A hard rib material for plastic-reinforced composite pipe and its preparation method and use

By combining hard ribs composed of ABS matrix material and energy storage luminescent material with thermoplastic TPU material, the quality problems of existing plastic reinforced composite pipes in harsh environments are solved, the impact resistance and high temperature resistance are improved, and the All-weather visual effects and multi-scene applicability.

CN118459926BActive Publication Date: 2024-10-18ZHONG YU HOSES TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410932998.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-18
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Existing plastic reinforced composite pipes are prone to quality problems under harsh operating conditions, such as breakage and performance degradation, and have poor impact resistance and strength, especially when used at high temperatures and in the wild.

Method used

It uses a hard rib material composed of ABS matrix material and energy storage luminescent material, combined with thermoplastic TPU material, and uses specific component ratios and process preparation methods to improve the hardness, bending resistance and brightness of the ribs to achieve all-weather visibility. Effect.

Benefits of technology

It has significantly improved the impact resistance, high temperature resistance and ultraviolet resistance of plastic reinforced composite pipes, extended its service life, achieved stable operation in harsh environments and all-weather visual transportation, and is suitable for a variety of application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a hard rib material for a plastic-reinforced composite pipe and a preparation method and use thereof. The hard rib material is composed of an ABS matrix material and an energy storage luminescent material. The matrix material includes 30-40 parts of ABS resin, 10-20 parts of ASA resin, 4-6 parts of toughening agent, 3-5 parts of plastic brightener, 2-4 parts of heat-resistant stiffening agent, 0.4-0.6 parts of antioxidant, 0.5-0.8 parts of anti-ultraviolet agent and 0.5-0.9 parts of thermal stabilizer; the energy storage luminescent material includes 30-40 parts of ABS resin, 20-25 parts of long afterglow luminous powder and 5-10 parts of dispersant; the plastic brightener is composed of high polyester resin, molecular weight regulator, transparent nucleating agent, light stable diffuser and high density resin; the stiffening agent is an organic compound with a thermal decomposition temperature greater than 400°C and good compatibility with ABS and ASA resins. The hard rib is used to produce a plastic-reinforced composite pipe with an all-weather transportation visual effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite pipes, and in particular to a hard rib material for a plastic-reinforced composite pipe, and a preparation method and application thereof. Background Art

[0002] At present, the rib materials used in existing plastic-reinforced composite pipes are mostly modified PVC materials or rubber-plastic alloy materials. In order to meet the performance requirements and the extrusion requirements of the production equipment, the raw materials need to be used with a large amount of additives and produced through various processes. The process is complicated, the cost is high and the output is low. At the same time, due to the characteristics of the material, although the plastic-reinforced composite pipes produced by the existing technology also have a certain strength, they are often prone to quality problems in more severe working conditions. For example, when used as a water pipe for water diversion in wild mountainous areas, the existing plastic-reinforced composite pipes are prone to fracture and cannot be used normally when they are punctured by falling rocks or sharp objects. At the same time, when transporting media with higher temperature requirements, it is also easy to cause the performance of the material to decline, thereby seriously reducing the service life of the product.

[0003] The soft materials of existing plastic-reinforced composite pipes (spiral suction pipes) mostly adopt thermoplastic TPU elastomers with excellent comprehensive performance, suitable for extrusion, and able to bond firmly with rib materials. However, if research and design are conducted from the aspect of material properties, the existing modified PVC materials or rubber-plastic alloy materials will have reduced bonding strength with thermoplastic TPU soft materials due to modification, which will make the impact resistance and strength of the obtained plastic-reinforced composite pipes poor. Summary of the invention

[0004] The purpose of the present invention is to provide a hard rib material for plastic-reinforced composite pipes in view of the problem of poor performance of plastic-reinforced composite pipes prepared by combining modified PVC materials or rubber-plastic alloy materials with thermoplastic TPU materials in the prior art. The plastic-reinforced composite pipes prepared by combining the hard rib material with the thermoplastic TPU material can solve the problem of poor performance.

[0005] To achieve the above object, the present invention is implemented by the following technical solutions:

[0006] The present invention provides a hard rib material for a plastic-reinforced composite pipe, the hard rib material being composed of an ABS base material and an energy storage luminescent material;

[0007] Wherein, the ABS matrix material comprises the following components in parts by weight:

[0008] 30-40 parts of ABS resin, 10-20 parts of ASA resin, 4-6 parts of toughening agent, 3-5 parts of plastic brightener, 2-4 parts of heat-resistant stiffening agent, 0.4-0.6 parts of antioxidant, 0.5-0.8 parts of anti-ultraviolet agent and 0.5-0.9 parts of heat stabilizer;

[0009] The energy storage luminescent material comprises the following components in parts by weight: 30-40 parts of ABS resin, 20-25 parts of long afterglow luminous powder and 5-10 parts of dispersant;

[0010] The plastic brightener is composed of a high polyester resin as a carrier, a molecular weight regulator, a transparent nucleating agent, a light-stable diffusing agent, and a high-density resin;

[0011] The heat-resistant stiffening agent is an organic compound with a thermal decomposition temperature greater than 400° C. and good compatibility with the ABS resin and the ASA resin.

[0012] Specifically, the plastic brightener can be the OM-DA-7G-2 plastic brightener produced by Linyi Mingshuo Trading Co., Ltd.; the heat-resistant stiffening agent is used to improve the hardness and bending resistance of the rib material, and the heat-resistant stiffening masterbatch HT-200 produced by Ningbo Xinjie New Material Technology Co., Ltd. can be used.

[0013] Furthermore, a hard rib material for a plastic-reinforced composite pipe: the weight ratio of the ABS base material to the energy storage luminescent material is (8-12): (1-3).

[0014] Furthermore, a hard rib material for a plastic-reinforced composite pipe: the ABS resin contained in the ABS matrix material is selected from Chimei PA-777D high-strength and heat-resistant ABS resin, which has a melt index of 5.5g / 10min, a density of about 1.06g / cm³, a yield strength of 45.0MPa, and a heat deformation temperature of 115°C;

[0015] The ASA resin is Chimei PW-978W heat-resistant and highly weather-resistant ASA resin, which has a melt index of 9.8g / 10min, a density of about 1.07g / cm³, a yield strength of 49.0MPa, and a heat deformation temperature of 105°C;

[0016] The ABS resin contained in the energy storage luminescent material is selected from Chimei PA-737 ABS resin, which has a melt index of 2.6g / 10min and a density of about 1.04g / cm³.

[0017] Furthermore, a hard rib material for a plastic-reinforced composite pipe: the toughening agent is selected from ethyl methacrylate toughening agent, which is an ethyl methacrylate toughening agent suitable for ABS resin, and specifically, Korean SKAX8900 toughening agent can be selected.

[0018] Specifically, the resins currently used to increase the brightness of plastics or rubber mainly include polyester amide, fluorescent whitening agent and high melting point wax, which can no longer meet production needs. The plastic brightener of the present invention overcomes many shortcomings of common brighteners, such as easy generation of mist-like precipitates, spray on the surface of products, short-lasting brightness, poor temperature resistance, strong odor and not environmentally friendly, poor flow and dispersion performance, and poor light transmission performance. The plastic brightener of the present invention can achieve the original performance of the product resin without affecting or destroying it, and will quickly integrate into the product resin molecular chain after use, effectively accelerating the crystallization speed and fluidity of the product resin molecules; at the same time, the density of the resin molecular chain is increased, and a thin layer of glossy smooth film is quickly formed on the surface of the product, so that the product surface is delicate and bright to achieve an ideal bright effect, so that the product has many advantages such as long-lasting surface brightness, excellent light stability, high temperature resistance, superior dispersion performance, excellent aging resistance, excellent cold resistance, environmental protection, no pollution, and no odor.

[0019] The heat-resistant stiffening agent of the present invention can effectively increase the bending modulus, hardness thermodynamics and other mechanical properties of various plastics, and can also appropriately reduce the molding shrinkage of plastics, and increase the hardness and deformation resistance of the products thereof.

[0020] Further, a hard rib material for a plastic-reinforced composite pipe: the antioxidant is a hindered phenolic primary antioxidant having a melting temperature of about 110°C, and specifically, one or a mixture of two of BASF antioxidants 1010 and 168 can be selected;

[0021] The anti-ultraviolet agent is ultraviolet absorber UV-531;

[0022] The heat stabilizer is heat resistant agent CS-330, which is a random copolymer of styrene, aminophenylmaleimide (N-PMI) and maleic anhydride produced by continuous bulk polymerization process, with a thermal decomposition temperature of ≥350°C and a density of about 1.16 g / cm³.

[0023] Further, a hard rib material for a plastic-reinforced composite pipe: the long afterglow luminous powder is made of rare earth strontium aluminate, specifically strontium aluminate doped with europium and dysprosium with a density of 3.4g / cm³, with an excitation wavelength of 240 to 440nm, a luminescent wavelength of 520nm, and a particle size range of 75 to 95um;

[0024] The dispersant is dimethyl silicone oil, which is a colorless, odorless, non-polar liquid that is insoluble in water or short polar solvent chain alcohol. The preferred dispersant is Wacker dimethyl silicone oil AK-1000.

[0025] The present invention also provides a method for preparing a hard rib material for a plastic-reinforced composite pipe, the method comprising the following steps:

[0026] 1. Preparation of ABS matrix material:

[0027] S1, drying the ABS resin and the ASA resin contained in the ABS base material, and then uniformly mixing them with the toughening agent, the plastic brightening agent and the heat-resistant stiffening agent to obtain a mixed material A;

[0028] S2, after the antioxidant and the anti-ultraviolet agent are uniformly mixed, they are uniformly mixed with the mixed material A to obtain a mixed material B;

[0029] S3, mixing the mixed material B with the heat stabilizer, and extruding and granulating the mixture through an extruder to obtain the ABS matrix material;

[0030] Wherein: the extruder in this step is a twin-screw extruder, and the twin-screw extrusion temperature is set as follows: zone 1 temperature 190-230°C, zone 2 temperature 190-230°C, zone 3 temperature 190-230°C, zone 4 temperature 190-230°C, zone 5 temperature 190-230°C, zone 6 temperature 190-230°C, zone 7 temperature 190-230°C, zone 8 temperature 190-230°C, zone 9 temperature 190-230°C, and die head temperature 190-230°C;

[0031] 2. Preparation of energy storage luminescent materials:

[0032] S1, drying the ABS resin contained in the energy storage luminescent material, and then mixing it with 50-70% of a dispersant to obtain a mixed material C;

[0033] S2, drying the long afterglow luminous powder, and then mixing it with the mixed material C to obtain a mixed material D;

[0034] S3, mixing the mixed material D with the remaining dispersant, and extruding and granulating the mixed material through an extruder to obtain the energy storage luminescent material;

[0035] Wherein: the extruder in this step is a single screw extruder, and the single screw extrusion temperature is set as follows: the temperature of zone 1 is 170-190°C, the temperature of zone 2 is 170-190°C, the temperature of zone 3 is 170-190°C, the temperature of zone 4 is 170-190°C, and the temperature of die head is 170-190°C;

[0036] 3. Preparation of hard rib materials:

[0037] S1. After uniformly mixing the ABS matrix material and the energy storage luminescent material, the mixture is extruded and granulated to obtain a hard rib material.

[0038] The present invention also provides a use of a hard rib material for a plastic-reinforced composite pipe, wherein the hard rib material is used to produce a plastic-reinforced composite pipe with an all-weather transport visual effect.

[0039] Specifically, it means that when the medium is transported inside the plastic-reinforced composite pipe, it can be seen from the outside of the pipe, that is, after the hard rib material of the present invention is used to produce the plastic-reinforced composite pipe, the ribs in the composite pipe have the function of energy storage and luminescence, thereby achieving all-weather visibility of the transported medium and the operating appearance.

[0040] Further, a use of a hard rib material for a plastic-reinforced composite pipe: the production method of the plastic-reinforced composite pipe is:

[0041] (1) Co-extruding the hard rib material and the thermoplastic TPU elastomer soft material into a winding strip through an extruder;

[0042] (2) The extruded molten winding strips are overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe, and the plastic-reinforced composite pipe has an effect that the internal conveying medium is visible outside.

[0043] Furthermore, a use of a hard rib material for a plastic-reinforced composite pipe: the weight ratio of the hard rib material to the thermoplastic TPU elastomer soft material is (3-5):10.

[0044] The ABS matrix material used in the invention is a high-strength heat-resistant ABS material. The ABS resin is an acrylonitrile-butadiene-styrene copolymer. Its properties are controlled by the ratio of the three components and the chemical structure and physical form of each component. The properties of acrylonitrile are heat resistance, chemical resistance, rigidity, and tensile strength, the properties of butadiene are impact strength, and the properties of styrene are processing fluidity and gloss. The combination of these three components complements each other's advantages, making the ABS resin have excellent comprehensive properties, especially excellent impact resistance and high heat resistance.

[0045] However, ABS resin itself is not resistant to ultraviolet rays and decomposes quickly when exposed to light outdoors. Therefore, the present invention modifies and optimizes the ABS resin system so that the final plastic-reinforced composite pipe has excellent environmental resistance. At the same time, the plastic-reinforced composite pipe obtained by the present invention also has a luminous function, which provides more advantages than the existing technology (plastic-reinforced pipes with various other soft and hard material combinations) in practical applications, especially in outdoor use.

[0046] Beneficial effects of the present invention:

[0047] (1) Compared with the plastic-reinforced composite pipes prepared by modifying PVC materials or rubber-plastic alloy materials and thermoplastic TPU materials in the prior art, the plastic-reinforced composite pipes of the present invention have significantly improved impact resistance and high temperature resistance, so that the plastic-reinforced composite pipes of the present invention can be used in a wider range of application scenarios, making up for the gaps in the application fields of the existing plastic-reinforced composite pipes other than fire fighting, especially making up for the gaps in the use of plastic-reinforced composite pipes in more severe working conditions (such as water diversion in mountainous areas, where there are sharp objects and heavy objects touching, etc., which have higher requirements for the external rigidity strength of the product) and the use scenarios where the conveying medium is more complex (such as higher temperature requirements and other use scenarios that require temperature resistance).

[0048] (2) The rib material of the present invention has a luminous effect, and an energy-saving and environmentally friendly method is used to achieve energy storage and luminescence. The ribs are evenly spaced and spiral in the composite pipe body. The light is continuously gathered. After achieving this luminous function, the following excellent effects can be achieved: ① The existing related pipelines can observe the medium transportation through the transparent soft material in a bright environment, but the medium transportation cannot be observed in a dark environment, and the all-weather transportation visual effect cannot be achieved. The rib material provided by the present invention can emit bright yellow-green light at night, so the plastic-reinforced composite pipe produced by it can also achieve medium visualization in a dim environment; ② Based on the all-weather transportation visual effect of the plastic-reinforced composite pipe obtained by the present invention, the working condition of the pipe can be observed at any time. For example, when external conditions damage the pipe body (such as rib cracks, water leakage, etc.), it can be discovered through the night light and timely response measures can be taken, reducing the loss and timeliness caused by failure to discover in time; ③ The all-weather visual effect brought by the present invention also has other functions. For example, when running on urban roads at night, the luminous pipe body can attract the attention of pedestrians or traffic vehicles, avoiding traffic damage caused by invisible conditions.

[0049] (3) The plastic-reinforced composite pipe of the present invention is also lightweight and easy to bend. It is suitable for multiple scenarios and can glow at night. It can be used in firefighting, emergency, chemical industry, energy, mining and other fields. The plastic-reinforced composite pipe body is both rigid and flexible and has excellent comprehensive properties such as high and low temperature resistance and aging resistance.

[0050] (4) The present invention adopts a multifunctional high-strength and heat-resistant ABS matrix material as the hard material of the ribs. Compared with modified PVC materials or rubber-plastic alloy materials, the ABS matrix material has higher impact resistance. The skeleton of the plastic-reinforced composite pipe will make the composite pipe have higher strength and more significant high temperature resistance and UV resistance. When used at special temperatures, the service life is long and safer. Even if the thermoplastic TPU soft material is worn and the ribs are exposed to the outdoors, they will not decay rapidly due to oxidation decomposition. At the same time, the rib material is a polar material and can be perfectly and firmly combined with the highly polar TPU soft material without relying on adhesives. It has high strength and does not require additional adhesives.

[0051] (5) The material production process of the integral plastic-reinforced composite pipe of the present invention is more convenient and efficient, while also energy-saving and environmentally friendly, and is conducive to mass production and application. DETAILED DESCRIPTION

[0052] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0053] Example 1

[0054] Provided is a hard rib material for a plastic-reinforced composite pipe, the hard rib material being composed of an ABS base material and an energy storage luminescent material in a weight ratio of 10:2;

[0055] Wherein, the ABS matrix material comprises the following components in parts by weight:

[0056] 30 parts of Chimei PA-777D ABS resin from Taiwan, China, 12 parts of Chimei PW-978W ASA resin from Taiwan, China, 4 parts of ethyl methacrylate toughening agent (SK AX8900 toughening agent from South Korea), 3 parts of plastic brightener (OM-DA-7G-2 plastic brightener from Linyi Mingshuo Trading), 2 parts of heat-resistant stiffening agent (HT-200 heat-resistant stiffening masterbatch from Ningbo Xinjie New Material Technology Co., Ltd.), 0.4 parts of antioxidant (BASF antioxidant 1010), 0.5 parts of anti-ultraviolet agent (UV absorber UV-531), and 0.5 parts of heat stabilizer (heat-resistant agent CS-330).

[0057] The energy storage luminescent material comprises the following components in parts by weight: 30 parts of Chimei PA-737 ABS resin from Taiwan, China, 20 parts of long afterglow luminous powder (rare earth strontium aluminate) and 6 parts of dispersant (Wacker dimethyl silicone oil AK-1000).

[0058] Preparation 1: The preparation method of the hard rib material for the plastic-reinforced composite pipe of the above-mentioned embodiment 1 comprises the following specific steps:

[0059] 1. Preparation of ABS matrix material:

[0060] S1, Chi Mei PA-777D ABS resin and Chi Mei PW-978W ASA resin from Taiwan, China were placed in an oven at 80° C. and dried for 4 hours, and then uniformly mixed with ethyl methacrylate toughening agent, plastic brightener and heat-resistant stiffening agent in a high-speed mixer to obtain a mixed material A;

[0061] S2, mixing the antioxidant and the anti-ultraviolet agent uniformly at high speed in a high-speed powdering machine, and then uniformly mixing with the above-mentioned mixed material A to obtain a mixed material B;

[0062] S3, adding the above-mentioned mixed material B into the twin-screw extruder from the feed port, feeding the heat stabilizer into the twin-screw extruder through the side feed port, and performing melt shearing extrusion granulation at 190-230° C. to obtain an ABS matrix material;

[0063] Among them, the twin-screw extrusion temperature is set as follows: zone 1 temperature 190 ~ 230 ° C, zone 2 temperature 190 ~ 230 ° C, zone 3 temperature 190 ~ 230 ° C, zone 4 temperature 190 ~ 230 ° C, zone 5 temperature 190 ~ 230 ° C, zone 6 temperature 190 ~ 230 ° C, zone 7 temperature 190 ~ 230 ° C, zone 8 temperature 190 ~ 230 ° C, zone 9 temperature 190 ~ 230 ° C, die head temperature 190 ~ 230 ° C;

[0064] 2. Preparation of energy storage luminescent materials:

[0065] S1, placing Chi Mei PA-737 ABS resin from Taiwan, China in an oven at 80° C. and drying for 4 hours, and after drying, mixing at high speed with 60% of the total weight of dimethyl silicone oil dispersant to obtain a mixed material C;

[0066] S2, drying the long afterglow luminous powder (rare earth strontium aluminate) and mixing it with the above-mentioned mixed material C at a high speed to obtain a mixed material D;

[0067] S3, adding the mixed material D into the single screw extruder from the feed port, feeding 40% of the total weight of the remaining dimethyl silicone oil dispersant into the single screw extruder through the side feed port, and performing melt shear extrusion granulation at 170-190° C. to obtain an energy storage luminescent material;

[0068] Among them, the single screw extrusion temperature is set as follows: zone 1 temperature 170 ~ 190 ° C, zone 2 temperature 170 ~ 190 ° C, zone 3 temperature 170 ~ 190 ° C, zone 4 temperature 170 ~ 190 ° C, die head temperature 170 ~ 190 ° C;

[0069] 3. Preparation of hard rib materials:

[0070] S1. The ABS matrix material and the energy storage luminescent material are uniformly mixed at a weight ratio of 10:2, and then extruded and granulated to obtain a hard rib material.

[0071] Application Example 1

[0072] The hard rib material of the above-mentioned embodiment 1 is used to produce a plastic rib composite pipe with a visual effect of all-weather medium transportation, and the production method thereof is as follows:

[0073] (1) The hard rib material and the thermoplastic TPU elastomer soft material are co-extruded into a winding strip by an extruder at a weight ratio of 3:10;

[0074] (2) The extruded molten winding strips are overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe.

[0075] Example 2

[0076] Provided is a hard rib material for a plastic-reinforced composite pipe, the hard rib material being composed of an ABS base material and an energy storage luminescent material in a weight ratio of 8:1;

[0077] Wherein, the ABS matrix material comprises the following components in parts by weight:

[0078] 35 parts of Chi Mei PA-777D ABS resin from Taiwan, China, 15 parts of Chi Mei PW-978W ASA resin from Taiwan, China, 4.5 parts of ethyl methacrylate toughening agent (SK AX8900 toughening agent from South Korea), 4.0 parts of plastic brightener (OM-DA-7G-2 plastic brightener from Linyi Mingshuo Trading), 3.0 parts of heat-resistant stiffening agent (HT-200 heat-resistant stiffening masterbatch from Ningbo Xinjie New Material Technology Co., Ltd.), 0.5 parts of antioxidant (BASF antioxidant 1010), 0.6 parts of anti-ultraviolet agent (UV absorber UV-531), and 0.7 parts of heat stabilizer (heat-resistant agent CS-330).

[0079] The energy storage luminescent material comprises the following components in parts by weight: 35 parts of PA-737 ABS resin from Chimei of Taiwan, China, 22 parts of long afterglow luminous powder (using rare earth strontium aluminate) and 8 parts of dimethyl silicone oil dispersant.

[0080] Preparation 2: The preparation method of the hard rib material for the plastic-reinforced composite pipe in Example 2 is the same as that in Preparation 1.

[0081] Application Example 2

[0082] The hard rib material of the above-mentioned embodiment 2 is used to produce a plastic-rib composite pipe with a visual effect of all-weather medium transportation, and the production method thereof is as follows:

[0083] (1) The hard rib material and the thermoplastic TPU elastomer soft material are co-extruded into a winding strip by an extruder at a weight ratio of 4:10;

[0084] (2) The extruded molten winding strips are overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe.

[0085] Example 3

[0086] Provided is a hard rib material for a plastic-reinforced composite pipe, the hard rib material being composed of an ABS base material and an energy storage luminescent material in a weight ratio of 12:3;

[0087] Wherein, the ABS matrix material comprises the following components in parts by weight:

[0088] 40 parts of Chimei PA-777D ABS resin from Taiwan, China, 19 parts of Chimei PW-978W ASA resin from Taiwan, China, 6.0 parts of ethyl methacrylate toughening agent (SK AX8900 toughening agent from South Korea), 4.8 parts of plastic brightener (OM-DA-7G-2 plastic brightener from Linyi Mingshuo Trading), 3.6 parts of heat-resistant stiffening agent (HT-200 heat-resistant stiffening masterbatch from Ningbo Xinjie New Materials Technology Co., Ltd.), 0.6 parts of antioxidant (BASF antioxidant 1010), 0.8 parts of anti-ultraviolet agent (UV absorber UV-531), and 0.9 parts of heat stabilizer (heat-resistant agent CS-330).

[0089] The energy storage luminescent material comprises the following components in parts by weight: 40 parts of Chi Mei PA-737 ABS resin from Taiwan, China, 25 parts of long afterglow luminous powder (rare earth strontium aluminate) and 9 parts of dimethyl silicone oil dispersant.

[0090] Preparation 3: The preparation method of the hard rib material for the plastic-reinforced composite pipe in Example 3 is the same as that in Preparation 1.

[0091] Application Example 3

[0092] The hard rib material of the above-mentioned embodiment 3 is used to produce a plastic rib composite pipe with an all-weather medium transport visual effect, and the production method thereof is as follows:

[0093] (1) The hard rib material and the thermoplastic TPU elastomer soft material are co-extruded into a winding strip by an extruder at a weight ratio of 5:10;

[0094] (2) The extruded molten winding strips are overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe.

[0095] Comparative Example 1

[0096] A method for producing an existing plastic-reinforced composite pipe is provided, comprising the following steps:

[0097] (1) Using modified PVC material (Sinopec S-1000 PVC) as the rib material, and then co-extrude the modified PVC material and thermoplastic TPU elastomer soft material (Merui New Materials Polyether 85A thermoplastic TPU) into a winding strip through an extruder at a weight ratio of 3:10;

[0098] (2) The extruded molten winding strips are overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe.

[0099] Comparative Example 2

[0100] Another existing method for producing a plastic reinforced composite pipe is provided, comprising the following steps:

[0101] (1) The rubber-plastic alloy material is used as the rib material, and then the rubber-plastic alloy material and the thermoplastic TPU elastomer soft material (using Meirui New Material Polyether 85A thermoplastic TPU) are co-extruded into a winding strip through an extruder according to the weight ratio of 3:10;

[0102] The rubber-plastic alloy material is obtained by mixing 30 parts by weight of NBR (using powdered nitrile SCP-830H) and 50 parts by weight of PVC (using S-1000 PVC from Sinopec) at 90°C, mixing and powdering at high speed, drying, cooling, and then granulating with a twin-screw extruder. The extrusion temperature range is 150-165°C.

[0103] (2) The extruded molten winding strips are overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe.

[0104] The difference between the above-mentioned Comparative Examples 1 and 2 and Application Example 1 is that the selection of rib materials is different. Comparative Examples 1 and 2 respectively use existing modified PVC materials and rubber-plastic alloy materials as the rib materials of the composite pipe, while Application Example 1 uses the specially prepared hard rib material of the present invention as the skeleton of the plastic-reinforced composite pipe, which has higher strength.

[0105] Comparative Example 3

[0106] A method for producing a plastic-reinforced composite pipe is provided, comprising the following steps:

[0107] (1) The hard rib material A and the thermoplastic TPU elastomer soft material are co-extruded into a winding strip A by an extruder at a weight ratio of 3:10;

[0108] The difference between the hard rib material A and the hard rib material in Example 1 is that the plastic brightener selected in the component of the hard rib material A is different from the plastic brightener selected in Example 1, and the plastic brightener in the component of the hard rib material A is a common plastic brightener (specifically, Chi Mei PA-756 from Taiwan, China).

[0109] (2) The extruded molten winding strip A is overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe.

[0110] Therefore, the difference between the plastic-reinforced composite pipe produced in the comparative example 3 and the plastic-reinforced composite pipe produced in the application example 1 is that the plastic brighteners used in the two are different, and the rest are the same.

[0111] Comparative Example 4

[0112] A method for producing a plastic-reinforced composite pipe is provided, comprising the following steps:

[0113] (1) The hard rib material B and the thermoplastic TPU elastomer soft material are co-extruded into a winding strip B by an extruder at a weight ratio of 3:10;

[0114] Among them, the difference between the hard rib material B and the hard rib material in Example 1 is that the stiffener selected in the component of the hard rib material B is different from the heat-resistant stiffener selected in Example 1, and the stiffener in the component of the hard rib material B is a common stiffener (specifically, MBS Japan Zhongyuan PA-20 is selected);

[0115] (2) The extruded molten winding strip B is overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe.

[0116] Therefore, the difference between the plastic-reinforced composite pipe produced in the comparative example 4 and the plastic-reinforced composite pipe produced in the application example 1 is that the stiffening agents used in the two are different, and the rest are the same.

[0117] test:

[0118] The plastic reinforced composite pipes obtained in the above application example 1 and comparative examples 1 to 4 were subjected to various performance tests, and the test results are shown in the following table:

[0119]

[0120] Note: The original test condition of "High Temperature Negative Pressure A" is to test in 55℃ hot water. The qualified judgment standard of High Temperature Negative Pressure A is: the plastic reinforced composite pipe does not have suction, shrinkage or cracking phenomenon, and the unqualified judgment standard is: the plastic reinforced composite pipe has suction, shrinkage or cracking phenomenon;

[0121] The original test condition of "High Temperature Negative Pressure B" is to test in 55℃ hot water. The qualified judgment standard of High Temperature Negative Pressure B is: the plastic reinforced composite pipe does not have suction and crack damage, and the unqualified judgment standard is: the plastic reinforced composite pipe has suction and crack damage;

[0122] The qualified judgment standard of "normal temperature negative pressure" is: the plastic reinforced composite pipe has no suction, shrinkage or cracking phenomenon; the unqualified judgment standard is: the plastic reinforced composite pipe has suction, shrinkage or cracking phenomenon;

[0123] The qualified judgment standard of "low temperature performance" is: after a 15 cm short sample of plastic reinforced composite pipe is kept in a -45℃ constant temperature box for 24 hours, it is dropped vertically from a vertical height of 1.5m three times without any cracking; the unqualified judgment standard is: after a 15 cm short sample of plastic reinforced composite pipe is kept in a -45℃ constant temperature box for 24 hours, it is dropped vertically from a vertical height of 1.5m three times and cracking occurs;

[0124] The qualified judgment standard of "bursting pressure" is: the positive pressure bursting pressure of plastic reinforced composite pipe is greater than 9kg, and the unqualified judgment standard is: the positive pressure bursting pressure of plastic reinforced composite pipe is less than 9kg;

[0125] The criteria for judging the “luminous effect” are: comparing the brightness effect with the naked eye;

[0126] The qualified judgment standard of "aging resistance" is: the "normal temperature and negative pressure" test is qualified after the aging condition is completed, and the unqualified judgment standard is: the "normal temperature and negative pressure" test is unqualified after the aging condition is completed;

[0127] "Heat deformation temperature" is measured data. The higher the value, the better the performance.

[0128] "Bending modulus" is measured data. The higher the value, the better the performance. A value greater than 1900 MPa is considered qualified, and a value less than 1900 MPa is considered unqualified.

[0129] It can be seen from the test results in the above table that the plastic-reinforced composite pipe obtained by the present invention has excellent performances in all aspects.

[0130] The special hard rib material prepared by the present invention can enable the prepared plastic-reinforced composite pipe to have the function of energy storage and luminescence. Compared with the existing plastic-reinforced composite pipes (Comparative Examples 1 to 2), it provides more help and benefits for product application in actual use, can prolong the visible time of the conveying medium, can observe the real-time deformation appearance of the pipe body through the luminous pipe body, and because the pipe body is luminous, it can be discovered and avoided in time by pedestrians and vehicles on urban roads at night, etc.

[0131] It can be seen from the test results of Application Example 1 and Comparative Example 3 in the "Low Temperature Performance" column in the above table that the low temperature performance test result of the plastic-reinforced composite pipe obtained in Application Example 1 is qualified, while the low temperature performance test result of the plastic-reinforced composite pipe obtained in Comparative Example 3 using an ordinary plastic brightener is unqualified, which shows that the present invention can make the product have excellent cold resistance through the preferred plastic brightener.

[0132] From the test results of Application Example 1 and Comparative Example 3 in the "Luminous Effect" column in the above table, it can be seen that the luminous effect of the plastic-reinforced composite pipe obtained in Application Example 1 is bright, while the luminous effect of the plastic-reinforced composite pipe obtained in Comparative Example 3 using an ordinary plastic brightener is slightly bright, which shows that the preferred plastic brightener of the present invention can make the surface of the product have an excellent brightening effect. The present invention achieves the effect of significantly improving the luminous brightness of the rib material under the condition of the same light source energy storage through the preferred plastic brightener, so that the transportation visibility is enhanced.

[0133] It can be seen from the test results of Application Example 1 and Comparative Example 3 in the "Aging Resistance" column in the above table that the aging resistance test result of the plastic-reinforced composite pipe obtained in Application Example 1 is qualified, while the aging resistance test result of the plastic-reinforced composite pipe obtained in Comparative Example 3 using an ordinary plastic brightener is unqualified, which shows that the present invention can make the product have excellent aging resistance through the preferred plastic brightener.

[0134] From the test results of Application Example 1 and Comparative Example 3 in the "Heat Deformation Temperature" column in the above table, it can be seen that the heat deformation temperature of the plastic-reinforced composite pipe obtained in Application Example 1 is about 105°C, while the heat deformation temperature of the plastic-reinforced composite pipe obtained in Comparative Example 3 after using an ordinary plastic brightener is about 63°C, which shows that the present invention can make the product have better high temperature resistance through the preferred plastic brightener.

[0135] It can be seen from the test results of Application Example 1 and Comparative Example 4 in the "High Temperature Negative Pressure B" column in the above table that the high temperature negative pressure B test result of the plastic-reinforced composite pipe obtained in Application Example 1 is qualified, while the high temperature negative pressure B test result of the plastic-reinforced composite pipe obtained in Comparative Example 4 using an ordinary stiffener is unqualified, which shows that the present invention can make the product have better mechanical properties through the preferred heat-resistant stiffener.

[0136] It can be seen from the test results of Application Example 1 and Comparative Example 4 in the "Burst Pressure" column in the above table that the burst pressure test result of the plastic-reinforced composite pipe obtained in Application Example 1 is qualified, while the burst pressure test result of the plastic-reinforced composite pipe obtained in Comparative Example 4 using an ordinary stiffener is unqualified, which shows that the present invention can make the product have better mechanical properties through the preferred heat-resistant stiffener.

[0137] From the test results of Application Example 1 and Comparative Example 4 in the "Flexural Modulus" column in the above table, it can be seen that the flexural modulus test result of the plastic-reinforced composite pipe obtained in Application Example 1 is about 2850MPa, while the flexural modulus test result of the plastic-reinforced composite pipe obtained in Comparative Example 4 using an ordinary stiffener is only about 1920MPa, which shows that the present invention can effectively increase the flexural modulus of the material, increase the hardness and deformation resistance of the product through the preferred heat-resistant stiffener. The present invention achieves a significant improvement in the flexural modulus of the rib material through the preferred heat-resistant stiffener, and can maintain the rigidity of the structure unchanged at higher temperatures.

[0138] The plastic-reinforced composite pipe prepared by the present invention has high impact resistance, and the rib skeleton has high strength; the plastic-reinforced composite pipe of the present invention has more significant high temperature resistance and UV resistance. When used at special temperatures, the rib performance is stable, and the product structure strength attenuation rate is greatly reduced. At the same time, even if the TPU soft material is worn and part of the ribs are exposed outdoors, the high weather resistance of the rib material of the present invention will not cause rapid attenuation due to oxidative decomposition problems. At the same time, the rib material of the present invention is a polar material, and can be perfectly and firmly combined with the highly polar TPU soft material without relying on adhesives.

[0139] Related explanation:

[0140] Plastic reinforced composite pipe: The composite pipe referred to here is a plastic reinforced water suction pipe, also known as a spiral water suction pipe or a fire water suction hose. The structure is composed of a soft elastomer wrapped with ribs with certain strength and physical and chemical properties.

[0141] Transport visibility: refers to the fact that after the rib material of the present invention is applied as the rib material of the composite pipe, the ribs of the pipe body have the function of storing energy and emitting light, thereby realizing the all-weather visibility of the transport medium and the operating appearance.

[0142] The above are preferred embodiments of the present invention and are only used to explain the present invention, not to limit the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A hard rib material for plastic reinforced composite pipes, It is characterized in that The hard rib material is composed of an ABS matrix material and an energy storage luminescent material, and the weight ratio of the ABS matrix material to the energy storage luminescent material is (8-12): (1-3); Wherein, the ABS matrix material comprises the following components in parts by weight: 30-40 parts of ABS resin, 10-20 parts of ASA resin, 4-6 parts of toughening agent, 3-5 parts of plastic brightener, 2-4 parts of heat-resistant stiffening agent, 0.4-0.6 parts of antioxidant, 0.5-0.8 parts of anti-ultraviolet agent and 0.5-0.9 parts of heat stabilizer; The energy storage luminescent material comprises the following components in parts by weight: 30-40 parts of ABS resin, 20-25 parts of long afterglow luminous powder and 5-10 parts of dispersant; Wherein, the plastic brightener adopts Linyi Mingshuo Trading OM-DA-7G-2 plastic brightener; The heat-resistant stiffening agent is HT-200 heat-resistant stiffening masterbatch produced by Ningbo Xinjie New Material Technology Co., Ltd.

2. The hard rib material for plastic-reinforced composite pipe according to claim 1, It is characterized in that The ABS resin contained in the ABS matrix material is selected from Chimei PA-777D high-strength and heat-resistant ABS resin; the ASA resin is selected from Chimei PW-978W heat-resistant and highly weather-resistant ASA resin; the ABS resin contained in the energy storage luminescent material is selected from Chimei PA-737 ABS resin.

3. The hard rib material for plastic-reinforced composite pipe according to claim 1, It is characterized in that The toughening agent is ethyl methacrylate toughening aid.

4. The hard rib material for plastic-reinforced composite pipe according to claim 1, It is characterized in that The antioxidant is a hindered phenolic main antioxidant; the anti-ultraviolet agent is an ultraviolet absorber UV-531; and the heat stabilizer is a heat stabilizer CS-330.

5. The hard rib material for plastic-reinforced composite pipe according to claim 1, It is characterized in that The long afterglow luminous powder is made of rare earth strontium aluminate; and the dispersant is made of dimethyl silicone oil.

6. A method for preparing a hard rib material for a plastic-reinforced composite pipe according to any one of claims 1 to 5, It is characterized in that The method comprises the following steps:

1. Preparation of ABS matrix material: S1, drying the ABS resin and the ASA resin contained in the ABS base material, and then uniformly mixing them with the toughening agent, the plastic brightening agent and the heat-resistant stiffening agent to obtain a mixed material A; S2, after the antioxidant and the anti-ultraviolet agent are uniformly mixed, they are uniformly mixed with the mixed material A to obtain a mixed material B; S3, mixing the mixed material B with the heat stabilizer, and extruding and granulating the mixture through an extruder to obtain the ABS matrix material; 2. Preparation of energy storage luminescent materials: S1, drying the ABS resin contained in the energy storage luminescent material, and then mixing it with 50-70% of a dispersant to obtain a mixed material C; S2, drying the long afterglow luminous powder, and then mixing it with the mixed material C to obtain a mixed material D; S3, mixing the mixed material D with the remaining dispersant, and extruding and granulating the mixed material through an extruder to obtain the energy storage luminescent material; 3. Preparation of hard rib materials: S1. After mixing the ABS matrix material and the energy storage luminescent material, the mixture is extruded and granulated to obtain a hard rib material.

7. Use of a hard rib material for a plastic-reinforced composite pipe, It is characterized in that The hard rib material described in any one of claims 1 to 5 is used to produce a plastic-reinforced composite pipe with an all-weather transportation visual effect.

8. Use of the hard rib material for plastic-reinforced composite pipe according to claim 7, It is characterized in that The production method of the plastic reinforced composite pipe is: (1) co-extruding the hard rib material and the thermoplastic TPU elastomer soft material into a winding strip through an extruder; (2) The extruded molten winding strips are overlapped and wound by a spiral winding unit, cooled and shaped, thereby preparing a plastic-reinforced composite pipe.

9. Use of the hard rib material for plastic-reinforced composite pipe according to claim 8, It is characterized in that The weight ratio of the hard rib material to the thermoplastic TPU elastomer soft material is (3-5):10.

Citation Information

Patent Citations

  • ABS (acrylonitrile butadiene styrene) alloy for multi-rib highly-smooth base and preparation method thereof

    CN102382413A

  • Process for the adhesive bonding of plastics pipes by means of (meth)acrylate adhesive

    CN103974816A