End point detection window, chemical mechanical polishing pad and application thereof

By using a specific composition to prepare an endpoint detection window in a chemical mechanical polishing pad, the problem of insufficient accuracy and consistency in polishing endpoint detection is solved, achieving higher polishing accuracy and consistency, and reducing yellowing.

CN118456278BActive Publication Date: 2024-12-03WANHUA CHEM GRP ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410921714.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-12-03
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

Existing chemical mechanical polishing pads suffer from insufficient accuracy and consistency in the detection of polishing endpoints during the polishing process.

Method used

A composition of isocyanate-terminated prepolymer containing unreacted NCO groups, curing agent containing active hydrogen groups, and small molecule isocyanate was used as the endpoint detection window. By controlling the amount of small molecule isocyanate at 3.5-20 wt%, an endpoint detection window with a yellowness index of 1-30 was prepared and used in chemical mechanical polishing pads to improve the accuracy of polishing endpoint detection.

Benefits of technology

It improves the accuracy and consistency of polishing results, reduces yellowing during the polishing process, and enhances the precision of endpoint detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118456278B_ABST
    Figure CN118456278B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of chemical mechanical polishing, and provides an endpoint detection window, a chemical mechanical polishing pad and an application thereof. Chemical mechanical polishing is performed using a chemical mechanical polishing pad with an endpoint detection window provided by the present invention, which can effectively improve the accuracy of polishing endpoint detection and the polishing consistency. The endpoint detection window comprises the reaction product of the following components: component a, an isocyanate-terminated prepolymer containing unreacted NCO groups; component b, a curing agent containing active hydrogen groups; component c, a small molecule isocyanate; wherein the relative molecular mass of the small molecule isocyanate is less than 1000 and is greater than the molecular weight of the isocyanate used to prepare the prepolymer; the amount of the component c accounts for 3.5-20wt% of the total mass of the component a, the component b and the component c.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical mechanical polishing, and in particular to an endpoint detection window, a chemical mechanical polishing pad and applications thereof. Background Art

[0002] In the process of integrated circuit manufacturing, it is usually necessary to eliminate the fine bumps on the surface of the wafer and achieve flatness. Chemical mechanical planarization or chemical mechanical polishing (CMP) is a common technology used to planarize or polish workpieces (such as semiconductor wafers). Generally speaking, the chemical mechanical polishing process is to supply a polishing liquid with a chemical mixture to the polishing pad, and to form a relative movement between the polishing element and the polishing pad. Through the mechanical friction generated by the relative movement and the chemical action of the polishing liquid, part of the surface layer of the element is removed, and the surface is gradually flattened to achieve the purpose of flattening.

[0003] During the polishing process, an endpoint detection system is often used to detect the polishing endpoint to determine when the desired planarization level is achieved. In-situ detection methods use a polishing pad with an endpoint detection window that provides access to the laser during polishing to allow inspection of the wafer surface. In-situ optical endpoint indication techniques can be divided into two basic categories: monitoring a reflected light signal of a single wavelength, such as light from a laser source, or monitoring reflected light signals from multiple wavelengths. When monitoring the light signal, the reflectivity of the substrate changes as the composition at the substrate surface changes from one material to another. This change in reflectivity is then used to detect the CMP polishing endpoint.

[0004] Chinese patent CN105922126B proposes that the prepolymer for preparing the window is composed of three raw materials A, B, and C, wherein raw material A is an isocyanate whose isocyanate group is not directly connected to the benzene ring, raw material B is a polyol with a molecular weight of 500-1500, and raw material C is a difunctional thiol compound. Thus, a chemical mechanical polishing pad with good light transmittance, stable performance, and long service life is prepared.

[0005] The endpoint detection window disclosed in Chinese patent CN104029116B contains cyclic olefin addition polymer to ensure that it has a uniform chemical composition in thickness, and the spectral loss of the endpoint detection window block is less than 40%, so that the polishing pad has good chemical mechanical properties and polishing effect.

[0006] For chemical mechanical polishing pads, how to further improve them so that they can bring better polishing consistency during application is still one of the technical difficulties that urgently needs further breakthroughs in this field. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention provides an endpoint detection window, a chemical mechanical polishing pad and applications thereof. Using the chemical mechanical polishing pad with the endpoint detection window provided by the present invention for chemical mechanical polishing can effectively improve the accuracy of polishing endpoint detection and improve polishing consistency.

[0008] To achieve the purpose, the present invention provides the following technical solutions:

[0009] The present invention provides an endpoint detection window for a chemical mechanical polishing pad, wherein the endpoint detection window comprises a reaction product of the following components:

[0010] Component a, an isocyanate-terminated prepolymer containing unreacted NCO groups;

[0011] Component b, a curing agent containing an active hydrogen group;

[0012] Component c, small molecule isocyanate;

[0013] Wherein, the relative molecular mass of the small molecule isocyanate is less than 1000 and is greater than the molecular weight of the isocyanate used to prepare the prepolymer;

[0014] The amount of the component c is 3.5-20wt% of the total weight of the component a, the component b and the component c.

[0015] Furthermore, in the component a, the isocyanate used to prepare the prepolymer is toluene diisocyanate;

[0016] In the component b, the curing agent is selected from one or more of 4,4'-methylenebis(2-chloroaniline) and 4,4'-methylenebis(3-chloro-2,6-diethylaniline).

[0017] Preferably, the amount of the component c is 7-20 wt % of the total mass of the component a, the component b and the component c.

[0018] Further preferably, the amount of the component c accounts for 9-15wt% of the total mass of the component a, the component b and the component c.

[0019] In some embodiments, the small molecule isocyanate is selected from one or more of dicyclohexylmethane diisocyanate, 4,4-diphenylmethane diisocyanate, and isophorone diisocyanate.

[0020] In some embodiments, the step of preparing the reaction product includes: reacting and curing the component a, the component b and the component c at 70-120° C.;

[0021] And / or, the stoichiometric ratio of the total amount of unreacted NCO groups in the component a and the component c to the active hydrogen groups in the component b is 0.8-1.2.

[0022] Furthermore, the yellowness index YI of the endpoint detection window is 1-30.

[0023] The present invention also provides a chemical mechanical polishing pad with an endpoint detection window, wherein the endpoint detection window adopts the endpoint detection window described above.

[0024] Furthermore, the polishing pad comprises a polishing layer, and the polishing layer is provided with an opening for accommodating the endpoint detection window; and an absolute value of a difference in compression rate between the endpoint detection window and the polishing layer is ≤10%.

[0025] The present invention also provides use of the chemical mechanical polishing pad described above in chemical mechanical polishing.

[0026] The technical solution provided by the present invention has the following beneficial effects:

[0027] The use of a chemical mechanical polishing pad with the endpoint detection window of the present invention is beneficial to improving the accuracy of polishing endpoint detection. The window has good yellowing resistance, can improve the accuracy of polishing results, and ultimately improve the consistency of chemical mechanical polishing. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 FIG. 4 is a schematic cross-sectional view of a polishing pad in one embodiment.

[0029] Explanation of the reference numerals: 1 - chemical mechanical polishing pad, 2 - polishing layer, 3 - adhesive layer, 4 - buffer layer, 5 - endpoint detection window. DETAILED DESCRIPTION

[0030] In order to facilitate the understanding of the present invention, the present invention will be further described below in conjunction with examples. It should be understood that the following examples are only for a better understanding of the present invention and do not mean that the present invention is limited to the following examples.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the invention belongs. The term "and / or" as may be used herein includes any and all combinations of one or more of the related listed items. The top, bottom, etc. mentioned or may be mentioned in this specification are defined relative to the structures shown in the drawings. They are relative concepts and may therefore change accordingly according to their different locations and different usage states.

[0032] In one aspect, the present invention provides an endpoint detection window for a chemical mechanical polishing pad, wherein the endpoint detection window comprises a reaction product of the following components:

[0033] Component a, an isocyanate-terminated prepolymer containing unreacted NCO groups;

[0034] Component b, a curing agent containing an active hydrogen group;

[0035] Component c, small molecule isocyanate;

[0036] Wherein, the relative molecular mass of the small molecule isocyanate is less than 1000 and is greater than the molecular weight of the isocyanate used to prepare the prepolymer;

[0037] The amount of the component c is 3.5-20wt% of the total mass of the component a, the component b and the component c, for example, 3.5wt%, 7wt%, 10wt%, 15wt%, 18wt%, 20wt% and the like.

[0038] The endpoint detection window of the present invention is based on an isocyanate-terminated prepolymer containing unreacted NCO groups and a curing agent containing a hydrogen-spraying group, and the above-mentioned component C with a relative molecular mass less than 1000 and greater than the molecular weight of the isocyanate used to prepare the prepolymer is added for reaction and curing. The endpoint detection window is used in a chemical mechanical polishing pad, which can improve the accuracy of endpoint detection and further improve the polishing uniformity. In the preparation of the endpoint detection window of the present invention, the small molecule isocyanate used is a product that is easily available on the market. In the process of preparing the window, there is no need to adjust too many process parameters, and it can be easily adapted to the existing preparation process.

[0039] Further, in the component a, the isocyanate used to prepare the prepolymer is toluene diisocyanate (TDI); in the component b, the curing agent is selected from one or more of 4,4'-methylenebis(2-chloroaniline), 4,4'-methylenebis(3-chloro-2,6-diethylaniline). The inventors have found that the endpoint detection window system based on the prepolymer of TDI and the curing agent based on 4,4'-methylenebis(2-chloroaniline) and / or 4,4'-methylenebis(3-chloro-2,6-diethylaniline) can obtain an endpoint detection window with a yellowness index YI of 1-30 and good yellowing resistance by adding a small molecule isocyanate with a relative molecular mass less than 1000 and a molecular weight greater than that of TDI during the preparation of the endpoint detection window, and controlling the amount thereof to 3.5-20wt% of the total mass of the components a, b and c. Moreover, the endpoint detection window is applied in a chemical mechanical polishing pad to improve the accuracy of the polishing result and the consistency of the polishing.

[0040] In a preferred embodiment, the amount of component c is 7-20wt% of the total mass of component a, component b and component c. With the preferred amount of component c, the prepared endpoint detection window is used in a chemical mechanical polishing pad, has better yellowing resistance, and is conducive to further improving the consistency of polishing.

[0041] More preferably, the amount of component c is 9-15wt% of the total weight of component a, component b and component c. With the preferred amount of component c, the prepared endpoint detection window has better polishing consistency when used in a chemical mechanical polishing pad.

[0042] The above-mentioned toluene diisocyanate (TDI)-based prepolymer (component a) can directly adopt commercially available products, such as but not limited to Adiprene® prepolymer L325, LF750D, LF751D, LF600D, LF700D, LF950A, LFG963A, LF1950A, etc.

[0043] In some embodiments, the small molecule isocyanate is selected from one or more of dicyclohexylmethane diisocyanate, 4,4-diphenylmethane diisocyanate, and isophorone diisocyanate.

[0044] In some embodiments, the step of preparing the reaction product includes: reacting and curing the component a, the component b and the component c at 70-120°C (e.g., 70, 80, 90, 100, 110, 120°C, etc.), for example, curing for 12-48 hours. In some specific examples, the component a and the component c are first mixed, and then the component b is added and stirred evenly, and the combined liquid is poured into a 70-120°C mold, and then placed in a 70-120°C oven for curing for 12-48 hours, and the window block is obtained after demolding.

[0045] In some embodiments, the stoichiometric ratio of the total amount of unreacted NCO groups in the component a and the component c to the active hydrogen groups in the component b is 0.8-1.2, such as 0.8, 0.9, 1.0, 1.1, 1.2, etc., preferably 0.9-1.1.

[0046] The present invention also provides a chemical mechanical polishing pad with an endpoint detection window, wherein the endpoint detection window is the endpoint detection window described above. In the polishing pad, the number of the endpoint detection windows may be one or more.

[0047] In the present invention, the polishing pad may have a common structure of a polishing pad known in the art. For example, see Figure 1, the chemical mechanical polishing pad 1 includes a polishing layer 2, the polishing layer 2 is provided with an opening for accommodating the endpoint detection window; further includes a buffer layer 4 and an adhesive layer 3, etc. For example, the polishing layer 2 has a top surface and a bottom surface, the polishing layer 2 is provided with an opening extending from the top surface to the bottom surface, and the endpoint detection window 5 is provided at the opening of the polishing layer 2; the buffer layer 4 is attached to the bottom surface of the polishing layer 2 through the adhesive layer 3, and the opening is not covered or not completely covered by the adhesive layer 3 and the buffer layer 4. That is, the endpoint detection window is at least partially exposed relative to the adhesive layer and the buffer layer, and at least not completely covered by the two. There is no particular restriction on the specific structure of the polishing pad.

[0048] Furthermore, the absolute value of the difference between the compression rate of the endpoint detection window and the polishing layer is ≤10%, such as ≤5%, such as ≤2%, such as ≤1.5%, etc. The difference between the compression rate of the endpoint detection window and the polishing layer is within a preferred range, which is conducive to further improving the polishing effect.

[0049] In the present invention, there is no particular requirement for the specific installation method of the endpoint detection window. For example, it can be an insertion-type window, for example, installed on the polishing layer by insertion; or it can be an integrated window, for example, formed integrally with the polishing layer. The installation methods of the endpoint detection window of the insertion-type window and the integrated window are well known to those skilled in the art.

[0050] Further, the top surface of the polishing layer may be provided with grooves; polishing liquid and polishing debris, etc. may be conducted through the grooves. The number of grooves is not particularly limited, for example, a plurality of grooves may be provided. Preferably, the groove design is selected from a combination of one or more of the following: concentric grooves (which may be circular or spiral), curved grooves, cross-hatched grooves (for example, arranged as an XY grid on the surface of the polishing layer, such as a grid-shaped groove pattern), other regular designs (for example, hexagonal, triangular, etc.), tire surface patterns, irregular designs, and combinations thereof. More preferably, the groove design is selected from one or more of the following: concentric grooves (spiral grooves), cross-hatched grooves (XY grid grooves), other regular designs (hexagonal grooves, triangular grooves, etc.).

[0051] The material of the polishing layer is not particularly limited, for example, the material of the polishing layer may include one or more of segmented block copolymers and polyurethane elastomers. The segmented block copolymer is, for example, a segmented block copolymer including at least one hard segment and at least one soft segment, for example, including a variety of compositions of polyethylene oxide, poly(ether ester) block copolymers, polyamides, polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl pyridine, polyacrylic acid, polymethacrylic acid, polyaspartic acid, styrene polymers, epoxy polymers, maleic anhydride methyl vinyl ether copolymers, etc. The polyurethane elastomer may be, for example, selected from a combination of one or more of polyurethane elastomers, polyether elastomers, polyether polyester elastomers, polyamide-based elastomers, thermoplastic polyurethanes, thermoplastic rubbers, styrene-butadiene copolymers, silicone rubbers, synthetic rubbers, styrene-isoprene copolymers, styrene-ethylene-butylene copolymers, etc.

[0052] The material of the buffer layer is not particularly limited. For example, the buffer layer includes one or more of a textile material and a non-woven material, such as a felt material, a spunbond material and / or a needle-punched material. The material of the buffer layer may include, for example, one or more of a polymer-impregnated felt material (such as a polyurethane-impregnated felt material) and a textile material (such as a thick flannel material). The buffer layer material may also be selected from a polyurethane foam material.

[0053] There is no particular restriction on the specific selection of the adhesive layer, for example, the adhesive layer is selected from one or more of a pressure-sensitive adhesive and a reactive hot melt adhesive. Preferably, the reactive hot melt adhesive is selected from at least one of polyolefin, ethylene vinyl acetate, polyamide, polyester, polyurethane, polyvinyl chloride or epoxy resin; the pressure-sensitive adhesive is selected from at least one of an acrylic adhesive (PSAV) or a rubber-based adhesive (PSA8). The main function of the adhesive layer is to tightly bond the polishing layer and the buffer layer together.

[0054] The present invention also provides the use of the chemical mechanical polishing pad described above in chemical mechanical polishing, for example, pressing the element to be polished onto the polishing pad described above for chemical mechanical polishing. The element to be polished is, for example, a graphic sheet, a film-coated sheet, a copper sheet, etc. During the polishing process, relative motion is provided between the element to be polished and the polishing pad for polishing. The specific operation, polishing equipment, polishing process, etc. of chemical mechanical polishing of the element to be polished can refer to the prior art in the art, and the key lies in using the chemical mechanical polishing pad with an endpoint detection window provided by the present invention.

[0055] Furthermore, the yellowness index YI of the endpoint detection window prepared by the present invention is 1-30, preferably 5-20, and more preferably 10-20. The endpoint detection window formulation system of the present invention is used, especially for the TDI-based prepolymer, the 4,4'-methylenebis(2-chloroaniline) and / or 4,4'-methylenebis(3-chloro-2,6-diethylaniline)-based formulation system to prepare the endpoint detection window. The endpoint detection window with a yellowness index YI of 1-30 can be obtained by using the formulation system of the present invention. The provided endpoint detection window is not prone to significant yellowing during the polishing process, has little effect on the penetration and receiving accuracy of the front and rear laser beams during the polishing process, and is conducive to improving the accuracy of endpoint detection during the entire polishing process.

[0056] During the chemical mechanical polishing process of the component to be polished (wafer), the in-situ detection method in the endpoint detection system is often used to determine the polishing endpoint. The endpoint detection window serves as an entrance during polishing, allowing the laser to pass through and inspect the wafer surface. After long-term laser irradiation, the endpoint detection window is prone to yellowing, affecting the accuracy of the polishing result and the polishing flatness. The inventors have found through extensive research that the endpoint detection window provided by the present invention has good yellowing resistance and can be used in chemical mechanical polishing to improve the accuracy of endpoint detection and improve polishing uniformity.

[0057] The present invention is further described below by means of specific examples, but it should not be understood that the present invention is limited thereto.

[0058] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0059] The main raw materials used in the examples and comparative examples of the present invention are as follows:

[0060] Polishing equipment and polishing conditions: The polishing experiment was conducted on an Applied Reflexion polisher (Applied Materials) using a 300 mm wafer (Oxide film wafer), with a carrier (corresponding to the polishing head of the polisher) down pressure of 0.024 MPa and a polishing liquid (JEEZ oxide layer polishing liquid) slurry flow rate of 300 mL / min. The table rotation speed was 93 rpm, and the carrier rotation speed was 87 rpm.

[0061] Uniformity test method: Before and after each polishing experiment, a four-point probe (Four Dimensions, Inc, 333Å) tester was used to measure the thickness of 81 test points at the same position on the wafer, and the removal rate was calculated by the thickness difference. The removal rate calculation formula is as follows: .in, is the average thickness of 81 test points before polishing, is the average thickness of 81 test points after polishing. It is the average value of the thickness difference before and after polishing of each of the 81 test points. The non-uniformity ratio (%NUR) is calculated by calculating the standard deviation of the removal rate. The smaller the non-uniformity ratio, that is, the smaller the standard deviation of the removal rate, the closer the polishing rate on the entire polishing surface is and the more uniform the polishing effect is.

[0062] Compression rate test method: Take a sample block, place it on the thickness gauge, measure the initial thickness T1 without load, place a 50KPa weight, and read the thickness T2 after 60s of load. Compression rate = (T1-T2) / T1x100%.

[0063] Yellowness index test: The yellowness index test was performed using Ultra Scan VIS 1839 instrument according to GB 2409-80 standard.

[0064] Some of the raw materials used in the examples and comparative examples are described as follows:

[0065] Isocyanate-terminated prepolymer containing unreacted NCO groups: Adiprene® prepolymer LF750D produced by Chemtura has an unreacted NCO group content of 8.95wt% and is a TDI-type prepolymer.

[0066] Isocyanate-terminated prepolymers containing unreacted NCO groups: Adiprene® prepolymer LF751D produced by Chemtura has an unreacted NCO group content of 9.02 wt % and is a TDI-based prepolymer.

[0067] Curing agent: MOCA, 4,4'-methylenebis(2-chloroaniline), Jinan Lunan Chemical.

[0068] HMDI: dicyclohexylmethane diisocyanate, Wanhua Chemical;

[0069] MDI: 4,4-diphenylmethane diisocyanate, Wanhua Chemical;

[0070] IPDI: isophorone diisocyanate, Wanhua Chemical;

[0071] HDI: Hexamethylene diisocyanate, Wanhua Chemical.

[0072] Example 1

[0073] 20.5 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) was mixed with 2.5 kg of HMDI. After uniform mixing, 7.2 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into an 80°C mold, and placed in an 80°C oven. After high-temperature curing in the oven for 20 hours, the mold was removed to obtain a window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and HMDI to the active hydrogen groups in the curing agent was 1.00.

[0074] A polishing pad with an endpoint detection window is prepared by an integrated molding method. The preparation method of the polishing layer is as follows:

[0075] 50.7kg of Adiprene® prepolymer LF750D produced by Chemtura was mixed with 1.3kg of expanded microspheres 40D42 produced by Nouryon. After mixing evenly, 10.5kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture and poured into an 80°C mold. The window block was placed in advance at a fixed position in the mold. The whole was placed in an 80°C oven, cured at high temperature in the oven for 22 hours, and then demolded and taken out to obtain a polishing layer block, which was sliced ​​by a slicer to obtain a polishing layer with an endpoint detection window.

[0076] The buffer layer uses the commercially available SUBA IV product of DOW, and the adhesive layer uses Tesa PSA. The buffer layer is pressed onto the bottom surface of the polishing layer through the adhesive layer by rolling to form a laminated structure to obtain a polishing pad. See the schematic diagram for details. Figure 1 .

[0077] Example 2

[0078] 15.1 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) was mixed with 5 kg of MDI. After uniform mixing, 9.3 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into an 85°C mold, and placed in an 85°C oven. After high-temperature curing in the oven for 18 hours, the mold was removed to obtain a window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and MDI to the active hydrogen groups in the curing agent was 0.94.

[0079] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0080] Example 3

[0081] 27.5 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) was mixed with 5.5 kg of IPDI. After uniform mixing, 11 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into a 90°C mold, and placed in a 90°C oven. After high-temperature curing in the oven for 30 hours, the window block was removed from the mold to obtain the window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and IPDI to the active hydrogen groups in the curing agent was 1.16.

[0082] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0083] Example 4

[0084] 15 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF751D produced by Chemtura, NCO 9.02%) was mixed with 5 kg of IPDI. After uniform mixing, 9 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into a 115°C mold, and placed in a 115°C oven. After high-temperature curing in the oven for 29 hours, the mold was removed to obtain a window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and IPDI to the active hydrogen groups in the curing agent was 1.14.

[0085] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0086] Example 5

[0087] 30.5 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF751D produced by Chemtura, NCO 9.02%) was mixed with 1.5 kg of IPDI. After uniform mixing, 10.5 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into a 115°C mold, and placed in a 115°C oven. After high-temperature curing in the oven for 29 hours, the mold was removed to obtain a window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and IPDI to the active hydrogen groups in the curing agent was 1.00.

[0088] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0089] Example 6 (Compared with Example 2)

[0090] 15.1 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) was mixed with 4 kg of MDI. After uniform mixing, 9.3 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into an 85°C mold, and placed in an 85°C oven. After high-temperature curing in the oven for 18 hours, the mold was removed to obtain a window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and MDI to the active hydrogen groups in the curing agent was 0.83.

[0091] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0092] Example 7 (Compared with Example 2)

[0093] 21 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) was mixed with 3 kg of MDI. After uniform mixing, 7 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into an 85°C mold, and placed in an 85°C oven. After high-temperature curing in the oven for 18 hours, the mold was removed to obtain a window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and MDI to the active hydrogen groups in the curing agent was 1.14.

[0094] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0095] Example 8 (Compared with Example 2)

[0096] 23 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) was mixed with 3 kg of MDI. After uniform mixing, 7 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into an 85°C mold, and placed in an 85°C oven. After high-temperature curing in the oven for 18 hours, the mold was removed to obtain a window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and MDI to the active hydrogen groups in the curing agent was 1.19.

[0097] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0098] Comparative Example 1 (Compared with Example 1, no small molecule isocyanate was added)

[0099] 20.5 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) and 4.2 kg of curing agent (MOCA, Jinan Lunan Chemical) were mixed evenly, poured into an 80°C mold, and placed in an 80°C oven. After high-temperature curing in the oven for 20 hours, the window block was demoulded and taken out to obtain the window block. In the raw materials used in this comparative example, the stoichiometric ratio of the unreacted NCO groups of the prepolymer to the active hydrogen groups in the curing agent was 1.10.

[0100] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0101] Comparative Example 2 (Compared with Example 1, the amount of small molecule isocyanate used is too high)

[0102] 11.5 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) was mixed with 7.5 kg of HMDI. After uniform mixing, 10.2 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into an 80°C mold, and placed in an 80°C oven. After high-temperature curing in the oven for 20 hours, the mold was removed to obtain a window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and HMDI to the active hydrogen groups in the curing agent was 1.17.

[0103] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0104] Comparative Example 3 (the molecular weight of the added small molecule isocyanate is smaller than that of TDI)

[0105] 20.5 kg of isocyanate-terminated prepolymer containing unreacted NCO groups (Adiprene® prepolymer LF750D produced by Chemtura, NCO 8.95%) was mixed with 2.3 kg of HDI. After uniform mixing, 7.2 kg of curing agent (MOCA, Jinan Lunan Chemical) was added to the mixture, poured into an 80°C mold, and placed in an 80°C oven. After high-temperature curing in the oven for 20 hours, the window block was removed from the mold to obtain the window block. In the raw materials used in this embodiment, the stoichiometric ratio of the total amount of unreacted NCO groups of the prepolymer and HDI to the active hydrogen groups in the curing agent was 1.15.

[0106] Referring to Example 1, a polishing layer with an endpoint detection window was prepared by an integrated molding method. Referring to Example 1, a buffer layer, an adhesive layer and a polishing layer were rolled to form a laminated structure to obtain a polishing pad.

[0107] The endpoint detection windows prepared in the embodiments and comparative examples were subjected to yellowness index test and non-uniformity ratio test, and the results are shown in Table 1. In each embodiment and comparative example, the difference between the compression rate of the endpoint detection window of the polishing pad and the polishing layer is less than 5%, as shown in Table 1.

[0108] Table 1 is the yellowness index test results of the endpoint detection window of the embodiment and the comparative example

[0109]

[0110] It can be seen from the test data that the endpoint detection window prepared in the embodiment has better polishing consistency and uniformity and a lower non-uniform ratio when used in chemical mechanical polishing compared with the comparative example.

[0111] In comparative example 1, no small molecule isocyanate was added when preparing the endpoint detection window, and the non-uniform ratio increased significantly during chemical mechanical polishing. The amount of small molecule isocyanate used in comparative example 2 did not meet the dosage requirements of the present invention, and the non-uniform ratio also increased significantly. The molecular weight of the small molecule isocyanate added in comparative example 3 did not meet the requirement of being greater than the molecular weight of the isocyanate used in the prepolymer, and as a result, the non-uniform ratio also increased significantly.

[0112] Compared with Examples 1-4 and 6-8, Example 5 is different mainly in that the amount of small molecule isocyanate used is not within the preferred range of 7-20 wt %, and the resulting non-uniform ratio of the endpoint detection window is inferior to that of Example 4.

[0113] Compared with Example 2, Examples 6-8 use a more preferred amount of 9-15 wt % of small molecule isocyanate, and the resulting non-uniform ratio of the endpoint detection window is significantly better than that of Example 2.

[0114] It is easy to understand that the above embodiments are only examples for clear explanation and do not mean that the present invention is limited thereto. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the present invention.

Claims

1. An endpoint detection window for a chemical mechanical polishing pad, characterized in that: The endpoint detection window includes the reaction product of the following components: Component a, an isocyanate-terminated prepolymer containing unreacted NCO groups; Component b, a curing agent containing an active hydrogen group; Component c, small molecule isocyanate; Wherein, the relative molecular mass of the small molecule isocyanate is less than 1000 and is greater than the molecular weight of the isocyanate used to prepare the prepolymer; The amount of the component c is 3.5-20wt% of the total weight of the component a, the component b and the component c.

2. The endpoint detection window of the chemical mechanical polishing pad according to claim 1, characterized in that: In the component a, the isocyanate used to prepare the prepolymer is toluene diisocyanate; In the component b, the curing agent is selected from one or more of 4,4'-methylenebis(2-chloroaniline) and 4,4'-methylenebis(3-chloro-2,6-diethylaniline).

3. The endpoint detection window of the chemical mechanical polishing pad according to claim 2, characterized in that: The amount of the component c is 7-20wt% of the total weight of the component a, the component b and the component c.

4. The endpoint detection window of the chemical mechanical polishing pad according to claim 3, characterized in that: The amount of the component c is 9-15wt% of the total weight of the component a, the component b and the component c.

5. The endpoint detection window of the chemical mechanical polishing pad according to any one of claims 2 to 4, characterized in that: The small molecule isocyanate is selected from one or more of dicyclohexylmethane diisocyanate, 4,4-diphenylmethane diisocyanate and isophorone diisocyanate.

6. The endpoint detection window of the chemical mechanical polishing pad according to any one of claims 1 to 4, characterized in that: The preparation step of the reaction product comprises: reacting and curing the component a, the component b and the component c at 70-120° C.

7. The endpoint detection window of the chemical mechanical polishing pad according to any one of claims 1 to 4, characterized in that: The yellowness index YI of the endpoint detection window is 1-30.

8. A chemical mechanical polishing pad having an endpoint detection window according to any one of claims 1 to 7.

9. The chemical mechanical polishing pad according to claim 8, characterized in that: The polishing pad comprises a polishing layer, and the polishing layer is provided with an opening for accommodating the endpoint detection window; an absolute value of a difference between the compression rates of the endpoint detection window and the polishing layer is ≤10%.

10. Use of the chemical mechanical polishing pad according to claim 8 or 9 in chemical mechanical polishing.