Preparation method of orthopedic silicon nitride ceramics

By introducing specific sintering aids and a second reinforcing phase into silicon nitride ceramics, orthopedic silicon nitride ceramics with improved fracture toughness were prepared, solving the problems of insufficient implant toughness and poor osseointegration performance, and achieving an improvement in the strength and toughness of the material.

CN118459229BActive Publication Date: 2026-11-17XIAN DANHUAGUI TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410555210.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2026-11-17
Estimated Expiration
2044-05-07

AI Technical Summary

Technical Problem

Existing orthopedic silicon nitride implants lack sufficient toughness and have poor osseointegration performance.

Method used

Orthopedic silicon nitride ceramics are prepared by introducing one or more of the following sintering aids: Y2O3, MgO, Al2O3, Yb2O3, Nd2O3, Eu2O3, La2O3, Sm2O3, and CeO, as well as the second reinforcing phases: TiC particles, SiC whiskers, and graphene, through photocuring, low-temperature debinding, and high-temperature sintering.

Benefits of technology

It significantly improves the fracture toughness of silicon nitride ceramics, forming a long columnar β-Si3N4 structure, which enhances the strength and toughness of the material, hinders crack propagation, and improves the bending resistance and toughness of the implant.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004825816140000221
    Figure BDA0004825816140000221
  • Figure BDA0004825816140000231
    Figure BDA0004825816140000231
Patent Text Reader

Abstract

This invention discloses a method for preparing orthopedic silicon nitride ceramics. The raw materials include silicon nitride, a sintering aid, and a second reinforcing phase. The method specifically includes: mixing the sintering aid and the second reinforcing phase with silicon nitride to obtain a mixed powder; mixing the mixed powder with resin to obtain a ceramic slurry; and subjecting the ceramic slurry to photocuring, low-temperature debinding, and high-temperature sintering to obtain orthopedic silicon nitride ceramics. This method creatively introduces one or more sintering aids and a second reinforcing phase selected from Y₂O₃, MgO, Al₂O₃, Yb₂O₃, Nd₂O₃, Eu₂O₃, La₂O₃, Sm₂O₃, and CeO into silicon nitride. Through a preparation process including photocuring, low-temperature debinding, and high-temperature sintering, a reinforcement body with three-dimensional strengthening at points, lines, and surfaces is formed, promoting a complete phase transformation of silicon nitride grains to generate long columnar β-Si₃N₄, resulting in silicon nitride ceramics with significantly improved fracture toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biomaterials technology, specifically relating to a method for preparing orthopedic silicon nitride ceramics. Background Technology

[0002] Silicon nitride ceramics possess excellent strength, corrosion resistance, wear resistance, and high-temperature resistance, and have long been widely studied and applied. Recent research has found that silicon nitride exhibits outstanding bone growth promotion capabilities, good antibacterial properties, and superior imaging quality. Furthermore, porous silicon nitride ceramics possess porosity similar to human bone tissue and are non-cytotoxic, meeting the requirements of orthopedic biology and making them an excellent bone replacement material.

[0003] α-Si3N4 is a low-temperature stable crystal form and is the main phase of Si3N4 raw material powder. β-Si3N4 is a high-temperature stable crystal form, formed by a phase transformation of α-Si3N4 at high temperatures. Adding sintering aids can promote the development and growth of the β phase, forming a self-reinforcing and toughened microstructure. Currently, medical silicon nitride materials used for hard tissue replacement therapy suffer from drawbacks such as excessively high elastic modulus and a need for further improvement in toughness. Summary of the Invention

[0004] The technical problem to be solved by this invention is to address the shortcomings of the prior art by providing a method for preparing orthopedic silicon nitride ceramics. This method creatively introduces one or more sintering aids selected from Y₂O₃, MgO, Al₂O₃, Yb₂O₃, Nd₂O₃, Eu₂O₃, La₂O₃, Sm₂O₃, and CeO, along with a second reinforcing phase comprising TiC particles, SiC whiskers, and graphene, into silicon nitride, resulting in a fracture toughness of 20.7 MPa·m. 1 / 2 The mechanical properties of silicon nitride ceramics are significantly improved.

[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for preparing orthopedic silicon nitride ceramics, characterized in that the raw materials include silicon nitride and sintering aids, and the method specifically includes:

[0006] The sintering aid was mixed with silicon nitride to obtain a mixed powder;

[0007] The mixed powder is mixed with resin to obtain a ceramic slurry;

[0008] The ceramic slurry was subjected to photocuring, low-temperature degreasing, and high-temperature sintering to obtain orthopedic silicon nitride ceramics.

[0009] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the sintering aid is one or more of Y2O3, MgO, Al2O3, Yb2O3, Nd2O3, Eu2O3, La2O3, Sm2O3 and CeO.

[0010] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the mass of the sintering aid is 0.01 to 20% of the mass of silicon nitride.

[0011] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the silicon nitride particle size is 0.2-10 μm; the sintering aid particle size is 1-8 μm; and the resin is a resin with an absorption wavelength of 405 nm.

[0012] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the solid content of the ceramic slurry is 75wt% to 86wt%.

[0013] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the low-temperature degreasing temperature is 1050-1200℃ and the time is 0.5-2h; the high-temperature sintering temperature is 1700-1900℃ and the time is 0.5-2h.

[0014] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the method for obtaining the ceramic slurry includes ball milling for a time of 2 to 10 hours.

[0015] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the raw materials further include a second reinforcing phase, wherein the second reinforcing phase is TiC particles, SiC whiskers or graphene, and the mass of the second reinforcing phase is 0.01 to 10% of the mass of silicon nitride; the method includes mixing a sintering aid and the second reinforcing phase with silicon nitride to obtain a mixed powder.

[0016] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the TiC particle size is 2-10 μm; the SiC whisker aspect ratio is 30-100; and the graphene size is 20-80 μm.

[0017] The above-mentioned method for preparing orthopedic silicon nitride ceramics is characterized in that the second reinforcing phase is TiC particles, SiC whiskers and graphene, and the mass of the second reinforcing phase is 0.01 to 10% of the mass of silicon nitride.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] 1. This invention provides a method for preparing orthopedic silicon nitride ceramics. By creatively introducing one or more sintering aids selected from Y2O3, MgO, Al2O3, Yb2O3, Nd2O3, Eu2O3, La2O3, Sm2O3 and CeO into silicon nitride, the silicon nitride grains undergo a complete phase transformation to generate long columnar β-Si3N4, thereby obtaining silicon nitride ceramics with significantly improved fracture toughness.

[0020] 2. Preferably, the method of the present invention further includes introducing a second reinforcing phase comprising TiC particles, SiC whiskers, and graphene into the raw materials, thereby promoting a complete phase transformation of the silicon nitride grains to generate long columnar β-Si3N4, resulting in silicon nitride ceramics with a fracture toughness of up to 20.7 MPa·m. 1 / 2 .

[0021] 3. Preferably, in the method of the present invention, a sintering aid comprising one or more of Y2O3, MgO, Al2O3, Yb2O3, Nd2O3, Eu2O3, La2O3, Sm2O3 and CeO, and a second reinforcing phase comprising TiC particles, SiC whiskers and graphene, are formed through a preparation process comprising photocuring, low-temperature debinding and high-temperature sintering, thereby forming a reinforcement that is strengthened in three dimensions of points, lines and surfaces, which greatly hinders crack propagation.

[0022] The technical solution of the present invention will be further described in detail below with reference to the embodiments. Detailed Implementation

[0023] This invention provides a method for preparing orthopedic silicon nitride ceramics. The raw materials include silicon nitride powder mixed with a sintering aid, wherein the sintering aid is one or more of Y₂O₃, MgO, Al₂O₃, Yb₂O₃, Nd₂O₃, Eu₂O₃, La₂O₃, Sm₂O₃, and CeO. During high-temperature sintering, the sintering aid forms a silicate liquid phase with the oxygen-rich layer (SiO₂) on the surface of the Si₃N₄ powder. Through particle rearrangement, dissolution, and reprecipitation, as well as grain growth, a dense body is formed. α-Si₃N₄ is completely transformed into fine-grained, long columnar interwoven β-Si₃N₄. The unique microstructure of the long columnar interwoven grains produces an in-situ toughening effect, endowing the modified silicon nitride with higher flexural strength and fracture toughness. Compared to traditional ceramic fracture mechanisms, the fiber-interlocked Si₃N₄ ceramics achieve higher fracture toughness through mechanisms such as crack deflection, crack bridging, and grain debonding and pull-out.

[0024] Preferably, the method of the present invention further includes introducing a second reinforcing phase into the raw material, which can further improve the fracture toughness of the material. The second reinforcing phase is TiC particles, SiC whiskers, or graphene.

[0025] Preferably, the second reinforcing phase comprises TiC particles, SiC whiskers, and graphene. The TiC particles are a hard phase that strengthens the matrix material, improves load-bearing capacity, prevents crack propagation, or deflects cracks. A tortuous crack path consumes more fracture energy, thus improving the material's strength and toughness. The SiC whiskers not only enhance the interlocking effect of the matrix β-Si3N4 grains and refine the grains, but also hinder crack propagation. This helps the whiskers at the crack location to offset more external stress, reducing the stress field intensity factor at the crack, alleviating stress concentration around the crack, and slowing crack propagation, thereby further improving the material's bending resistance and toughness. The interface between graphene and silicon nitride is relatively weak. When a crack propagates to the interface, it will extend along the interface instead of continuing along the original path. Furthermore, graphene has a layered structure with weak interlayer bonding. When a crack propagates to the graphene surface, it can cause interlayer separation, increasing the crack's extension path and thus achieving a toughening effect.

[0026] The three substances enhance the fracture toughness of silicon nitride through different pathways. When used together, TiC particles act as pinning agents, causing cracks to bypass the particles and reach the silicon nitride grains. SiC whiskers are distributed between or through the matrix grains, and cracks extend axially or radially along the SiC whiskers. During the extension process, when encountering graphene sheets, the cracks extend along the graphene surface or between layers. Compared to a single reinforcing phase, the combined reinforcement achieves strengthening in three dimensions: point, line, and surface. The combined effect on the crack extension process increases the resistance of the second phase, making the extension more difficult, and the strength and toughness of silicon nitride ceramics are significantly improved.

[0027] Furthermore, the three reinforcements are used together, along with sintering aids, to ensure that the silicon nitride implant does not fail instantly when subjected to load.

[0028] The following description, in conjunction with specific embodiments, illustrates the content of the present invention. However, the following description is not intended to limit the scope of the present invention.

[0029] A series of orthopedic silicon nitride ceramics were prepared according to the method of the present invention, as detailed below.

[0030] Example 1

[0031] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0032] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 200 nm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 7% of the mass of the silicon nitride powder, the sintering aid is 4 wt.% Y2O3 + 3 wt.% CeO, and the particle size of the sintering aid is 3-5 μm;

[0033] Step 2: Mix the mixed powder with a resin with an absorption wavelength of 405nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 75wt%; the solid content is the mass of the mixed powder / (mass of the mixed powder + mass of the resin).

[0034] Step 3: Use DLP 3D printing equipment to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; the parameters in the photopolymerization printing can be adjusted according to common knowledge in the field. For example, in this embodiment, the power is 2W, the exposure time is 10s, and the model placement angle is 45°.

[0035] Step 4: Place the ceramic green body in a low-temperature furnace at 1050℃ for 1 hour to degrease it, and then sinter it in a nitrogen atmosphere furnace at 1750℃ for 1 hour to obtain orthopedic silicon nitride ceramic.

[0036] Example 2

[0037] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0038] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 5 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 20% of the mass of the silicon nitride powder, the sintering aid is 10 wt.% Y2O3 + 5 wt.% Al2O3 + 5 wt.% MgO, and the particle size of the sintering aid is 1-3 μm;

[0039] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2.5 h to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 78 wt%.

[0040] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.05w, the exposure time is 12s, and the model placement angle is 45°;

[0041] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0042] Example 3

[0043] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0044] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 3 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 15% of the mass of the silicon nitride powder, the sintering aid is 7 wt.% Y2O3 + 4 wt.% Al2O3 + 4 wt.% Yb2O3, and the particle size of the sintering aid is 3-5 μm;

[0045] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 75 wt%.

[0046] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2W, the exposure time is 10s, and the model placement angle is 45°;

[0047] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 2 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0048] Example 4

[0049] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0050] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 12% of the mass of the silicon nitride powder, the sintering aid is 5 wt.% Al2O3 + 4 wt.% Nd2O3 + 3 wt.% Yb2O3, and the particle size of the sintering aid is 6-8 μm;

[0051] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 4 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 76 wt%.

[0052] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.05w, the exposure time is 12s, and the model placement angle is 45°;

[0053] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0054] Example 5

[0055] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0056] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 200 nm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 0.01% of the mass of the silicon nitride powder, the sintering aid is 0.005 wt.% Eu2O3 + 0.005 wt.% La2O3, and the particle size of the sintering aid is 3-5 μm;

[0057] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 78 wt%.

[0058] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.1W, the exposure time is 10s, and the model placement angle is 45°;

[0059] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 0.5h to degrease, and then sinter it in a nitrogen atmosphere furnace at 1700℃ for 2h to obtain orthopedic silicon nitride ceramic.

[0060] Example 6

[0061] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0062] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 5 μm, and ball mill for 2 hours to ensure uniform mixing, obtaining a mixed powder; the mass of the sintering aid is 1% of the mass of the silicon nitride powder, and the sintering aid is...

[0063] 0.4 wt.% Eu2O3 + 0.2 wt.% La2O3 + 0.2 wt.% Sm2O3 + 0.2 wt.% CeO, wherein the particle size of the sintering aid is 1-3 μm;

[0064] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 10 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 76 wt%.

[0065] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.0W, the exposure time is 10s, and the model placement angle is 45°;

[0066] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1900℃ for 0.5 hours to obtain orthopedic silicon nitride ceramic.

[0067] Example 7

[0068] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0069] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 3 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 10% of the mass of the silicon nitride powder, and the sintering aid is composed of 2wt.% Y2O3 + 2wt.% MgO + 2wt.% Al2O3 + 2wt.% Yb2O3 + 1wt.% Nd2O3 + 1wt.% CeO, and the particle size of the sintering aid is 3-5 μm;

[0070] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 5 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 80 wt%.

[0071] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.2W, the exposure time is 15s, and the model placement angle is 45°;

[0072] Step 4: Place the ceramic green body in a low-temperature furnace at 1050℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 1 hour to obtain orthopedic silicon nitride ceramic.

[0073] Example 8

[0074] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0075] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 0.01% of the mass of the silicon nitride powder, the sintering aid is Y2O3, and the particle size of the sintering aid is 6-8 μm;

[0076] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 4 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 78 wt%.

[0077] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.1W, the exposure time is 15s, and the model placement angle is 45°.

[0078] Step 4: Place the ceramic green body in a low-temperature furnace at 1050℃ for 1 hour to degrease it, and then sinter it in a nitrogen atmosphere furnace at 1750℃ for 1 hour to obtain orthopedic silicon nitride ceramic.

[0079] Example 9

[0080] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0081] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 200 nm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 1% of the mass of the silicon nitride powder, the sintering aid is MgO, and the particle size of the sintering aid is 3-5 μm;

[0082] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 76 wt%.

[0083] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.1W, the exposure time is 10s, and the model placement angle is 45°;

[0084] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0085] Example 10

[0086] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0087] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 5 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 10% of the mass of the silicon nitride powder, the sintering aid is Al2O3, and the particle size of the sintering aid is 1-3 μm;

[0088] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 6 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 82 wt%.

[0089] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.3W, the exposure time is 15s, and the model placement angle is 45°;

[0090] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 2 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0091] Example 11

[0092] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0093] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 3 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 5% of the mass of the silicon nitride powder, the sintering aid is Yb2O3, and the particle size of the sintering aid is 3-5 μm;

[0094] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 5 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 80 wt%.

[0095] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.2W, the exposure time is 15s, and the model placement angle is 45°;

[0096] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0097] Example 12

[0098] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0099] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 10% of the mass of the silicon nitride powder, the sintering aid is Nd2O3, and the particle size of the sintering aid is 6-8 μm;

[0100] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 78 wt%.

[0101] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.1W, the exposure time is 12s, and the model placement angle is 45°;

[0102] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 0.5h to degrease, and then sinter it in a nitrogen atmosphere furnace at 1700℃ for 2h to obtain orthopedic silicon nitride ceramic.

[0103] Example 13

[0104] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0105] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 200 nm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 2% of the mass of the silicon nitride powder, the sintering aid is Eu2O3, and the particle size of the sintering aid is 3-5 μm;

[0106] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 76 wt%.

[0107] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2W, the exposure time is 10s, and the model placement angle is 45°;

[0108] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1900℃ for 0.5 hours to obtain orthopedic silicon nitride ceramic.

[0109] Example 14

[0110] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0111] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 5 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 15% of the mass of the silicon nitride powder, the sintering aid is La2O3, and the particle size of the sintering aid is 1-3 μm;

[0112] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 8 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 85 wt%.

[0113] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.5W, the exposure time is 15s, and the model placement angle is 45°;

[0114] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 0.5h to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 1h to obtain orthopedic silicon nitride ceramic.

[0115] Example 15

[0116] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0117] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 3 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 20% of the mass of the silicon nitride powder, the sintering aid is Sm2O3, and the particle size of the sintering aid is 3-5 μm;

[0118] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 5 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 80 wt%.

[0119] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.3W, the exposure time is 20s, and the model placement angle is 45°;

[0120] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0121] Example 16

[0122] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0123] Step 1: Add the sintering aid to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 12% of the mass of the silicon nitride powder, the sintering aid is CeO, and the particle size of the sintering aid is 6-8 μm;

[0124] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 4 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 78 wt%.

[0125] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.1W, the exposure time is 15s, and the model placement angle is 45°;

[0126] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 0.5h to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2h to obtain orthopedic silicon nitride ceramic.

[0127] Example 17

[0128] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0129] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 200 nm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 7% of the mass of the silicon nitride powder, the sintering aid is 4 wt.% Y2O3 + 3 wt.% CeO, and the particle size of the sintering aid is 3-5 μm; the mass of the second reinforcing phase is 0.01% of the mass of the silicon nitride powder, the second reinforcing phase is TiC particles, and the size of the TiC particles is 2 μm;

[0130] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 82 wt%.

[0131] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.3W, the exposure time is 15s, and the model placement angle is 45°;

[0132] Step 4: Place the ceramic green body in a low-temperature furnace at 1050℃ for 1 hour to degrease it, and then sinter it in a nitrogen atmosphere furnace at 1750℃ for 1 hour to obtain orthopedic silicon nitride ceramic.

[0133] Example 18

[0134] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0135] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 5 μm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a mixed powder; the mass of the sintering aid is 20% of the mass of the silicon nitride powder, the sintering aid is 10 wt.% Y2O3 + 5 wt.% Al2O3 + 5 wt.% MgO, and the particle size of the sintering aid is 1-3 μm; the mass of the second reinforcing phase is 5% of the mass of the silicon nitride powder, the second reinforcing phase is TiC particles, and the size of the TiC particles is 5 μm;

[0136] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 10 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 82 wt%.

[0137] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.3W, the exposure time is 20s, and the model placement angle is 45°;

[0138] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0139] Example 19

[0140] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0141] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 200 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a mixed powder; the mass of the sintering aid is 0.01% of the mass of the silicon nitride powder, the sintering aid is 0.005 wt.% Eu2O3 + 0.005 wt.% La2O3, and the particle size of the sintering aid is 3-5 μm; the mass of the second reinforcing phase is 10% of the mass of the silicon nitride powder, the second reinforcing phase is TiC particles, and the size of the TiC particles is 7 μm;

[0142] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 78 wt%.

[0143] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.1W, the exposure time is 20s, and the model placement angle is 45°;

[0144] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 0.5h to degrease, and then sinter it in a nitrogen atmosphere furnace at 1700℃ for 2h to obtain orthopedic silicon nitride ceramic.

[0145] Example 20

[0146] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0147] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 3 μm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a mixed powder; the mass of the sintering aid is 10% of the mass of the silicon nitride powder, and the sintering aid consists of 2 wt.% Y₂O₃ + 2 wt.% MgO + 2 wt.% Al₂O₃ + 2 wt.% Yb₂O₃ + 1 wt.% Nd₂O₃ + 1 wt.% CeO, with a particle size of 3-5 μm; the mass of the second reinforcing phase is 0.01% of the mass of the silicon nitride powder, and the second reinforcing phase is SiC whiskers with an aspect ratio of 30;

[0148] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 5 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 86 wt%.

[0149] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.5W, the exposure time is 20s, and the model placement angle is 45°;

[0150] Step 4: Place the ceramic green body in a low-temperature furnace at 1050℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 1 hour to obtain orthopedic silicon nitride ceramic.

[0151] Example 21

[0152] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0153] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 0.01% of the mass of the silicon nitride powder, the sintering aid is Y2O3, and the particle size of the sintering aid is 6-8 μm; the mass of the second reinforcing phase is 2% of the mass of the silicon nitride powder, the second reinforcing phase is SiC whiskers, and the aspect ratio of the SiC whiskers is 50;

[0154] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 4 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 86 wt%.

[0155] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.5W, the exposure time is 20s, and the model placement angle is 45°;

[0156] Step 4: Place the ceramic green body in a low-temperature furnace at 1050℃ for 1 hour to degrease it, and then sinter it in a nitrogen atmosphere furnace at 1750℃ for 1 hour to obtain orthopedic silicon nitride ceramic.

[0157] Example 22

[0158] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0159] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 200 nm, and ball mill for 2 hours to ensure uniform mixing and obtain a mixed powder; the mass of the sintering aid is 1% of the mass of the silicon nitride powder, the sintering aid is MgO, and the particle size of the sintering aid is 3-5 μm; the mass of the second reinforcing phase is 10% of the mass of the silicon nitride powder, the second reinforcing phase is SiC whiskers, and the aspect ratio of the SiC whiskers is 60.

[0160] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 85 wt%.

[0161] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.4W, the exposure time is 20s, and the model placement angle is 45°;

[0162] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0163] Example 23

[0164] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0165] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 5 μm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a mixed powder; the mass of the sintering aid is 10% of the mass of the silicon nitride powder, the sintering aid is Al2O3, and the particle size of the sintering aid is 1-3 μm; the mass of the second reinforcing phase is 0.01% of the mass of the silicon nitride powder, the second reinforcing phase is graphene, and the graphene size is 30 μm;

[0166] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 10 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 86 wt%.

[0167] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.6W, the exposure time is 20s, and the model placement angle is 45°;

[0168] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 2 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0169] Example 24

[0170] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0171] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 3 μm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a mixed powder; the mass of the sintering aid is 20% of the mass of the silicon nitride powder, the sintering aid is Sm2O3, and the particle size of the sintering aid is 3-5 μm; the mass of the second reinforcing phase is 4% of the mass of the silicon nitride powder, the second reinforcing phase is graphene, and the graphene size is 50 μm;

[0172] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 5 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 85 wt%.

[0173] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.4W, the exposure time is 20s, and the model placement angle is 45°;

[0174] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0175] Example 25

[0176] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0177] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing, thereby obtaining a mixed powder; the mass of the sintering aid is 12% of the mass of the silicon nitride powder, the sintering aid is CeO, and the particle size of the sintering aid is 6-8 μm; the mass of the second reinforcing phase is 10% of the mass of the silicon nitride powder, the second reinforcing phase is graphene, and the graphene size is 80 μm;

[0178] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 4 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 86 wt%.

[0179] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.5W, the exposure time is 20s, and the model placement angle is 45°;

[0180] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 0.5h to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2h to obtain orthopedic silicon nitride ceramic.

[0181] Example 26

[0182] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0183] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 200 nm, and ball mill for 2 hours to ensure uniform mixing, obtaining a mixed powder; the mass of the sintering aid is 7% of the mass of the silicon nitride powder, the sintering aid is 4 wt.% Y₂O₃ + 3 wt.% CeO, and the particle size of the sintering aid is 3-5 μm; the mass of the second reinforcing phase is 5% of the mass of the silicon nitride, the second reinforcing phase is 3 wt.% TiC particles + 2 wt.% SiC whiskers; the size of the TiC particles is 6 μm; the aspect ratio of the SiC whiskers is 80.

[0184] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 5 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 83 wt%.

[0185] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.3W, the exposure time is 20s, and the model placement angle is 45°;

[0186] Step 4: Place the ceramic green body in a low-temperature furnace at 1050℃ for 1 hour to degrease it, and then sinter it in a nitrogen atmosphere furnace at 1750℃ for 1 hour to obtain orthopedic silicon nitride ceramic.

[0187] Example 27

[0188] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0189] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 5 μm, and ball mill for 2 hours to ensure uniform mixing, obtaining a mixed powder; the mass of the sintering aid is 20% of the mass of the silicon nitride powder, and the sintering aid consists of 10 wt.% Y₂O₃ + 5 wt.% Al₂O₃ + 5 wt.% MgO, with a particle size of 1-3 μm; the mass of the second reinforcing phase is 10% of the mass of the silicon nitride, and the second reinforcing phase consists of 4 wt.% TiC particles + 3 wt.% SiC whiskers + 3 wt.% graphene; the size of the TiC particles is 6 μm, the aspect ratio of the SiC whiskers is 40, and the size of the graphene is 60 μm;

[0190] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 10 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 86 wt%.

[0191] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.6W, the exposure time is 20s, and the model placement angle is 45°;

[0192] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1850℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0193] Example 28

[0194] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0195] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 3 μm, and ball mill for 2 hours to ensure uniform mixing, obtaining a mixed powder; the mass of the sintering aid is 15% of the mass of the silicon nitride powder, and the sintering aid consists of 7 wt.% Y₂O₃ + 4 wt.% Al₂O₃ + 4 wt.% Yb₂O₃, with a particle size of 3-5 μm; the mass of the second reinforcing phase is 8% of the mass of the silicon nitride, and the second reinforcing phase consists of 3 wt.% TiC particles + 3 wt.% SiC whiskers + 2 wt.% graphene; the TiC particles have a size of 3 μm, the SiC whiskers have an aspect ratio of 90, and the graphene has a size of 80 μm;

[0196] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 6 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 85 wt%.

[0197] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.5W, the exposure time is 20s, and the model placement angle is 45°;

[0198] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 2 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0199] Example 29

[0200] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0201] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing, obtaining a mixed powder; the mass of the sintering aid is 12% of the mass of the silicon nitride powder, and the sintering aid consists of 5 wt.% Al2O3 + 4 wt.% Nd2O3 + 3 wt.% Yb2O3, with a particle size of 6-8 μm; the mass of the second reinforcing phase is 6% of the mass of the silicon nitride, and the second reinforcing phase consists of 2 wt.% TiC particles + 2 wt.% SiC whiskers + 2 wt.% graphene; the TiC particles have a size of 7 μm, the SiC whiskers have an aspect ratio of 100, and the graphene has a size of 60 μm;

[0202] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 6 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 85 wt%.

[0203] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.5W, the exposure time is 18s, and the model placement angle is 45°;

[0204] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1800℃ for 2 hours to obtain orthopedic silicon nitride ceramic.

[0205] Example 30

[0206] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0207] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing, obtaining a mixed powder; the mass of the sintering aid is 12% of the mass of the silicon nitride powder, and the sintering aid consists of 5 wt.% Al2O3 + 4 wt.% Nd2O3 + 3 wt.% Yb2O3, with a particle size of 6-8 μm; the mass of the second reinforcing phase is 0.01% of the mass of silicon nitride, and the second reinforcing phase consists of 0.005 wt.% TiC particles + 0.003 wt.% SiC whiskers + 0.002 wt.% graphene; the size of the TiC particles is 2 μm, the aspect ratio of the SiC whiskers is 30, and the size of the graphene is 20 μm;

[0208] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 4 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 85 wt%.

[0209] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.4W, the exposure time is 22s, and the model placement angle is 45°;

[0210] Step 4: Place the ceramic green body in a low-temperature furnace at 1200℃ for 0.5h to degrease, and then sinter it in a nitrogen atmosphere furnace at 1700℃ for 2h to obtain orthopedic silicon nitride ceramic.

[0211] Example 31

[0212] This embodiment provides a method for preparing orthopedic silicon nitride ceramics, including:

[0213] Step 1: Add the sintering aid and the second reinforcing phase to silicon nitride powder with an average particle size of 10 μm, and ball mill for 2 hours to ensure uniform mixing, obtaining a mixed powder; the mass of the sintering aid is 12% of the mass of the silicon nitride powder, the sintering aid is 5 wt.% Al2O3 + 4 wt.% Nd2O3 + 3 wt.% Yb2O3, and the particle size of the sintering aid is 6-8 μm; the mass of the second reinforcing phase is 2% of the mass of silicon nitride, the second reinforcing phase is 1 wt.% TiC particles + 0.5 wt.% SiC whiskers + 0.5 wt.% graphene; the size of the TiC particles is 10 μm, the aspect ratio of the SiC whiskers is 50, and the size of the graphene is 30 μm;

[0214] Step 2: Mix the powder with a resin that absorbs at a wavelength of 405 nm, and ball mill for 4 hours to ensure uniform mixing, thereby obtaining a ceramic slurry; the resin is a casting resin purchased from UNIZ; the solid content of the ceramic slurry is 83 wt%.

[0215] Step 3: Use a DLP 3D printing device to perform photopolymerization printing on the ceramic slurry to obtain a ceramic green body; in the photopolymerization printing, the power is 2.3W, the exposure time is 20s, and the model placement angle is 45°;

[0216] Step 4: Place the ceramic green body in a low-temperature furnace at 1150℃ for 1.5 hours to degrease, and then sinter it in a nitrogen atmosphere furnace at 1900℃ for 0.5 hours to obtain orthopedic silicon nitride ceramic.

[0217] Performance Evaluation

[0218] Based on GB / T 23805, the room temperature tensile strength test method for fine ceramics, the fracture toughness of orthopedic silicon nitride ceramics in Examples 1 to 31 is shown in Table 1.

[0219] Table 1 Fracture toughness of orthopedic silicon nitride ceramics in Examples 1-31

[0220]

[0221]

[0222] As shown in Table 1, by using the second reinforcing phase of the present invention, which includes TiC particles, SiC whiskers and graphene, and under the action of sintering aids, the fracture toughness of silicon nitride ceramics can be effectively improved through low-temperature debinding and high-temperature sintering, thus obtaining silicon nitride ceramic materials with significantly improved mechanical properties.

[0223] The above description is merely a preferred embodiment of the present invention and does not constitute any limitation on the present invention. Any simple modifications, alterations, or equivalent structural changes made to the above embodiments based on the technical essence of the invention shall still fall within the protection scope of the present invention.

Claims

1. A method for preparing orthopedic silicon nitride ceramics, characterized in that, The raw materials include silicon nitride and sintering aids, and the method specifically includes: The sintering aid was mixed with silicon nitride to obtain a mixed powder; The mixed powder is mixed with resin to obtain a ceramic slurry; The ceramic slurry was subjected to photocuring, low-temperature degreasing, and high-temperature sintering to obtain orthopedic silicon nitride ceramics; The silicon nitride has a particle size of 0.2~10μm; the sintering aid has a particle size of 1~8μm; the resin is a resin with an absorption wavelength of 405nm; the solid content of the ceramic slurry is 75wt%~86wt%; the low-temperature debinding temperature is 1050~1200℃, and the time is 0.5~2h; the high-temperature sintering temperature is 1700~1900℃, and the time is 0.5~2h; the method for obtaining the ceramic slurry includes ball milling for 2~10h; the raw material also includes a second reinforcing phase, which is TiC particles, SiC whiskers and graphene, and the mass of the second reinforcing phase is 2~10% of the mass of silicon nitride; the method includes mixing the sintering aid and the second reinforcing phase with silicon nitride to obtain a mixed powder; The sintering aid has a mass of 12-20% of the silicon nitride mass; the TiC particle size is 2-10 μm; the SiC whisker aspect ratio is 30-100; and the graphene size is 20-80 μm.

2. The method for preparing orthopedic silicon nitride ceramics according to claim 1, characterized in that, The sintering aid is one or more of Y2O3, MgO, Al2O3, Yb2O3, Nd2O3, Eu2O3, La2O3, and Sm2O3.

Citation Information

Patent Citations

  • High-wear-resistance silicon nitride-based ceramic, and preparation method and application thereof

    CN111517805A

  • High-toughness silicon nitride ceramic and preparation method thereof

    CN111517806A

  • Preparation method of silicon nitride acetabular cup

    CN112174676A