A nanofiber-doped polybenzimidazole composite membrane and preparation method thereof

Through the preparation method of nanofiber-doped polybenzimidazole composite membranes, the problems of vanadium ion penetration and electrolyte cross-contamination in perfluorosulfonic acid membranes in vanadium redox flow batteries are solved, and a battery with high ion conductivity and low cost is achieved. Membrane materials improve battery performance and efficiency.

CN118459812BActive Publication Date: 2024-10-18HANGZHOU DEHAI AIKE ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410923877.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-18
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Existing perfluorosulfonic acid membranes have problems such as vanadium ion penetration and electrolyte cross-contamination in vanadium redox flow batteries, resulting in low Coulombic efficiency, poor battery performance, and high cost. It is necessary to develop membranes with low vanadium ion penetration and high ion Conductivity, low-cost battery membrane materials.

Method used

The preparation method of nanofiber-doped polybenzimidazole composite membranes is adopted, and through halogenated alkylation and graft modification of amphoteric multi-ion exchange group polymers, combined with electrospinning technology, a nanofiber-doped polybenzimidazole composite membrane with long-range ordered ion transmission channels is formed. Fiber membrane, combined with polybenzimidazole-based membrane, improves ionic conductivity and vanadium resistance.

Benefits of technology

The ionic conductivity and vanadium resistance of the composite membrane are significantly improved, the voltage efficiency and energy efficiency of the battery are improved, and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118459812B_ABST
    Figure CN118459812B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of vanadium flow batteries, and in particular to a nanofiber-doped polybenzimidazole composite membrane and a preparation method thereof. Specifically, the process comprises reacting polybenzimidazole with halogenated alkanes, amine compounds, and lactone compounds to prepare amphoteric polybenzimidazole with multiple ion exchange groups, then compounding the polybenzimidazole with an ion conductive polymer, preparing nanofibers by an electrospinning method, and finally doping the nanofibers into a polybenzimidazole-based membrane to form a nanofiber-doped polybenzimidazole composite membrane. The present invention prepares polybenzimidazole containing multiple ion exchange groups and quaternary ammonium groups by modification, and compounding the nanofibers with an ion conductive polymer containing a sulfonic acid group to prepare nanofibers doped into a polybenzimidazole-based membrane, thereby greatly improving the ionic conductivity of the membrane while maintaining a relatively high vanadium resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of vanadium liquid flow batteries, and in particular to a nanofiber-doped polybenzimidazole composite membrane and a preparation method thereof. Background Art

[0002] Vanadium flow battery (VFB) is considered to be one of the most promising large-scale and long-term energy storage technologies for industrialization due to its special advantages such as energy and power decoupling, scalability, and intrinsic safety generated by water-based electrolytes. As a key component of all-vanadium flow batteries, ion exchange membranes play the role of isolating the active substances of the positive and negative electrolytes and transferring carriers in the battery. To date, perfluorosulfonic acid membranes (such as Nafion) have been widely used due to their high proton conductivity and excellent chemical stability. However, their main disadvantages are crossover problems caused by extensive ion transport channels and high costs. During the long-term operation of the battery, Nafion membranes have serious vanadium ion penetration, electrolyte cross-contamination and other problems, resulting in low coulombic efficiency and poor battery performance. Therefore, it is crucial to develop battery membrane materials with low vanadium ion penetration, high ion conductivity, high ion selectivity and low cost.

[0003] Non-fluorinated ion exchange membranes have the advantages of good ion selectivity, high ion conductivity and low cost, and are one of the important membrane materials. By modifying non-fluorinated polymer substrates such as polyetheretherketone, polyethersulfone, polybenzimidazole, and polyimide, they have ion conductivity. Polybenzimidazole (PBI) is a class of polymers with high stability and relatively low cost. As a member of non-fluorinated ion exchange membranes, its dense rigid skeleton structure has excellent vanadium resistance, so it has good application prospects in vanadium flow batteries. However, due to its dense characteristics and the absence of ion exchange groups in its molecular structure, its ion conductivity is extremely low. Summary of the invention

[0004] In order to solve the above problems, the present invention discloses a method for preparing a nanofiber-doped polybenzimidazole composite membrane, which specifically comprises the following steps:

[0005] Step S1, preparation of halogenated alkylated polybenzimidazole: 5-20 parts of polybenzimidazole powder and 800-1000 parts of solvent are heated and stirred to dissolve, cooled to 25°C, 3-4 parts of sodium hydride are added for the first reaction, and when the system temperature drops to 0°C, 0.85-1.25 parts of halogenated hydrocarbon are added for the second reaction, the reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and dried in vacuo at 30°C for 24 hours to obtain halogenated alkylated polybenzimidazole;

[0006] Step S2, preparation of amphoteric polybenzimidazole with multiple ion exchange groups: take 5-20 parts of the halogenated alkylated polybenzimidazole and 800-1000 parts of a solvent, heat and stir to dissolve, cool to 25°C, add 1.5-2 parts of an amine compound, mix and stir evenly, heat to carry out a third reaction, lower the temperature of the reaction system to 0°C, then dropwise add 3-6 parts of a lactone compound, mix and stir evenly, heat to 25°C and stir to carry out a fourth reaction, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and vacuum dry at 30°C for 24h to obtain amphoteric polybenzimidazole with multiple ion exchange groups;

[0007] Step S3, preparation of nanofiber membrane: 2.5-7.5 parts of amphoteric polybenzimidazole with multiple ion exchange groups, 7.5-10 parts of ion conductive polymer, and 75-85 parts of solvent are added, heated and stirred to obtain a spinning solution, and the spinning solution is electrostatically spun and then heat-treated to obtain a nanofiber membrane;

[0008] Step S4, preparation of nanofiber-doped polybenzimidazole composite membrane: take 3-8 parts of polybenzimidazole powder and 87-95 parts of solvent, heat and stir to dissolve, cool to 25°C, add 2-5 parts of nanofiber membrane, use a high-speed stirring disperser to stir and disperse to obtain a membrane-making liquid, cast the membrane-making liquid on a glass plate, and heat treat to obtain a nanofiber-doped polybenzimidazole composite membrane.

[0009] Preferably, the solvent in step S1 is any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone, and the halogenated hydrocarbon is any one of 1-bromo-4-chlorobutane, 1-bromo-3-chloropropane, 1-bromo-3,4-dichlorobutane, and 1-bromo-3-chloro-2-propanol.

[0010] Preferably, the heating stirring dissolution temperature in step S1 is 80-100° C., the time is 2-4 h, the first reaction time is 20-40 h, and the second reaction time is 10-20 h.

[0011] Preferably, the solvent in step S2 is any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone, the amine compound is any one of tetraethylenepentamine, triethylenetetramine, pentaethylenehexamine, N,N,N',N'-tetrakis(3-aminopropyl)-1,4-butanediamine, tris(2-aminoethyl)amine, and 1,4,7,10-tetraazacyclododecane, and the lactone compound is any one of 1,3-propanesultone, 1,4-butanesultone, β-propiolactone, and 1,4-butyrolactone.

[0012] Preferably, the heating and stirring temperature in step S2 is 80-100° C., the time is 2-4 h, the third reaction temperature is 50-70° C., the third reaction time is 20-40 h, and the fourth reaction time is 5-10 h.

[0013] Preferably, the ion conductive polymer in step S3 is any one of perfluorosulfonic acid resin, sulfonated polyetheretherketone, sulfonated polyethersulfone, and sulfonated polyimide, and the solvent is any one of N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide.

[0014] Preferably, the heating and stirring temperature in step S3 is 80~100°C, and the heating and stirring time is 2~4h; the electrospinning conditions are temperature 25~30°C, humidity 10~30%, voltage 12~18kV, injection speed 0.8~1.4ml / h, and receiving distance 12~18cm; the heat treatment temperature is 140~180°C, and the time is 2~4h.

[0015] Preferably, the solvent in step S4 is any one of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

[0016] Preferably, the heating and stirring temperature in step S4 is 80-100°C, the time is 2-4h, the stirring and dispersing time of the high-speed stirring and dispersing machine is 2-6min, the speed is 3000-6000r / min, and the heat treatment temperature is 80-120°C, and the time is 2-4h.

[0017] The invention discloses a nanofiber-doped polybenzimidazole composite membrane, which is prepared by adopting the above-mentioned method for preparing a nanofiber-doped polybenzimidazole composite membrane.

[0018] Beneficial effects of the present invention:

[0019] 1. In the preparation process of the polybenzimidazole composite membrane of the present invention, nanofibers are prepared by electrospinning an ion conductive polymer containing a sulfonic acid group, the base membrane is doped, and a long-range orderly ion transmission channel is formed in the thickness direction of the composite membrane, which significantly improves the ion conductivity of the membrane.

[0020] 2. In the preparation process of the polybenzimidazole composite membrane of the present invention, the polybenzimidazole of the spinning substrate is grafted and modified to prepare the amphoteric polybenzimidazole with multiple ion exchange groups, so that it contains multiple sulfonic acid groups and quaternary ammonium groups, which is used for preparing nanofibers by electrospinning, thereby improving the ionic conductivity of the nanofibers while maintaining a high vanadium resistance, thereby also improving the ionic conductivity and vanadium resistance of the composite membrane.

[0021] 3. In the preparation process of the polybenzimidazole composite membrane of the present invention, nanofibers are prepared by compounding polybenzimidazole with amphoteric multiple ion exchange groups and ion conductive polymers, which not only forms long-range orderly ion transmission channels inside the fibers, but also constructs acid-base proton transmission channels at the interface between the sulfonic acid groups on the fiber surface and the base membrane, thereby further improving the ion conductivity of the composite membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of a nanofiber-doped polybenzimidazole composite membrane and a preparation method thereof according to the present invention;

[0023] Figure 2 The synthetic reaction flow chart of the amphoteric multi-ion exchange group polybenzimidazole in Example 1 of the present invention;

[0024] Figure 3 The infrared images of polybenzimidazole, halogenated alkylated polybenzimidazole and amphoteric polybenzimidazole with multiple ion exchange groups in Example 1 of the present invention are shown;

[0025] Figure 4 This is a scanning electron microscope image of the nanofiber and polybenzimidazole composite membrane in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below through the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0027] See also Figure 1 The present invention discloses a nanofiber-doped polybenzimidazole composite membrane and a preparation method thereof: first, polybenzimidazole is grafted with halogenated alkane to prepare halogenated alkylated polybenzimidazole. Secondly, halogenated alkylated polybenzimidazole reacts with amine compounds and lactone compounds to prepare amphoteric polybenzimidazole with multiple ion exchange groups. Further, the amphoteric polybenzimidazole with multiple ion exchange groups is composited with an ion conductive polymer to prepare nanofibers by an electrospinning method. Finally, the nanofibers are doped into a polybenzimidazole-based membrane to form a nanofiber-doped polybenzimidazole composite membrane.

[0028] Embodiment 1:

[0029] Step 1: Preparation of halogenated alkylated polybenzimidazole: 1) Take 5 parts of polybenzimidazole powder and 800 parts of N,N-dimethylformamide, heat and stir at 80°C for 2 hours to dissolve, cool to 25°C, add 3 parts of sodium hydride, and continue to stir and react for 20 hours. The temperature of the reaction system is lowered to 0°C, 0.85 parts of 1-bromo-4-chlorobutane is added, and the reaction is stirred for 10 hours. The reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and vacuum dried at 30°C for 24 hours to obtain halogenated alkylated polybenzimidazole.

[0030] Step 2: Preparation of amphoteric polybenzimidazole with multiple ion exchange groups: Take 5 parts of halogenated alkylated polybenzimidazole in step 1 and 800 parts of N,N-dimethylformamide, heat and stir at 80°C for 2 hours to dissolve, cool to 25°C, add 1.5 parts of tetraethylenepentamine, mix and stir for 0.5 hours, heat to 50°C, continue stirring and reacting for 20 hours, lower the temperature of the reaction system to 0°C, then add 3 parts of 1,3-propanesulfonic acid lactone dropwise, mix and stir for 0.5 hours, heat to 25°C and stir and react for 5 hours, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and vacuum dry at 30°C for 24 hours to obtain amphoteric polybenzimidazole with multiple ion exchange groups. Figure 2 As shown in the synthetic reaction flow chart of the polybenzimidazole in this embodiment to prepare the amphoteric polybenzimidazole with multiple ion exchange groups, the infrared characterization spectrum of the synthetic reaction product is as shown in Figure 3 As shown, at 2918cm -1 and 1442cm -1 The characteristic absorption at the two locations is due to the symmetrical stretching vibration of CH in the haloalkane, proving the successful preparation of halogenated alkylated polybenzimidazole, 1643 cm -1 The absorption characteristics of CH and NH groups are shown at 1178 cm -1 and 1078cm -1 The characteristic absorption peak at corresponds to the stretching vibration of S=O, indicating the successful introduction of sulfonic acid groups, thereby proving the successful preparation of amphoteric multi-ion exchange group polybenzimidazole.

[0031] Step 3: Preparation of nanofiber membrane: Take 2.5 parts of the amphoteric polybenzimidazole with multiple ion exchange groups in step 2, 7.5 parts of perfluorosulfonic acid resin, and 75 parts of N,N-dimethylformamide, and heat and stir at 80°C for 2h to obtain a spinning solution. Electrospin the spinning solution, and control the electrospinning conditions to 25°C, 10% humidity, 12kV voltage, 0.8ml / min injection speed, and 12cm receiving distance to obtain an electrospun nanofiber membrane. Heat treat at 140°C for 2h to obtain a nanofiber membrane.

[0032] Step 4: Preparation of nanofiber doped polybenzimidazole composite membrane: Cut the nanofiber membrane prepared in step 3 into 2mm×2mm size. Take 3 parts of polybenzimidazole powder and 87 parts of N,N-dimethylformamide, heat and stir at 80℃ for 2h to dissolve, cool to 25℃, add 2 parts of the cut nanofiber membrane, stir and disperse with a high-speed stirring disperser for 2min at a speed of 3000r / min to obtain a membrane-making solution. Cast the membrane-making solution on a glass plate and heat treat at 80℃ for 2h to obtain a nanofiber doped polybenzimidazole composite membrane. Figure 4 As shown, the scanning electron microscope image of the nanofiber and polybenzimidazole composite membrane of this embodiment illustrates the successful preparation of the nanofiber and polybenzimidazole composite membrane.

[0033] Embodiment 2:

[0034] Step 1: Preparation of halogenated alkylated polybenzimidazole: 1) Take 7.5 parts of polybenzimidazole powder and 840 parts of N,N-dimethylacetamide, heat and stir at 84°C for 2.4 hours to dissolve, cool to 25°C, add 3.2 parts of sodium hydride, and continue to stir and react for 24 hours. The temperature of the reaction system is lowered to 0°C, 0.9 parts of 1-bromo-3-chloropropane is added, and the reaction is stirred for 12 hours. The reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and vacuum dried at 30°C for 24 hours to obtain halogenated alkylated polybenzimidazole.

[0035] Step 2: Preparation of amphoteric polybenzimidazole with multiple ion exchange groups: Take 7.5 parts of halogenated alkylated polybenzimidazole in step 1 and 840 parts of N,N-dimethylacetamide, heat and stir at 84°C for 2.4 hours to dissolve, cool to 25°C, add 1.6 parts of triethylenetetramine, mix and stir for 0.75 hours, heat to 55°C, continue stirring and reacting for 25 hours, lower the temperature of the reaction system to 0°C, then add 3.5 parts of 1,4-butanesulfonic acid lactone dropwise, mix and stir for 0.75 hours, heat to 25°C and stir and react for 6 hours, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and dry in vacuo at 30°C for 24 hours to obtain amphoteric polybenzimidazole with multiple ion exchange groups.

[0036] Step 3: Preparation of nanofiber membrane: Take 3.5 parts of the amphoteric polyion exchange group polybenzimidazole in step 2, 8 parts of sulfonated polyetheretherketone, and 77 parts of N,N-dimethylacetamide, and heat and stir at 84°C for 2.4 hours to obtain a spinning solution. Electrospin the spinning solution, and control the electrospinning conditions, temperature 26°C, humidity 15%, voltage 13kV, injection speed 0.9ml / min, receiving distance 13cm, to obtain an electrospun nanofiber membrane. Heat treatment at 150°C for 2.4 hours to obtain a nanofiber membrane.

[0037] Step 4: Preparation of nanofiber-doped polybenzimidazole composite membrane: Cut the nanofiber membrane prepared in step 3 into 2mm×2mm size. Take 4 parts of polybenzimidazole powder and 89 parts of N,N-dimethylacetamide, heat and stir at 84℃ for 2.4h to dissolve, cool to 25℃, add 2.5 parts of the cut nanofiber membrane, stir and disperse with a high-speed stirring disperser for 3min at a speed of 3500r / min to obtain a membrane solution. Cast the membrane solution on a glass plate and heat treat at 90℃ for 2.4h to obtain a nanofiber-doped polybenzimidazole composite membrane.

[0038] Embodiment three:

[0039] Step 1: Preparation of halogenated alkylated polybenzimidazole: 1) Take 10 parts of polybenzimidazole powder and 880 parts of dimethyl sulfoxide, heat and stir at 88°C for 2.8 hours to dissolve, cool to 25°C, add 3.4 parts of sodium hydride, and continue to stir and react for 28 hours. The temperature of the reaction system is lowered to 0°C, 0.95 parts of 1-bromo-3,4-dichlorobutane is added, and the reaction is stirred for 14 hours. The reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and vacuum dried at 30°C for 24 hours to obtain halogenated alkylated polybenzimidazole.

[0040] Step 2: Preparation of amphoteric polybenzimidazole with multiple ion exchange groups: Take 10 parts of the halogenated alkylated polybenzimidazole in step 1 and 880 parts of dimethyl sulfoxide, heat and stir at 88°C for 2.8 hours to dissolve, cool to 25°C, add 1.7 parts of pentaethylenehexamine, mix and stir for 0.95 hours, heat to 58°C, continue to stir and react for 28 hours, lower the temperature of the reaction system to 0°C, then add 4 parts of β-propiolactone dropwise, mix and stir for 0.95 hours, heat to 25°C and stir and react for 7 hours, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and dry in vacuo at 30°C for 24 hours to obtain amphoteric polybenzimidazole with multiple ion exchange groups.

[0041] Step 3: Preparation of nanofiber membrane: Take 5 parts of the amphoteric polybenzimidazole with multiple ion exchange groups in step 2, 8.5 parts of sulfonated polyethersulfone, and 79 parts of dimethyl sulfoxide, and heat and stir at 88°C for 2.8 hours to obtain a spinning solution. Electrospin the spinning solution, and control the electrospinning conditions to 27°C, 18% humidity, 14kV voltage, 1.0ml / min injection speed, and 14cm receiving distance to obtain an electrospun nanofiber membrane. Heat treat at 160°C for 2.8 hours to obtain a nanofiber membrane.

[0042] Step 4: Preparation of nanofiber-doped polybenzimidazole composite membrane: Cut the nanofiber membrane prepared in step 3 into 2mm×2mm size. Take 5 parts of polybenzimidazole powder and 91 parts of dimethyl sulfoxide, heat and stir at 88℃ for 2.8h to dissolve, cool to 25℃, add 3 parts of cut nanofiber membrane, stir and disperse with a high-speed stirring disperser for 4min, speed 4000r / min, and obtain membrane solution. Cast the membrane solution on a glass plate and heat treat at 95℃ for 2.8h to obtain a nanofiber-doped polybenzimidazole composite membrane.

[0043] Embodiment 4:

[0044] Step 1: Preparation of halogenated alkylated polybenzimidazole: 1) Take 15 parts of polybenzimidazole powder and 920 parts of N-methylpyrrolidone, heat and stir at 92°C for 3.2 hours to dissolve, cool to 25°C, add 3.6 parts of sodium hydride, and continue to stir and react for 32 hours. The temperature of the reaction system is lowered to 0°C, 1.05 parts of 1-bromo-3-chloro-2-propanol are added, and the reaction is stirred for 16 hours. The reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and vacuum dried at 30°C for 24 hours to obtain halogenated alkylated polybenzimidazole.

[0045] Step 2: Preparation of amphoteric polybenzimidazole with multiple ion exchange groups: Take 15 parts of the halogenated alkylated polybenzimidazole in step 1 and 920 parts of N-methylpyrrolidone, heat and stir at 92°C for 3.2 hours to dissolve, cool to 25°C, add 1.8 parts of N,N,N',N'-tetrakis(3-aminopropyl)-1,4-butanediamine, mix and stir for 1.15 hours, heat to 62°C, continue stirring and reacting for 32 hours, lower the temperature of the reaction system to 0°C, then add 5 parts of 1,4-butyrolactone dropwise, mix and stir for 1.15 hours, heat to 25°C and stir and react for 8 hours, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and dry in vacuo at 30°C for 24 hours to obtain amphoteric polybenzimidazole with multiple ion exchange groups.

[0046] Step 3: Preparation of nanofiber membrane: Take 5.5 parts of the amphoteric polybenzimidazole, 9 parts of sulfonated polyimide, and 81 parts of N,N-dimethylformamide in step 2, and heat and stir at 92°C for 3.2 hours to obtain a spinning solution. Electrospin the spinning solution, and control the electrospinning conditions to 28°C, 22% humidity, 16kV voltage, 1.2ml / min injection speed, and 16cm receiving distance to obtain an electrospun nanofiber membrane. Heat treat at 165°C for 3.2 hours to obtain a nanofiber membrane.

[0047] Step 4: Preparation of nanofiber-doped polybenzimidazole composite membrane: Cut the nanofiber membrane prepared in step 3 into 2mm×2mm size. Take 6 parts of polybenzimidazole powder and 92 parts of N,N-dimethylformamide, heat and stir at 92℃ for 3.2h to dissolve, cool to 25℃, add 4 parts of cut nanofiber membrane, stir and disperse with a high-speed stirring disperser for 4.5min, speed 5000r / min, and obtain membrane solution. Cast the membrane solution on a glass plate and heat treat at 105℃ for 3.2h to obtain a nanofiber-doped polybenzimidazole composite membrane.

[0048] Embodiment five:

[0049] Step 1: Preparation of halogenated alkylated polybenzimidazole: 1) Take 17.5 parts of polybenzimidazole powder and 960 parts of N,N-dimethylformamide, heat and stir at 96°C for 3.6 hours to dissolve, cool to 25°C, add 3.8 parts of sodium hydride, and continue to stir and react for 36 hours. The temperature of the reaction system is lowered to 0°C, 1.15 parts of 1-bromo-4-chlorobutane are added, and the reaction is stirred for 18 hours. The reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and vacuum dried at 30°C for 24 hours to obtain halogenated alkylated polybenzimidazole.

[0050] Step 2: Preparation of amphoteric polybenzimidazole with multiple ion exchange groups: Take 17.5 parts of halogenated alkylated polybenzimidazole in step 1 and 960 parts of N,N-dimethylformamide, heat and stir at 96°C for 3.6 hours to dissolve, cool to 25°C, add 1.9 parts of tri(2-aminoethyl)amine, mix and stir for 1.25 hours, heat to 65°C, continue stirring and reacting for 35 hours, lower the temperature of the reaction system to 0°C, then add 5.5 parts of 1,3-propanesulfone dropwise, mix and stir for 1.25 hours, heat to 25°C and stir and react for 9 hours, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and dry in vacuo at 30°C for 24 hours to obtain amphoteric polybenzimidazole with multiple ion exchange groups.

[0051] Step 3: Preparation of nanofiber membrane: Take 6.5 parts of the amphoteric polybenzimidazole in step 2, 9.5 parts of perfluorosulfonic acid resin, and 83 parts of N,N-dimethylacetamide, and heat and stir at 96°C for 3.6 hours to obtain a spinning solution. Electrospin the spinning solution, and control the electrospinning conditions to 29°C, 25% humidity, 17kV voltage, 1.3ml / min injection speed, and 17cm receiving distance to obtain an electrospun nanofiber membrane. Heat treat at 170°C for 3.6 hours to obtain a nanofiber membrane.

[0052] Step 4: Preparation of nanofiber-doped polybenzimidazole composite membrane: Cut the nanofiber membrane prepared in step 3 into 2mm×2mm size. Take 7 parts of polybenzimidazole powder and 93 parts of N,N-dimethylacetamide, heat and stir at 96℃ for 3.6h to dissolve, cool to 25℃, add 4.5 parts of the cut nanofiber membrane, stir and disperse with a high-speed stirring disperser for 5min, and rotate at 5500r / min to obtain a membrane solution. Cast the membrane solution on a glass plate and heat treat at 110℃ for 3.6h to obtain a nanofiber-doped polybenzimidazole composite membrane.

[0053] Embodiment six:

[0054] Step 1: Preparation of halogenated alkylated polybenzimidazole: 1) Take 20 parts of polybenzimidazole powder and 1000 parts of N,N-dimethylacetamide, heat and stir at 100℃ for 4 hours to dissolve, cool to 25℃, add 4 parts of sodium hydride, and continue to stir and react for 40 hours. The temperature of the reaction system is lowered to 0℃, 1.25 parts of 1-bromo-3-chloropropane are added, and the reaction is stirred for 20 hours. The reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and vacuum dried at 30℃ for 24 hours to obtain halogenated alkylated polybenzimidazole.

[0055] Step 2: Preparation of amphoteric polybenzimidazole with multiple ion exchange groups: Take 20 parts of the halogenated alkylated polybenzimidazole in step 1 and 1000 parts of N,N-dimethylacetamide, heat and stir at 100°C for 4 hours to dissolve, cool to 25°C, add 2 parts of 1,4,7,10-tetraazacyclododecane, mix and stir for 1.5 hours, heat to 70°C, continue stirring and reacting for 40 hours, lower the temperature of the reaction system to 0°C, then add 6 parts of 1,4-butanesulfonic acid lactone dropwise, mix and stir for 1.5 hours, heat to 25°C and stir and react for 10 hours, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and dry in vacuo at 30°C for 24 hours to obtain amphoteric polybenzimidazole with multiple ion exchange groups.

[0056] Step 3: Preparation of nanofiber membrane: Take 7.5 parts of the amphoteric polyion exchange group polybenzimidazole in step 2, 10 parts of sulfonated polyetheretherketone, and 85 parts of dimethyl sulfoxide, and heat and stir at 100°C for 4 hours to obtain a spinning solution. Electrospin the spinning solution, and control the electrospinning conditions, temperature 30°C, humidity 30%, voltage 18kV, injection speed 1.4ml / min, receiving distance 18cm, to obtain an electrospun nanofiber membrane. Heat treat at 180°C for 4 hours to obtain a nanofiber membrane.

[0057] Step 4: Preparation of nanofiber-doped polybenzimidazole composite membrane: Cut the nanofiber membrane prepared in step 3 into 2mm×2mm size. Take 8 parts of polybenzimidazole powder and 95 parts of dimethyl sulfoxide, heat and stir at 100℃ for 4h to dissolve, cool to 25℃, add 5 parts of the cut nanofiber membrane, stir and disperse with a high-speed stirring disperser for 6min, and rotate at 6000r / min to obtain a membrane solution. Cast the membrane solution on a glass plate and heat treat at 120℃ for 4h to obtain a nanofiber-doped polybenzimidazole composite membrane.

[0058] Comparative Example 1:

[0059] Preparation of polybenzimidazole film: 5 parts of polybenzimidazole powder and 87 parts of N,N-dimethylformamide were heated and stirred at 80°C for 2 hours to dissolve to obtain a film-making solution. The film-making solution was cast on a glass plate and heat-treated at 80°C for 2 hours to obtain a polybenzimidazole film.

[0060] Comparative Example 2:

[0061] Step 1: Preparation of nanofiber membrane: Take 7.5 parts of perfluorosulfonic acid resin and 75 parts of N,N-dimethylformamide, heat and stir at 80℃ for 2h to obtain spinning solution. Electrospin the spinning solution, control the electrospinning conditions, temperature 25℃, humidity 10%, voltage 12kV, injection speed 0.8ml / min, receiving distance 12cm, and obtain electrospun nanofiber membrane. Heat treat at 140℃ for 2h to obtain nanofiber membrane.

[0062] Step 2: Preparation of nanofiber-doped polybenzimidazole composite membrane: Cut the nanofiber membrane prepared in step 1 into 2mm×2mm size. Take 3 parts of polybenzimidazole powder and 87 parts of N,N-dimethylformamide, heat and stir at 80℃ for 2h to dissolve, cool to 25℃, add 2 parts of the cut nanofiber membrane, stir and disperse with a high-speed stirring disperser for 2min at a speed of 3000r / min to obtain a membrane-making solution. Cast the membrane-making solution on a glass plate and heat-treat at 80℃ for 2h to obtain a nanofiber-doped polybenzimidazole composite membrane.

[0063] Comparative Example 3:

[0064] Step 1: Preparation of halogenated alkylated polybenzimidazole: 1) Take 5 parts of polybenzimidazole powder and 800 parts of N,N-dimethylformamide, heat and stir at 80°C for 2 hours to dissolve, cool to 25°C, add 3 parts of sodium hydride, and continue to stir and react for 20 hours. The temperature of the reaction system is lowered to 0°C, 0.85 parts of 1-bromo-4-chlorobutane is added, and the reaction is stirred for 10 hours. The reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and vacuum dried at 30°C for 24 hours to obtain halogenated alkylated polybenzimidazole.

[0065] Step 2: Preparation of amphoteric polybenzimidazole with multiple ion exchange groups: Take 5 parts of the halogenated alkylated polybenzimidazole in step 1 and 800 parts of N,N-dimethylformamide, heat and stir at 80°C for 2 hours to dissolve, cool to 25°C, add 1.5 parts of tetraethylenepentamine, mix and stir for 0.5 hours, heat to 50°C, continue stirring and reacting for 20 hours, lower the temperature of the reaction system to 0°C, then add 3 parts of 1,3-propanesulfonic acid lactone dropwise, mix and stir for 0.5 hours, heat to 25°C and stir and react for 5 hours, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and dry in vacuo at 30°C for 24 hours to obtain amphoteric polybenzimidazole with multiple ion exchange groups.

[0066] Step 3: Preparation of nanofiber membrane: Take 10 parts of the amphoteric polybenzimidazole and 75 parts of N,N-dimethylformamide in step 2, heat and stir at 80℃ for 2h to obtain a spinning solution. Electrospin the spinning solution, control the electrospinning conditions, temperature 25℃, humidity 10%, voltage 12kV, injection speed 0.8ml / min, receiving distance 12cm, and obtain an electrospun nanofiber membrane. Heat treat at 140℃ for 2h to obtain a nanofiber membrane.

[0067] Step 4: Preparation of nanofiber-doped polybenzimidazole composite membrane: Cut the nanofiber membrane prepared in step 3 into 2mm×2mm size. Take 3 parts of polybenzimidazole powder and 87 parts of N,N-dimethylformamide, heat and stir at 80℃ for 2h to dissolve, cool to 25℃, add 2 parts of the cut nanofiber membrane, stir and disperse with a high-speed stirring disperser for 2min, speed 3000r / min, and obtain the membrane solution. Cast the membrane solution on a glass plate and heat treat at 80℃ for 2h to obtain a nanofiber-doped polybenzimidazole composite membrane.

[0068] Experimental process and data:

[0069] Proton conductivity test method of ion conductive membrane: Infiltrate the inner chamber of the conductivity cell with 3.0 mol / L sulfuric acid aqueous solution. Combine the two half slots of the conductivity cell, press them tightly with an iron clamp, and use a dropper to add 3.0 mol / L sulfuric acid aqueous solution to the liquid addition hole of the conductivity cell and eliminate bubbles. Clamp the test wires of the counter electrode and reference electrode of the electrochemical workstation to the electrode at one end of the conductivity cell at the same time, and clamp the working electrode test wire to the electrode at the other end of the conductivity cell; measure the impedance of the quantity battery cell, and after the test is completed, read the resistance value in the high-frequency region that intersects with the real axis, which is the blank impedance R1 of the conductivity cell; cut a certain size (15 mm×15 mm) of the embodiment and comparative example membrane and immerse it in 3.0 mol / L sulfuric acid aqueous solution, and let it stand at room temperature for 24 hours. Clamp the pretreated membrane sample between the two half slot circular holes of the conductivity test device, and use the electrochemical workstation to test the impedance R2 of the conductivity cell of the membrane sample. Repeat the measurement 3 times, record all impedance data and calculate the average value, which is recorded as , . Membrane conductivity , where d is the average thickness of the membrane, A is the effective area of ​​the membrane, is the impedance value of the conductivity cell without membrane sample installed, is the impedance value of the conductivity cell with the membrane sample installed.

[0070] The ion exchange membranes prepared in the embodiment and the comparative example were assembled into stacks and charged and discharged under the same test conditions. Before the test, the ion exchange membranes were immersed in 3 mol / L sulfuric acid for 3 days. The charge and discharge current density was 160 mA / cm 2 , record the battery coulombic efficiency, voltage efficiency, and energy efficiency. The test results are shown in Table 1.

[0071] Table 1 Composite membrane battery efficiency and proton conductivity test results

[0072]

[0073] As can be seen from Table 1, embodiments 1 to 6 have higher battery efficiency and proton conductivity than comparative example 1. This is because the polybenzimidazole composite membrane of the present invention is prepared by composite nanofibers with amphoteric polybenzimidazole and ion conductive polymers during the preparation process, forming long-range ordered ion transmission channels inside the fibers, and constructing acid-base proton transmission channels at the interface between the sulfonic acid groups on the fiber surface and the base membrane, thereby further improving the ion conductivity of the composite membrane. Comparative example 2 is a nanofiber-doped polybenzimidazole composite membrane whose components are only perfluorosulfonic acid resin. It can be seen that the proton conductivity of the composite membrane is significantly increased compared to comparative example 1, and the corresponding composite membrane voltage efficiency and energy efficiency are also significantly increased, indicating that the polybenzimidazole composite membrane of the present invention is prepared by electrospinning nanofibers containing sulfonic acid groups to dope the base membrane during the preparation process, forming long-range ordered ion transmission channels in the thickness direction of the composite membrane, and significantly improving the ion conductivity of the membrane. Comparative Example 3 is a nanofiber-doped polybenzimidazole composite membrane whose only component is amphoteric multi-ion exchange group polybenzimidazole. It can be seen that the proton conductivity of the composite membrane is significantly increased compared with that of Comparative Example 1, and the corresponding composite membrane voltage efficiency is also significantly increased, while maintaining a relatively high Coulomb efficiency. This indicates that in the preparation process of the polybenzimidazole composite membrane of the present invention, amphoteric multi-ion exchange group polybenzimidazole is prepared by grafting modification of the spinning substrate polybenzimidazole, so that it contains multiple sulfonic acid groups and quaternary ammonium groups, which are used for electrospinning to prepare nanofibers, thereby improving the ionic conductivity of the nanofibers while maintaining a relatively high vanadium resistance, thereby also improving the ionic conductivity and vanadium resistance of the composite membrane.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a nanofiber-doped polybenzimidazole composite membrane, characterized in that: The specific steps include: Step S1, preparation of halogenated alkylated polybenzimidazole: 5-20 parts of polybenzimidazole powder and 800-1000 parts of solvent are heated and stirred to dissolve, the temperature is lowered to 25° C., 3-4 parts of sodium hydride are added for a first reaction, and when the system temperature is lowered to 0° C., 0.85-1.25 parts of halogenated hydrocarbon are added for a second reaction, the reaction product is added to an ice-water bath for precipitation, filtered, washed with ice water and isopropanol, and vacuum dried at 30° C. for 24 hours to obtain halogenated alkylated polybenzimidazole; the halogenated hydrocarbon is any one of 1-bromo-4-chlorobutane, 1-bromo-3-chloropropane, 1-bromo-3,4-dichlorobutane, and 1-bromo-3-chloro-2-propanol; Step S2, preparation of amphoteric polybenzimidazole with multiple ion exchange groups: take 5-20 parts of the halogenated alkylated polybenzimidazole and 800-1000 parts of a solvent, heat and stir to dissolve, cool to 25°C, add 1.5-2 parts of an amine compound, mix and stir evenly, heat to carry out a third reaction, lower the temperature of the reaction system to 0°C, then dropwise add 3-6 parts of a lactone compound, mix and stir evenly, heat to 25°C and stir to carry out a fourth reaction, precipitate the reaction product in deionized water, then wash with deionized water and isopropanol, and vacuum dry at 30°C for 24h to obtain amphoteric polybenzimidazole with multiple ion exchange groups; the amine compound is any one of tetraethylenepentamine, triethylenetetramine, pentaethylenehexamine, N,N,N',N'-tetrakis(3-aminopropyl)-1,4-butanediamine, tris(2-aminoethyl)amine, and 1,4,7,10-tetraazacyclododecane; Step S3, preparation of nanofiber membrane: take 2.5-7.5 parts of amphoteric polybenzimidazole with multiple ion exchange groups, 7.5-10 parts of ion conductive polymer, and 75-85 parts of solvent, heat and stir to obtain a spinning solution, electrospin the spinning solution and then perform heat treatment to obtain a nanofiber membrane; the ion conductive polymer is any one of perfluorosulfonic acid resin, sulfonated polyetheretherketone, sulfonated polyethersulfone, and sulfonated polyimide, and the solvent is any one of N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide; the heating and stirring temperature is 80-100°C, and the heating and stirring time is 2-4h; the electrospinning conditions are temperature 25-30°C, humidity 10-30%, voltage 12-18kV, injection speed 0.8-1.4ml / h, and receiving distance 12-18cm; the heat treatment temperature is 140-180°C, and the time is 2-4h; Step S4, preparation of nanofiber-doped polybenzimidazole composite membrane: take 3-8 parts of polybenzimidazole powder and 87-95 parts of solvent, heat and stir to dissolve, cool to 25°C, add 2-5 parts of nanofiber membrane, use a high-speed stirring and dispersing machine to stir and disperse to obtain a membrane-making liquid, cast the membrane-making liquid on a glass plate, and heat treat to obtain a nanofiber-doped polybenzimidazole composite membrane; the stirring and dispersing time of the high-speed stirring and dispersing machine is 2-6 minutes, and the rotation speed is 3000-6000 r / min; the heating and stirring temperature is 80-100°C, the time is 2-4 hours, and the heat treatment temperature is 80-120°C, and the time is 2-4 hours.

2. The method for preparing a nanofiber-doped polybenzimidazole composite membrane according to claim 1, characterized in that: The solvent in step S1 is any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.

3. The method for preparing a nanofiber-doped polybenzimidazole composite membrane according to claim 1, characterized in that: The heating stirring dissolution temperature in step S1 is 80-100° C., the time is 2-4 hours, the first reaction time is 20-40 hours, and the second reaction time is 10-20 hours.

4. The method for preparing a nanofiber-doped polybenzimidazole composite membrane according to claim 1, characterized in that: The solvent in step S2 is any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone, and the lactone compound is any one of 1,3-propane sultone, 1,4-butane sultone, β-propiolactone, and 1,4-butyrolactone.

5. The method for preparing a nanofiber-doped polybenzimidazole composite membrane according to claim 1, characterized in that: The heating and stirring temperature in step S2 is 80-100° C., the time is 2-4 hours, the third reaction temperature is 50-70° C., the third reaction time is 20-40 hours, and the fourth reaction time is 5-10 hours.

6. The method for preparing a nanofiber-doped polybenzimidazole composite membrane according to claim 1, characterized in that: The solvent in step S4 is any one of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

7. A nanofiber-doped polybenzimidazole composite membrane, characterized in that: The nanofiber-doped polybenzimidazole composite membrane is prepared by the method for preparing a nanofiber-doped polybenzimidazole composite membrane according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • PBI fiber membrane reinforced high-temperature-resistant composite proton exchange membrane and preparation method thereof

    CN110739476A

  • Zwitter-ion conducting membrane for flow battery and preparation method thereof