A pulping process using plant fiber raw materials

Through the comprehensive process of organic acid compound solution soaking, enzymatic hydrolysis and mechanical grinding, the problems of environmental pollution and low non-wood fiber pulping efficiency of traditional papermaking processes are solved, the extraction efficiency of cellulose and paper quality are improved, and the paper quality is significantly improved. physical properties and reduced contamination.

CN118461348BActive Publication Date: 2024-10-15LINYI LINXING WOOD IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410925036.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-15
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The traditional papermaking process causes serious environmental pollution, especially the chemical pulping method that pollutes water bodies. The pulping efficiency of non-wood fiber is low, and the quality of the pulp is difficult to reach the level of wood pulp.

Method used

Processes such as soaking in organic acids and other composite solutions, enzymatic hydrolysis, and mechanical grinding are used, combined with chemical, biological, and mechanical treatments to improve cellulose extraction efficiency and paper quality.

Benefits of technology

It significantly improves the extraction efficiency of cellulose and the whiteness, folding resistance, tensile index and tear index of paper, reduces the use of harmful chemicals and pollutant emissions, and reduces environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of cellulose preparation, and specifically relates to a pulping process using plant fiber raw materials. The pulping process using plant fiber raw materials comprises the following steps: S1, removing impurities from the raw materials, cutting them, adding a composite solution to soak them, and obtaining a pretreated raw material; S2, adjusting the pH in the pretreated raw material, and then adding a composite enzyme preparation for enzymolysis to obtain an enzymolysis solution; S3, filtering the enzymolysis solution, washing it, adding water and an auxiliary agent, stirring it evenly, and then mechanically grinding it, screening it, and washing it to obtain fiber pulp. The pulping process provided by the present invention effectively improves the extraction efficiency of cellulose, ensures the integrity and strength of the fibers, improves the bonding between the fibers, and the paper products made from the obtained fiber pulp have a high whiteness, and its physical properties such as smoothness, folding endurance, tensile index, and tear index are significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cellulose preparation, and in particular relates to a pulping process using plant fiber raw materials. Background Art

[0002] The papermaking industry is one of the world's important manufacturing industries, but it is also a resource-intensive industry and a potential source of environmental pollution. The traditional pulping process mainly relies on wood as raw material, and converts wood raw materials into fiber pulp that can be used for papermaking through chemical or mechanical means. However, with the acceleration of industrialization, the impact of traditional papermaking technology on the environment has become increasingly prominent, especially the over-exploitation of natural resources and pollution of the ecological environment, which has become the focus of global attention.

[0003] Limitations of traditional pulping technology The core of traditional papermaking technology is to convert plant fibers into usable pulp. Among them, chemical pulping is one of the most mainstream methods, especially the Kraft process. The Kraft process can effectively decompose lignin and separate cellulose, thereby obtaining pulp with high purity and good strength. However, this process requires a large amount of chemicals, such as caustic soda (NaOH), sodium sulfide (Na2S), etc. The black liquor produced contains complex organic matter and heavy metals. If it is discharged into the environment without proper treatment, it will cause serious pollution to the water body and destroy the ecological balance. On the other hand, although the mechanical pulping method can avoid the large-scale use of chemicals, since it only relies on physical means to break the fibers, the purity and strength of the resulting pulp are low, which limits its scope of application.

[0004] In addition, with the reduction of forest resources, it is becoming more urgent to find alternative sources of fiber. Non-wood fibers, such as rice straw, wheat straw, bagasse, bamboo, etc., are considered to be very promising pulping raw materials because of their wide sources and strong renewability. The use of such raw materials can not only reduce the pressure on forest resources, but also effectively recycle agricultural and urban waste to achieve resource recycling.

[0005] However, pulping non-wood fibers is not an easy task. Compared with wood, non-wood fibers have a complex and variable structure, with large differences in fiber length and strength, and often contain more impurities. This results in low fiber dissociation efficiency and high energy consumption during the pulping process, and it is difficult for the pulp quality to reach the same level as wood pulp. At the same time, the pigments and impurities naturally present in non-wood fibers are not easy to remove during the pulping process, which affects the whiteness and stability of the pulp and increases the difficulty and cost of subsequent bleaching treatments.

[0006] Therefore, it is necessary to provide a pulping process using non-wood plant fiber raw materials, which can reduce the impact on the environment, improve the fiber utilization rate, and ensure the quality of the pulp product. Summary of the invention

[0007] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a pulping process using plant fiber raw materials. The pulping process using plant fiber raw materials provided by the present invention uses non-wood plants as raw materials, adopts processes such as soaking in composite solutions of organic acids, enzymatic hydrolysis, and mechanical grinding, and comprehensively coordinates chemical, biological and mechanical treatment methods, effectively improves the extraction efficiency of cellulose, improves the bonding between fibers, and comprehensively improves the quality of the produced paper.

[0008] The technical solution of the present invention is:

[0009] A pulping process using plant fiber raw materials, the specific steps are as follows:

[0010] S1. Select non-wood plant fiber raw materials, remove impurities, cut them, and soak them in a composite solution to obtain pretreated raw materials; the non-wood plant fiber raw materials are selected from one of wheat straw, corn straw, and reed; the composite solution is composed of organic acid, cocamidopropyl betaine and water in a weight ratio of (5-10:0.8-1.2:100); the CAS number of cocamidopropyl betaine is 86438-79-1;

[0011] S2, adjusting the pH of the pretreated raw material obtained in step S1, and then adding the composite enzyme preparation for enzymolysis to obtain an enzymolysis solution;

[0012] S3, filtering the enzymatic hydrolyzate obtained in step S2, washing, then adding water and additives to the obtained solid matter, stirring evenly, performing mechanical grinding treatment, and then screening and washing to obtain fiber pulp.

[0013] Furthermore, the composite solution in step S1 is composed of an organic acid, cocamidopropyl betaine and water in a weight ratio of (8:1:100); the organic acid is one or a combination of two of acetic acid, citric acid, oxalic acid and tartaric acid.

[0014] Furthermore, the organic acid is composed of acetic acid and citric acid in a weight ratio of (1:2).

[0015] Furthermore, the amount of the composite solution added in step S1 is 6 to 10 times the weight of the non-wood plant fiber raw material in step S1.

[0016] Furthermore, the soaking temperature in step S1 is 40-50° C., and the soaking time is 3-5 h.

[0017] Furthermore, the composite enzyme preparation in step S2 is a combination of cellulase and lignin peroxidase;

[0018] The cellulase and lignin peroxidase used in the present invention are commonly used biological enzyme preparations in the prior art. The CAS number of the cellulase is 9012-54-8, and the CAS number of the lignin peroxidase is 42613-30-9.

[0019] Furthermore, the amount of cellulase added in step S2 is 20-40 IU / g, preferably 30 IU / g, and the amount of lignin peroxidase added is 20-30 IU / g, preferably 25 IU / g, based on the dry weight of the non-wood plant fiber raw material in step S1.

[0020] Furthermore, in step S2, the pH is adjusted to 4.0-5.5, and then the complex enzyme preparation is added and the mixture is placed in a water bath at a temperature of 30-45° C. for 10-12 h.

[0021] Furthermore, the amount of water added in step S3 is 2 to 3 times the amount of the solid matter after filtration and washing, and the amount of the auxiliary agent added is 13 to 16% of the total weight of the solid matter and water, preferably 15%.

[0022] Furthermore, the auxiliary agent is composed of an ionic liquid and lauryl amide propyl amine oxide in a weight ratio of (10~15:1.5~3); preferably (13:2.5); the CAS number of the lauryl amide propyl amine oxide is 69898-00-6; the ionic liquid is one of 1-butyl-3-methylimidazolium acetate and 1-ethyl-3-methylimidazolium trifluoromethanesulfonate.

[0023] Furthermore, the CAS number of the 1-butyl-3-methylimidazolium acetate is 284049-75-8; the CAS number of the 1-ethyl-3-methylimidazolium trifluoromethanesulfonate is 145022-44-2.

[0024] Furthermore, the grinding gap of the mechanical grinding process in step S3 is controlled to be 0.1 mm to 0.3 mm, and the grinding speed is 1000 rpm to 3000 rpm.

[0025] Furthermore, after the mechanical grinding treatment in step S3, two screenings are performed, with the screening mesh numbers being 80 mesh and 120 mesh respectively, followed by three washings, with the water temperature being controlled at 30-40° C., and after the washing, a fiber pulp with a pulp concentration of 10-15% is obtained.

[0026] The invention provides a pulping process using plant fiber raw materials. First, non-wood plant raw materials such as straws, reeds, etc. are preliminarily screened and impurities are removed, and then soaked in a composite solution consisting of organic acid, cocamidopropyl betaine and water, which can effectively promote the composite solution to penetrate deeper into the raw materials, soften the non-wood plant fiber raw materials, preliminarily dissolve lignin and hemicellulose, destroy chemical bonds between fibers, and effectively prevent fiber agglomeration, thereby improving subsequent enzymatic hydrolysis efficiency.

[0027] Furthermore, by using specific bio-enzyme preparations to enzymolyze the above-mentioned pretreated raw materials and precisely controlling the conditions such as time, temperature, pH, etc. during the enzymolysis process, cellulose and hemicellulose can be further decomposed under milder conditions, effectively improving the cellulose extraction rate, while also effectively maintaining the length and strength of the fibers, which can reduce the energy consumption of subsequent mechanical processing.

[0028] Next, water and an auxiliary agent consisting of an ionic liquid and lauryl amide propyl amine oxide are added to the solid matter obtained after filtering the above-mentioned enzymatic hydrolyzate, and then mechanical grinding is carried out. The added auxiliary agent at a specific content can dissolve the residual lignin and hemicellulose, making the cellulose fibers easier to separate. At the same time, the applicant found in the study that when a certain amount of lauryl amide propyl amine oxide is added to the auxiliary agent, it can synergize with the ionic liquid, which can not only effectively improve the dispersion of the fibers in the grinding slurry, reduce the friction between the fibers, and reduce the energy consumption during mechanical grinding; it can also effectively reduce the damage to the fibers, maintain the integrity and strength of the fibers, and help improve the physical properties of the prepared paper, such as tear strength, tensile strength and folding endurance.

[0029] At the same time, the method of adding ionic liquid and lauryl amide propyl amine oxide and then performing mechanical grinding can reduce the use of chemical reagents, reduce the emission of pollutants, and help reduce the impact on the environment. At the same time, the added ionic liquid can be recovered and recycled by conventional distillation, effectively reducing production costs.

[0030] Compared with the prior art, the pulping process using plant fiber raw materials provided by the present invention has the following advantages:

[0031] The present invention adopts a specific method to provide a pulping process using plant fiber raw materials. Non-wood plants are used as raw materials, and processes such as soaking in composite solutions such as organic acids, enzymatic hydrolysis, and mechanical grinding are adopted. Chemical, biological and mechanical treatment methods are comprehensively coordinated to effectively improve the extraction efficiency of cellulose, improve the bonding between fibers, and improve the quality of the produced paper. Experimental verification shows that the paper products made from the fiber pulp prepared by the treatment method provided by the present invention have high whiteness, and their physical properties such as smoothness, folding resistance, tensile index, and tear index are significantly improved. At the same time, in the entire pulping process provided by the present invention, the use of harmful chemicals is reduced, so that emissions are effectively controlled and the impact on the environment is reduced. DETAILED DESCRIPTION

[0032] The present invention is further illustrated below through the description of specific implementation methods, but this is not a limitation of the present invention. Those skilled in the art can make various modifications or improvements based on the basic idea of ​​the present invention, but as long as they do not deviate from the basic idea of ​​the present invention, they are all within the protection scope of the present invention.

[0033] In the following examples and comparative examples, reagents not otherwise specified are conventional reagents and can be purchased from conventional reagent production and sales companies. The methods used are all prior art unless otherwise specified.

[0034] Embodiment 1:

[0035] A pulping process using plant fiber raw materials comprises the following steps:

[0036] S1. After removing impurities from wheat straw, cut it into small segments of 2 cm, add a composite solution 6 times its mass (the composite solution consists of acetic acid, cocamidopropyl betaine and water in a weight ratio of (5:0.8:100)) and soak for 3 h. The soaking temperature is controlled at 50° C. to obtain a pretreated raw material;

[0037] S2, adjusting the pH of the pretreated raw material obtained in step S1 to 4.0, then adding a composite enzyme preparation and water bathing at a temperature of 30°C for 10 hours to obtain an enzymatic solution; the composite enzyme preparation is cellulase and lignin peroxidase, the addition amount of the cellulase is 20 IU / g, and the addition amount of the lignin peroxidase is 30 IU / g, based on the dry weight of the non-wood plant fiber raw material in step S1;

[0038] S3. Filter the enzymatic hydrolyzate obtained in step S2, wash it, then add water twice the mass of the solid substance to the obtained solid substance, and then add an auxiliary agent (the auxiliary agent consists of 1-butyl-3-methylimidazole acetate and lauryl amide propyl amine oxide in a weight ratio of (10:3)) in an amount of 13% of the total weight of the solid substance and water, stir evenly and then perform mechanical grinding. The grinding gap of the mechanical grinding treatment is controlled at 0.1 mm~0.3 mm, and the grinding speed is 1000 rpm. Then, screen it twice, and the number of screening meshes is 80 mesh and 120 mesh respectively. Then wash it three times. The water temperature is controlled at 30°C during the washing process. After washing, a fiber pulp with a pulp concentration of 10% is obtained.

[0039] Embodiment 2:

[0040] A pulping process using plant fiber raw materials comprises the following steps:

[0041] S1. After removing impurities from wheat straw, cut it into small segments of 3 cm, add a composite solution 8 times its weight (the composite solution consists of organic acid, cocamidopropyl betaine and water in a weight ratio of (8:1:100), and the organic acid consists of acetic acid and citric acid in a weight ratio of (1:2)) and soak for 4 h. The soaking temperature is controlled at 45°C to obtain a pretreated raw material;

[0042] S2, adjusting the pH of the pretreated raw material obtained in step S1 to 5.0, then adding a composite enzyme preparation and water bathing at a temperature of 40°C for 12 hours to obtain an enzymatic solution; the composite enzyme preparation is cellulase and lignin peroxidase, the addition amount of the cellulase is 30 IU / g, and the addition amount of the lignin peroxidase is 25 IU / g, based on the dry weight of the non-wood plant fiber raw material in step S1;

[0043] S3. Filter the enzymatic hydrolyzate obtained in step S2, wash it, then add water 2 to 3 times the weight of the solid substance obtained, and then add an auxiliary agent (the auxiliary agent consists of 1-ethyl-3-methylimidazole trifluoromethanesulfonate and lauramide propylamine oxide in a weight ratio of (13:2.5)) in an amount of 15% of the total weight of the solid substance and water), stir evenly and then perform mechanical grinding treatment, the grinding gap of the mechanical grinding treatment is controlled at 0.1 mm to 0.3 mm, the grinding speed is 2000 rpm, and then screen twice, the screening mesh numbers are 80 mesh and 120 mesh respectively, followed by washing three times, the water temperature is controlled at 35°C during the washing process, and after washing, a fiber pulp with a pulp concentration of 12% is obtained.

[0044] Embodiment 3:

[0045] A pulping process using plant fiber raw materials comprises the following steps:

[0046] S1. After removing impurities from wheat straw, cut it into small segments of 3 cm, add a composite solution 10 times its mass (the composite solution consists of tartaric acid, cocamidopropyl betaine and water in a weight ratio of (10:1.2:100)) and soak for 5 h. The soaking temperature is controlled at 40°C to obtain a pretreated raw material;

[0047] S2, adjusting the pH of the pretreated raw material obtained in step S1 to 5.5, then adding a composite enzyme preparation and water bathing at a temperature of 45°C for 12 hours to obtain an enzymatic solution; the composite enzyme preparation is cellulase and lignin peroxidase, the addition amount of the cellulase is 40 IU / g, and the addition amount of the lignin peroxidase is 20 IU / g, based on the dry weight of the non-wood plant fiber raw material in step S1;

[0048] S3. Filter the enzymatic hydrolyzate obtained in step S2, wash it, then add water 3 times its mass to the obtained solid substance, and then add an auxiliary agent (the auxiliary agent is composed of 1-ethyl-3-methylimidazole trifluoromethanesulfonate and lauramide propylamine oxide in a weight ratio of (15:1.5)) in an amount of 16% of the total weight of the solid substance and water), stir evenly and then perform mechanical grinding treatment, the grinding gap of the mechanical grinding treatment is controlled at 0.1 mm~0.3 mm, the grinding speed is 3000 rpm, and then screen twice, the screening mesh numbers are 80 mesh and 120 mesh respectively, followed by washing three times, the water temperature is controlled at 40°C during the washing process, and after washing, a fiber pulp with a pulp concentration of 15% is obtained.

[0049] Comparative Example 1:

[0050] The difference from Example 2 is that no cocamidopropylamine oxide is added to the composite solution of step S1, and the amount of organic acid is increased accordingly, that is, the composite solution is composed of organic acid and water in a weight ratio of (9:100), and the organic acid is composed of acetic acid and citric acid in a weight ratio of (1:2). Other raw materials and preparation steps are the same as those in Example 2.

[0051] Comparative Example 2:

[0052] The difference from Example 2 is that the composite enzyme preparation in step S2 is composed of cellulase, hemicellulase (CAS No.: 9025-56-3) and pectinase (CAS No.: 9032-75-1), the addition amount of the cellulase is 30 IU / g, the addition amount of the hemicellulase is 15 IU / g, and the addition amount of the pectinase is 10 IU / g, based on the dry weight of the non-wood plant fiber raw material in step S1. Other raw materials and preparation steps are the same as in Example 2.

[0053] Comparative Example 3:

[0054] The difference from Example 2 is that the lauryl amide propylamine oxide in the auxiliary agent of step S3 is replaced by sodium dodecyl sulfate (CAS No. 151-21-3), that is, the auxiliary agent is composed of 1-ethyl-3-methylimidazolium trifluoromethanesulfonate and sodium dodecyl sulfate in a weight ratio of (13:2.5). Other raw materials and preparation steps are the same as those in Example 2.

[0055] Comparative Example 4:

[0056] The difference from Example 2 is that the amount of the additive added in step S3 is 20% of the total weight of the solid matter and water, and the other raw materials and preparation steps are the same as those in Example 2.

[0057] Test Example 1: Performance test of paper products made from the fiber pulp prepared by the present invention:

[0058] Test method:

[0059] The fiber pulp prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 4 was diluted to a pulp concentration of 1.0%, and then sheeted into a paper having a basis weight of 70 g / m by using a rapid Kaiser forming method. 2 of paper.

[0060] Inspection items and inspection methods:

[0061] Whiteness (ISO %): tested according to the method in national standard GB / T 7974-2013;

[0062] Smoothness (s): Tested according to the method in national standard GB / T 456-2022;

[0063] Transverse folding endurance (times): tested according to the method in national standard GB / T 457-2008;

[0064] Bulk thickness (cm 3 ·g -1 ): Tested according to the method in national standard GB / T 9648-2008;

[0065] Tensile index (N·m / g): tested according to the method in national standard GB / T 453-2022;

[0066] Tear index (mN·m 2 ·g -1 ): Test according to the method in national standard GB / T 455-2002.

[0067] The test results are shown in Table 1:

[0068] Table 1

[0069]

[0070] As can be seen from Table 1, after the fiber pulp prepared in Examples 1 to 3 of the present invention is used to make paper, the whiteness, folding resistance, smoothness, tensile index and tear index of the paper are significantly higher than the data in Comparative Examples 1 to 4, indicating that the fiber pulp obtained by the pulping process of the present invention, the synergistic effect of each step, can effectively decompose lignin to obtain a purer fiber pulp, which not only effectively improves the extraction efficiency and yield of cellulose, but also effectively improves the whiteness of the pulp; and ensures the integrity and strength of the fiber, improves the bonding between fibers, and significantly improves the physical properties of the paper products made from the fiber pulp prepared by the method of the invention, and its physical properties such as smoothness, folding resistance, tensile index, tear index, etc. are significantly improved.

[0071] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A pulping process using plant fiber raw materials, characterized in that: The specific steps are as follows: S1. Select non-wood plant fiber raw materials, remove impurities, cut them, and soak them in a composite solution to obtain pretreated raw materials; The composite solution is composed of organic acid, cocamidopropyl betaine and water in a weight ratio of (5-10:0.8-1.2:100); S2, adjusting the pH of the pretreated raw material obtained in step S1, and then adding the composite enzyme preparation for enzymolysis to obtain an enzymolysis solution; S3, filtering the enzymatic hydrolyzate obtained in step S2, washing, then adding water and an auxiliary agent to the obtained solid matter, stirring evenly, performing mechanical grinding treatment, and then screening and washing to obtain fiber pulp; The non-wood plant fiber raw material in step S1 is selected from one of wheat straw and corn straw; The organic acid in the composite solution in step S1 is one or a combination of two of acetic acid, citric acid, oxalic acid and tartaric acid; The composite enzyme preparation in step S2 is a combination of cellulase and lignin peroxidase, wherein the addition amount of the cellulase is 20-40 IU / g, and the addition amount of the lignin peroxidase is 20-30 IU / g, based on the dry weight of the non-wood plant fiber raw material in step S1; The amount of the auxiliary agent added in step S3 is 13-16% of the total weight of the solid matter and water, and the auxiliary agent is composed of an ionic liquid and lauryl amide propyl amine oxide in a weight ratio of (10-15:1.5-3); the ionic liquid is one of 1-butyl-3-methylimidazole acetate and 1-ethyl-3-methylimidazole trifluoromethanesulfonate.

2. The pulping process using plant fiber raw materials according to claim 1, characterized in that: The amount of the composite solution added in step S1 is 6 to 10 times the weight of the non-wood plant fiber raw material in step S1; the soaking temperature in step S1 is 40 to 50° C., and the soaking time is 3 to 5 hours.

3. The pulping process using plant fiber raw materials according to claim 1, characterized in that: In step S2, the pH is adjusted to 4.0-5.5, and then the complex enzyme preparation is added and placed in a water bath at a temperature of 30-45° C. for 10-12 hours.

4. The pulping process using plant fiber raw materials according to claim 1, characterized in that: The amount of water added in step S3 is 2 to 3 times the amount of the solid matter after filtering and washing.

5. The pulping process using plant fiber raw materials according to claim 1, characterized in that: The grinding gap of the mechanical grinding process in step S3 is controlled to be 0.1 mm to 0.3 mm, and the grinding speed is 1000 rpm to 3000 rpm.

6. The pulping process using plant fiber raw materials according to claim 1, characterized in that: After the mechanical grinding treatment in step S3, two screenings are performed, with the screening mesh numbers being 80 mesh and 120 mesh respectively, followed by three washes, with the water temperature being controlled at 30-40° C., and a fiber pulp with a pulp concentration of 10-15% is obtained after the washing is completed.