collected precipitate was washed 5 times with deionized water, and vacuum dried at 5 Pa and 55° C. for 7 h to obtain nitrogen-doped carbon quantum dots / vanadium vacancy defect state bismuth vanadate nanosheets;

[0056] (3) Nitrogen-doped carbon quantum dots / vanadium vacancy defective bismuth vanadate nanosheets, sodium molybdate, thioacetamide, and deionized water were mixed uniformly in a mass ratio of 1:0.032:0.33:30, stirred and dispersed at 25°C and 400 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 195°C for 24 h, naturally cooled to room temperature, centrifuged at 7000 r / min for 12 min, and the collected precipitate was washed 5 times with deionized water and ethanol respectively, and vacuum dried at 5 Pa and 55°C for 7 h to obtain molybdenum disulfide / nitrogen-doped carbon quantum dots / vanadium vacancy defective bismuth vanadate nanosheets, that is, high-activity defective bismuth vanadate nanosheets.

[0057] Comparative Example 3

[0058] A method for preparing highly active defective bismuth vanadate nanosheets, the method comprising the following preparation steps:

[0059] (1) bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol were mixed uniformly in a molar ratio of 1:0.45:55, stirred at 25°C and 700 r / min for 50 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 25°C and 700 r / min for 5 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160°C for 3 h, naturally cooled to 20°C, centrifuged at 9000 r / min for 12 min, collected the precipitate, washed 5 times with anhydrous ethanol and deionized water respectively, dried at 5 Pa and 55°C for 11 h, and annealed at 350°C in a nitrogen atmosphere at a heating rate of 5°C / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0060] (2) Nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, sodium molybdate, thioacetamide, and deionized water were mixed uniformly in a mass ratio of 1:0.032:0.33:30, stirred and dispersed at 25°C and 400 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 195°C for 24 h, naturally cooled to room temperature, centrifuged at 7000 r / min for 12 min, and the collected precipitate was washed 5 times with deionized water and ethanol respectively, and vacuum dried at 5 Pa and 55°C for 7 h to obtain molybdenum disulfide / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, that is, high-activity defect state bismuth vanadate nanoflakes.

[0061] Comparative Example 4

[0062] A method for preparing highly active defective bismuth vanadate nanosheets, the method comprising the following preparation steps:

[0063] (1) bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol were mixed uniformly in a molar ratio of 1:0.45:55, stirred at 25°C and 700 r / min for 50 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 25°C and 700 r / min for 5 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160°C for 3 h, naturally cooled to 20°C, centrifuged at 9000 r / min for 12 min, collected the precipitate, washed 5 times with anhydrous ethanol and deionized water respectively, dried at 5 Pa and 55°C for 11 h, and annealed at 350°C in a nitrogen atmosphere at a heating rate of 5°C / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0064] (2) The nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, carbon quantum dot suspension and deionized water were mixed uniformly in a mass ratio of 1:11:35, stirred and refluxed at 90°C and 400 r / min for 3.5 h, naturally cooled to room temperature, and centrifuged at 7000 r / min for 10 min. The collected precipitate was washed 5 times with deionized water, and vacuum dried at 5Pa and 55°C for 7 h to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, that is, highly active defect state bismuth vanadate nanoflakes.

[0065] Comparative Example 5

[0066] A method for preparing highly active defective bismuth vanadate nanosheets, the method comprising the following preparation steps:

[0067] (1) bismuth trichloride and ethylene glycol were mixed uniformly in a molar ratio of 1:0.45:55, stirred at 25°C and 700 r / min for 50 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 25°C and 700 r / min for 5 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160°C for 3 h, naturally cooled to 20°C, centrifuged at 9000 r / min for 12 min, collected the precipitate, washed with anhydrous ethanol and deionized water for 5 times respectively, dried at 5 Pa and 55°C for 11 h, and annealed at 350°C in a nitrogen atmosphere at a heating rate of 5°C / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0068] (2) mixing nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, carbon quantum dot suspension, and deionized water in a mass ratio of 1:11:35, stirring and refluxing at 90° C. and 400 r / min for 3.5 h, cooling naturally to room temperature, and centrifuging at 7000 r / min for 10 min. The collected precipitate was washed 5 times with deionized water, and vacuum dried at 5 Pa and 55° C. for 7 h to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets;

[0069] (3) Nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, sodium molybdate, thioacetamide, and deionized water were mixed uniformly in a mass ratio of 1:0.032:0.33:30, stirred and dispersed at 25°C and 400 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 195°C for 24 h, naturally cooled to room temperature, centrifuged at 7000 r / min for 12 min, and the collected precipitate was washed 5 times with deionized water and ethanol respectively, and vacuum dried at 5 Pa and 55°C for 7 h to obtain molybdenum disulfide / nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, that is, high-activity defect state bismuth vanadate nanoflakes.

[0070] Test Example 1

[0071] Nanosheet thickness test: The thickness of highly active defective bismuth vanadate nanosheets was measured using an atomic force microscope.

[0072] The results are shown in Table 1.

[0073] Table 1

[0074] thickness thickness Example 1 1.28nm Comparative Example 1 1.31nm Example 2 1.33nm Comparative Example 2 1.23nm Example 3 1.29nm Comparative Example 3 1.24nm Comparative Example 4 1.30nm Comparative Example 5 7.45nm

[0075] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 1, it can be found that the high-activity defective bismuth vanadate nanosheets prepared by the present invention have an extremely thin thickness.

[0076] By comparison, the thickness of Examples 1 to 3 is less than that of Comparative Example 5, indicating that the addition of lauryltrimethylammonium bromide forms a complex with bismuth trichloride during the hydrothermal stage of step (1) to separate the layers, thereby successfully preparing ultra-thin high-activity defective bismuth vanadate nanosheets.

[0077] Test Example 2

[0078] Light response range test: The UV-2550 UV-visible spectrophotometer from Shimadzu Corporation was used to measure the UV-visible diffuse reflectance spectrum and UV-visible absorption spectrum of the highly active defective bismuth vanadate nanoflakes. The spectrum was recorded in the scanning range of 200 to 1000 nm, and the light absorption edge obtained from the spectrum and the average absorbance in the wavelength range of 600 to 1000 nm were recorded.

[0079] The results are shown in Table 2.

[0080] Table 2

[0081] Light absorption edge Average absorbance in the wavelength range of 600 to 1000 nm Example 1 532nm 31.23% Example 2 535nm 32.67% Example 3 533nm 31.48% Comparative Example 1 531nm 25.19% Comparative Example 2 525nm 27.68% Comparative Example 3 519nm 9.51% Comparative Example 4 520nm 23.76% Comparative Example 5 530nm 30.94%

[0082] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 2, it can be found that the light response range of the highly active defective bismuth vanadate nanosheets prepared by the present invention has a red shift, and at the same time exhibits strong absorption in the wavelength range of 600 to 1000 nm.

[0083] By comparison, the average absorbance in the wavelength range of 600 to 1000 nm of Examples 1 to 3 is greater than the average absorbance in the wavelength range of 600 to 1000 nm of Comparative Example 1, indicating that the vanadium vacancy defects introduced by the higher reaction temperature and shorter reaction time on the highly active defective bismuth vanadate nanoflakes can improve the absorption and utilization efficiency of long-wavelength light.

[0084] By comparison, the light absorption edge and the average absorbance in the wavelength range of 600 to 1000 nm of Examples 1 to 3 are greater than the light absorption edge and the average absorbance in the wavelength range of 600 to 1000 nm of Comparative Example 2, indicating that nitrogen doping of highly active defective bismuth vanadate nanoflakes can red-shift its light response range and improve the absorption and utilization efficiency of long-wavelength light.

[0085] By comparison, the light absorption edge of Examples 1 to 3 and the average absorbance in the wavelength range of 600 to 1000 nm are greater than the light absorption edge of Comparative Example 3 and the average absorbance in the wavelength range of 600 to 1000 nm, indicating that loading carbon quantum dots on highly active defective bismuth vanadate nanoflakes can red-shift its light response range, and the up-conversion luminescence characteristics of carbon quantum dots can also greatly improve the absorption and utilization efficiency of long-wavelength light.

[0086] By comparison, the light absorption edge of Examples 1 to 3 and the average absorbance in the wavelength range of 600 to 1000 nm are greater than the light absorption edge of Comparative Example 4 and the average absorbance in the wavelength range of 600 to 1000 nm, indicating that loading molybdenum disulfide on highly active defective bismuth vanadate nanoflakes can red-shift its light response range and improve the absorption and utilization efficiency of long-wavelength light.

[0087] Test Example 3

[0088] Vanadium vacancy determination: Use an X-ray fluorescence spectrometer to measure the X-ray fluorescence spectrum of the highly active defective bismuth vanadate nanoflakes, and calculate and record the molar ratio of vanadium to bismuth in the sample from the obtained X-ray fluorescence spectrum.

[0089] The results are shown in Table 3.

[0090] Table 3

[0091] Vanadium / Bismuth molar ratio Vanadium / Bismuth molar ratio Example 1 0.912 Comparative Example 1 0.987 Example 2 0.918 Comparative Example 2 0.914 Example 3 0.921 Comparative Example 3 0.907 Comparative Example 4 0.916 Comparative Example 5 0.919

[0092] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 3, it can be found that the high-activity defective bismuth vanadate nanosheets prepared by the present invention have vanadium vacancy defects.

[0093] By comparison, the vanadium / bismuth molar ratios of Examples 1 to 3 are smaller than that of Comparative Example 1, indicating that using a higher hydrothermal temperature and a shorter reaction time in step (1) can introduce vanadium vacancy defect states on the bismuth vanadate nanosheets.

[0094] Test Example 4

[0095] Photogenerated carrier lifetime test: The time-resolved photoluminescence spectrum of highly active defective bismuth vanadate nanosheets was measured using a fluorescence spectrometer model FLS-920. The photogenerated carrier lifetime of the sample was calculated and recorded. The slits for excitation and emission were both 1 nm.

[0096] The results are shown in Table 4.

[0097] Table 4

[0098]

[0099]

[0100] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 4, it can be found that the highly active defective bismuth vanadate nanosheets prepared by the present invention have a relatively high photogenerated carrier lifetime.

[0101] By comparison, the photogenerated carrier lifetimes of Examples 1 to 3 are greater than that of Comparative Example 1, indicating that the alum vacancies formed by the higher reaction temperature and shorter reaction time in step (1) effectively reduce the recombination probability of photogenerated electron-hole pairs and increase the photogenerated carrier lifetime.

[0102] By comparison, the photogenerated carrier lifetimes of Examples 1 to 3 are greater than that of Comparative Example 3, indicating that the loading of nitrogen-doped carbon quantum dots in step (2) effectively reduces the recombination probability of photogenerated electron-hole pairs and increases the photogenerated carrier lifetime.

[0103] By comparison, the photogenerated carrier lifetimes of Examples 1 to 3 are greater than that of Comparative Example 4, indicating that the loading of molybdenum disulfide in step (3) greatly reduces the recombination probability of photogenerated electron-hole pairs and increases the photogenerated carrier lifetime.

[0104] By comparison, the photogenerated carrier lifetimes of Examples 1 to 3 are greater than that of Comparative Example 5, indicating that the addition of lauryltrimethylammonium bromide in step (1) reduces the thickness of the prepared sample, shortens the migration path of photogenerated electrons, effectively reduces the recombination probability of photogenerated electron-hole pairs, and increases the photogenerated carrier lifetime.

[0105] Test Example 5

[0106] Photocatalytic degradation performance test: The photocatalytic degradation performance of the prepared highly active defective bismuth vanadate nanosheets was tested by photocatalytic degradation of tetracycline hydrochloride and rhodamine B in water under light irradiation of different wavelengths. The test process is as follows:

[0107] (I) 30 mg of highly active defective bismuth vanadate nanosheets were dispersed in 100 ml of 10 mg / L tetracycline hydrochloride solution, stirred at 400 r / min for 30 min in the dark, and photocatalytic reaction was carried out under light irradiation. A 300 W Xe lamp equipped with a 420 nm cutoff filter and a UVVISCUT filter with a transmission wavelength greater than 760 nm was used as a visible light and near-infrared light source, respectively. After 3 h, the concentration of tetracycline hydrochloride remaining in the test solution was measured and the degradation rate was calculated;

[0108] (II) Prepare a 5 mg / L rhodamine B solution and store it in a dark place. Take 30 mg of highly active defective bismuth vanadate nanosheets and disperse them in 100 ml of rhodamine B solution. Stir at 400 r / min for 5 h in the dark and perform photocatalytic reaction under light irradiation. A 300W Xe lamp equipped with a 420nm cutoff filter and a UVVISCUT filter with a transmission wavelength greater than 760nm is used as a visible light and near-infrared light source, respectively. After 3 h, the remaining rhodamine B concentration in the test solution is measured and the degradation rate is calculated.

[0109] The results are shown in Table 5.

[0110] Table 5

[0111]

[0112] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 5, it can be found that the highly active defective bismuth vanadate nanosheets prepared in the present invention have a very high photocatalytic degradation ability.

[0113] By comparison, the photodegradation rates of tetracycline hydrochloride and rhodamine B in Examples 1 to 3 are greater than those of tetracycline hydrochloride and rhodamine B in Comparative Example 1, indicating that the vanadium vacancies formed by the higher hydrothermal reaction temperature and shorter reaction time in step (1) provide more catalytic active sites, thereby improving the photocatalytic reaction activity.

[0114] By comparison, the photodegradation rates of tetracycline hydrochloride and rhodamine B in Examples 1 to 3 are greater than those of tetracycline hydrochloride and rhodamine B in Comparative Example 2, indicating that the nitrogen doping introduced by the high-temperature annealing under a nitrogen atmosphere in step (1) reduces the band gap, increases the light response range, and improves the photocatalytic reaction activity.

[0115] By comparison, the visible light photodegradation rates of tetracycline hydrochloride and rhodamine B in Examples 1 to 3 are greater than the visible light photodegradation rates of tetracycline hydrochloride and rhodamine B in Comparative Example 3, indicating that the nitrogen-doped carbon quantum dots loaded in step (2) reduce the recombination probability of electron-hole pairs, increase the lifetime of photogenerated carriers, and improve the photocatalytic reaction activity.

[0116] By comparison, the near-infrared light degradation rates of tetracycline hydrochloride and rhodamine B in Examples 1 to 3 are much greater than the near-infrared light degradation rates of tetracycline hydrochloride and rhodamine B in Comparative Example 3, indicating that the upconversion photoluminescence ability of the nitrogen-doped carbon quantum dots loaded in step (2) gives the highly active defective bismuth vanadate nanosheets the ability to absorb and utilize near-infrared light, thereby improving the photocatalytic reaction activity.

[0117] By comparison, the photodegradation rates of tetracycline hydrochloride and rhodamine B in Examples 1 to 3 are greater than those of tetracycline hydrochloride and rhodamine B in Comparative Example 4, indicating that the molybdenum disulfide loaded in step (3) inhibits the recombination of photogenerated electron-hole pairs, increases the lifetime of photogenerated carriers, and improves the photocatalytic reaction activity.

[0118] By comparison, the photodegradation rates of tetracycline hydrochloride and rhodamine B in Examples 1 to 3 are greater than those of tetracycline hydrochloride and rhodamine B in Comparative Example 5, indicating that the lauryltrimethylammonium bromide added in step (1) enables the prepared high-activity defective bismuth vanadate nanosheets to have a lower thickness, shortens the migration distance of photogenerated electrons, reduces the recombination probability of photogenerated electron-hole pairs, increases the lifetime of photogenerated carriers, and increases the photocatalytic reaction activity.

[0119] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A highly active defective bismuth vanadate nanosheet, characterized in that: The high-activity defective bismuth vanadate nanosheets are prepared by firstly carrying out a solvothermal reaction with bismuth trichloride, sodium orthovanadate dodecahydrate and a complexing agent at 160° C. for 3 to 4 hours, and then annealing at high temperature in a nitrogen atmosphere to obtain nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets; preparing nitrogen-doped carbon quantum dot powder from biomass raw materials and lysine by a hydrothermal method; loading nitrogen-doped carbon quantum dots on nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets to obtain nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets; and growing molybdenum disulfide on nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defective bismuth vanadate nanosheets by a hydrothermal method to obtain high-activity defective bismuth vanadate nanosheets; The complexing agent is lauryltrimethylammonium bromide; The solvent used in the solvothermal reaction is ethylene glycol; The temperature of the high temperature annealing is 340-360°C.

2. The highly active defective bismuth vanadate nanosheet according to claim 1, characterized in that: The biomass raw material is one or more of corn stalks, sorghum stalks, rice stalks, peanut shells, coconut shells, and leaves.

3. A method for preparing highly active defective bismuth vanadate nanosheets, characterized in that: The method comprises the following preparation steps: (1) Bismuth trichloride, lauryl trimethylammonium bromide and ethylene glycol were mixed uniformly, stirred at 25-30°C and 600-800 r / min for 40-60 min, then sodium orthovanadate dodecahydrate in an equal molar amount to bismuth trichloride was added, stirred at 25-30°C and 600-800 r / min for 5-10 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 160°C for 3-4 h, naturally cooled to 20-25°C, centrifuged at 8000-10000 r / min for 10-15 min, collected the precipitate, washed with anhydrous ethanol and deionized water for 5-6 times respectively, dried at 5-10 Pa and 50-60°C for 10-12 h, and annealed at 340-360°C in a nitrogen atmosphere at a heating rate of 5°C / min for 2 h to obtain nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets; (2) The nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, nitrogen-doped carbon quantum dot suspension, and deionized water were mixed evenly, stirred and refluxed at 85-95°C and 300-500 r / min for 3-4 hours, cooled naturally to room temperature, and centrifuged at 6000-8000 r / min for 8-12 minutes. The collected precipitate was washed with deionized water for 4-6 times, and vacuum dried at 50-60°C at 5-10 Pa for 6-8 hours to obtain nitrogen-doped carbon quantum dot / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets; (3) The nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, molybdenum precursor, sulfur precursor and deionized water are mixed evenly, stirred and dispersed at 20-30°C and 300-500 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 190-200°C for 24 h, naturally cooled to room temperature, centrifuged at 6000-8000 r / min for 10-15 min, the collected precipitate is washed with deionized water and ethanol for 4-6 times respectively, and vacuum dried at 5-10 Pa and 50-60°C for 6-8 h to obtain molybdenum disulfide / nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanoflakes, that is, high-activity defect state bismuth vanadate nanoflakes.

4. The method for preparing a highly active defective bismuth vanadate nanosheet according to claim 3, characterized in that: The preparation method of the nitrogen-doped carbon quantum dot suspension in step (2) is as follows: (A) The biomass raw material is washed with deionized water, dried at 5-10 Pa and 60-80 ° C for 8-10 h, and a high-speed pulverizer is used to produce a biomass powder with a particle size of less than 2 mm; (B) The biomass powder, lysine and deionized water were mixed uniformly in a mass ratio of 1: (0.25-0.3): (45-55), stirred and dispersed at 20-30°C and 300-500 r / min for 20 min, added into a polytetrafluoroethylene-lined autoclave, reacted at 180-200°C for 12 h, naturally cooled to room temperature, centrifuged at 8000-12000 r / min for 10-15 min, the supernatant was collected, filtered using a 0.22 μm filter membrane, and freeze-dried at -15°C to -10°C to obtain nitrogen-doped carbon quantum dot powder; (C) The nitrogen-doped carbon quantum dot powder was dispersed in deionized water, stirred and dispersed at 20-30°C and 300-500 r / min for 20 min to prepare a 1 mg / ml nitrogen-doped carbon quantum dot suspension.

5. The method for preparing a highly active defective bismuth vanadate nanosheet according to claim 3, characterized in that: In the step (1), the molar ratio of bismuth trichloride, lauryltrimethylammonium bromide and ethylene glycol is 1:(0.4-0.5):(50-60).

6. The method for preparing a highly active defective bismuth vanadate nanosheet according to claim 3, characterized in that: In the step (2), the mass ratio of nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, nitrogen-doped carbon quantum dot suspension, and deionized water is 1:(10-12):(30-40).

7. The method for preparing a highly active defective bismuth vanadate nanosheet according to claim 3, characterized in that: In the step (3), the mass ratio of nitrogen-doped carbon quantum dots / nitrogen-doped vanadium vacancy defect state bismuth vanadate nanosheets, molybdenum precursor, sulfur precursor, and deionized water is 1:(0.03-0.035):(0.3-0.35):(25-35).

8. The method for preparing a highly active defective bismuth vanadate nanosheet according to claim 3, characterized in that: In the step (3), the molybdenum precursor is one of sodium molybdate and hexaammonium heptamolybdate tetrahydrate.

9. The method for preparing a highly active defective bismuth vanadate nanosheet according to claim 3, characterized in that: In the step (3), the sulfur precursor is one of thiourea and thioacetamide.

Citation Information

Patent Citations

  • Bismuth vanadate powder and preparation method thereof

    CN101318700A

  • P-n heterojunction BiVO4-MoS2 composite photocatalyst and preparation method thereof

    CN106311283A

  • Monoclinic scheelite crystal type pucherite nanosheet and preparation method and application thereof

    CN107032399A

  • BiVO4 nanosheet and preparation method and application thereof

    CN113896243A

  • An acid gas removal / capture system and process for converting carbon dioxide to chemical compounds

    WO2022177420A1