Extraction bags and methods for manufacturing extraction bags, as well as sheets for extraction bags and methods for manufacturing sheets for extraction bags.

By using polylactic acid resin with a lower crystallinity than the nonwoven fabric layer as a lamination layer in the extraction bag and bonding it with heat above the glass transition temperature, the problem of damage to the nonwoven fabric and auxiliary components during heating is solved, achieving a strong connection and functional maintenance.

CN118475519BActive Publication Date: 2026-11-17OHKI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202280086555.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-01-19
Filing Date
2022-12-28
Publication Date
2026-11-17
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

In existing extraction bags, the nonwoven fabric and auxiliary components made of biodegradable materials are easily damaged when heated, leading to problems such as filter detachment or label removal.

Method used

Polylactic acid resin with a crystallinity lower than that of the nonwoven fabric layer is used as the laminate layer of the auxiliary component. During bonding, it is heated to 30-100°C above the glass transition temperature of polylactic acid resin, so that the laminate layer softens and bites into the fibers of the nonwoven fabric layer, thereby achieving a firm bond between the nonwoven fabric and the auxiliary component.

Benefits of technology

The structural integrity of the nonwoven fabric layer was protected during the bonding process, preventing damage to the filter function. At the same time, the connection of the auxiliary components was ensured, and the adhesive force was properly controlled to prevent detachment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118475519B_ABST
    Figure CN118475519B_ABST
Patent Text Reader

Abstract

The present invention provides an extraction bag in which the auxiliary components can be properly bonded to the sheet without damaging the nonwoven fabric side, even when the resin of the nonwoven fabric used as the sheet constituting the extraction bag and the resin for lamination used in the auxiliary components of the extraction bag are both biodegradable polylactic acid resin. An extraction bag (100) is formed by bonding a spunbond nonwoven fabric layer (10) containing polylactic acid resin to an auxiliary component (20), wherein a laminate layer (21) containing polylactic acid resin is provided on the surface of the auxiliary component (20) that is at least in contact with the spunbond nonwoven fabric layer (10), and the crystallinity of the polylactic acid resin contained in the laminate layer (21) is set to be less than the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer (10).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an extraction bag formed by bonding a spunbond nonwoven fabric layer comprising polylactic acid resin to an auxiliary component, and a method for manufacturing an extraction bag, as well as a sheet for extracting bags and a method for manufacturing a sheet for extracting bags. Background Technology

[0002] Regarding the sheets that constitute extraction bags for extracting coffee, black tea, soup, etc., in order to reduce the environmental impact when discarded after use, sheets using biodegradable materials have been developed (for example, see Patent Documents 1 and 2).

[0003] The coffee extraction sheet material described in Patent Document 1 is a sheet material formed from meltblown microfiber nonwoven fabric containing a biodegradable thermoplastic polymer. In the embodiments of this document, a drip coffee filter formed using meltblown nonwoven fabric containing polylactic acid microfibers is described.

[0004] The extraction sheet described in Patent Document 2 is also a sheet obtained by laminating a meltblown nonwoven fabric layer containing polylactic acid resin and a spunbond nonwoven fabric layer. This document... Figure 2 The text describes a tea bag with a label attached to the surface of a bag formed using the extraction sheet, for pinching with fingertips.

[0005] Even if the extraction sheet described in the aforementioned patent documents 1 and 2 is buried in the soil after use in the state of being contained in a bag for extracting the extract, the environmental impact can be reduced because the extraction sheet is also degraded by microorganisms along with the extract.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: Japanese Patent Application Publication No. 2000-336570

[0009] Patent Document 2: Japanese Patent Application Publication No. 2016-168569 Summary of the Invention

[0010] The problem that the invention aims to solve

[0011] For extraction bags, to reduce environmental impact, it is desirable that not only the sheet material but also all associated components use biodegradable materials. Various biodegradable materials exist, such as polylactic acid (PLA), polyhydroxyalkanoates (PHA), and polybutylene succinate (PBS). PLA resin, made from the same raw material, is preferred in all components to have similar decomposition characteristics. While some PLA resins have different melting points, they generally have roughly the same melting point as common raw materials. Therefore, if PLA resin, made from the same raw material, is used for both the nonwoven fabric used in the extraction bag and the laminating resin for the associated components, the fibers forming the nonwoven fabric may be damaged during heating for bonding purposes.

[0012] Regarding this point, for the coffee extraction sheet material described in Patent Document 1, if the sheet becomes brittle due to heat damage, the filter may peel off or fall off from the hook part, which is an auxiliary component, due to the load during coffee extraction. For the extraction sheet material described in Patent Document 2, if the label's adhesion to the bag is too strong, holes may be created in the sheet when the label is peeled off the bag. On the other hand, if the label's adhesion to the bag is too weak, the label may detach from the bag when the extracted liquid is filled into it, potentially causing manufacturing defects.

[0013] The present invention was made in view of the above-mentioned problems, and its object is to provide an extraction bag and a method for manufacturing an extraction bag, as well as a sheet for manufacturing an extraction bag and a sheet for manufacturing an extraction bag, wherein even if the resin of the nonwoven fabric used as the sheet constituting the extraction bag and the resin used for lamination in the auxiliary components of the extraction bag are biodegradable polylactic acid resin, the auxiliary components can be properly bonded to the sheet without damaging the nonwoven fabric side.

[0014] Methods for solving problems

[0015] The extraction bag of the present invention, which is used to solve the above-mentioned problems, is characterized by the following:

[0016] It is an extraction bag made by bonding a spunbond nonwoven fabric layer containing polylactic acid resin to ancillary components.

[0017] A laminate containing polylactic acid resin is provided on at least the surface of the aforementioned auxiliary component that contacts the aforementioned spunbond nonwoven fabric layer.

[0018] The crystallinity of the polylactic acid resin contained in the above-mentioned laminate layer is set to be less than that of the polylactic acid resin contained in the above-mentioned spunbond nonwoven fabric layer.

[0019] According to the extraction bag of this configuration, since the crystallinity of the polylactic acid resin contained in the laminate of the auxiliary component is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer, when heated for bonding, only the polylactic acid resin contained in the laminate of the auxiliary component softens, allowing the softened laminate to bite into the fibers of the spunbond nonwoven fabric layer, thus integrating the auxiliary component with the spunbond nonwoven fabric layer. At this time, since the polylactic acid resin contained in the spunbond nonwoven fabric layer does not soften even at the softening temperature of the polylactic acid resin contained in the laminate, the spunbond nonwoven fabric layer is not damaged and its function as a filter is maintained. Furthermore, since the adhesive force between the spunbond nonwoven fabric layer and the auxiliary component is properly controlled, there is no concern about damaging the spunbond nonwoven fabric layer even when the auxiliary component is peeled off.

[0020] In the extraction bag of the present invention, the difference between the crystallinity of the polylactic acid resin contained in the laminate layer and the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer is preferably set to 10% or more.

[0021] According to the extraction bag of this configuration, since the difference in crystallinity between the polylactic acid resin contained in the laminate layer and the polylactic acid resin contained in the spunbond nonwoven fabric layer is set to 10% or more, only the polylactic acid resin contained in the laminate layer with lower crystallinity softens. The softened laminate layer then bites into the fibers of the spunbond nonwoven fabric layer, thereby achieving a firm bond and integration. At this time, the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer is more than 10% higher than that of the polylactic acid resin contained in the laminate layer. Therefore, it does not soften even at the softening temperature of the polylactic acid resin contained in the laminate layer, and the structure of the spunbond nonwoven fabric layer is maintained. Thus, the spunbond nonwoven fabric layer is not damaged and can maintain its function as a filter.

[0022] In the extraction bag of the present invention, preferably, a meltblown nonwoven fabric layer containing polylactic acid resin is provided on the spunbond nonwoven fabric layer.

[0023] The extraction bag according to this configuration reduces the environmental impact of the entire extraction bag because a meltblown nonwoven fabric layer containing polylactic acid resin is provided on the spunbond nonwoven fabric layer. Furthermore, the layered structure of the spunbond nonwoven fabric layer and the meltblown nonwoven fabric layer provides excellent functionality as a filter.

[0024] The method for manufacturing the extraction bag of the present invention for solving the above-mentioned problems is characterized by the following:

[0025] It is a method for manufacturing an extraction bag by bonding a spunbond nonwoven fabric layer containing polylactic acid resin to an auxiliary component.

[0026] A laminate containing polylactic acid resin is provided on at least the surface of the aforementioned auxiliary component that contacts the aforementioned spunbond nonwoven fabric layer.

[0027] The crystallinity of the polylactic acid resin contained in the above-mentioned laminate layer is set to be less than that of the polylactic acid resin contained in the above-mentioned spunbond nonwoven fabric layer.

[0028] When joining the spunbond nonwoven fabric layer to the attached component, a heating process is performed to impart a temperature 30 to 100°C higher than the glass transition temperature Tg of polylactic acid resin.

[0029] According to the manufacturing method of the extraction bag of this configuration, since the crystallinity of the polylactic acid resin contained in the laminate layer of the auxiliary component is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer, a heating process is performed when bonding the spunbond nonwoven fabric layer to the auxiliary component, applying a temperature 30 to 100°C higher than the glass transition temperature (Tg) of the polylactic acid resin. This softens only the polylactic acid resin contained in the laminate layer of the auxiliary component, allowing the softened laminate layer to penetrate between the fibers of the spunbond nonwoven fabric layer, thus integrating the auxiliary component and the spunbond nonwoven fabric layer. At this time, since the polylactic acid resin contained in the spunbond nonwoven fabric layer does not soften even at the softening temperature of the polylactic acid resin contained in the laminate layer, the spunbond nonwoven fabric layer is not damaged and its function as a filter is maintained. Furthermore, since the adhesive force between the spunbond nonwoven fabric layer and the auxiliary component is appropriately controlled, there is no concern about damaging the spunbond nonwoven fabric layer even when the auxiliary component is peeled off.

[0030] The sheet for extraction bags of the present invention, which is used to solve the above-mentioned problems, is characterized by the following:

[0031] It is a sheet material for extraction bags made by bonding a spunbond nonwoven fabric layer containing polylactic acid resin to ancillary components.

[0032] A laminate containing polylactic acid resin is provided on at least the surface of the aforementioned auxiliary component that contacts the aforementioned spunbond nonwoven fabric layer.

[0033] The crystallinity of the polylactic acid resin contained in the above-mentioned laminate layer is set to be less than that of the polylactic acid resin contained in the above-mentioned spunbond nonwoven fabric layer.

[0034] According to the sheet material for the extraction bag of this configuration, since the crystallinity of the polylactic acid resin contained in the laminate layer of the auxiliary component is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer, when heated for bonding, only the polylactic acid resin contained in the laminate layer of the auxiliary component softens, allowing the softened laminate layer to bite into the fibers of the spunbond nonwoven fabric layer, thus integrating the auxiliary component with the spunbond nonwoven fabric layer. At this time, since the polylactic acid resin contained in the spunbond nonwoven fabric layer does not soften at the softening temperature of the polylactic acid resin contained in the laminate layer, the spunbond nonwoven fabric layer is not damaged and can maintain its function as a filter. In addition, since the adhesive force between the spunbond nonwoven fabric layer and the auxiliary component is properly controlled, there is no concern about damaging the spunbond nonwoven fabric layer even when the auxiliary component is peeled off from it.

[0035] The method for manufacturing the extraction bag sheet of the present invention for solving the above-mentioned problems is characterized by the following:

[0036] This is a method for manufacturing a sheet material for extraction bags by bonding a spunbond nonwoven fabric layer containing polylactic acid resin to an auxiliary component.

[0037] A laminate containing polylactic acid resin is provided on at least the surface of the aforementioned auxiliary component that contacts the aforementioned spunbond nonwoven fabric layer.

[0038] The crystallinity of the polylactic acid resin contained in the above-mentioned laminate layer is set to be less than that of the polylactic acid resin contained in the above-mentioned spunbond nonwoven fabric layer.

[0039] When joining the spunbond nonwoven fabric layer to the attached component, a heating process is performed to impart a temperature 30 to 100°C higher than the glass transition temperature Tg of polylactic acid resin.

[0040] According to the manufacturing method of the extraction bag sheet of this configuration, since the crystallinity of the polylactic acid resin contained in the laminate layer of the auxiliary member is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer, a heating process is performed when bonding the spunbond nonwoven fabric layer to the auxiliary member, applying a temperature 30 to 100°C higher than the glass transition temperature (Tg) of the polylactic acid resin. This softens only the polylactic acid resin contained in the laminate layer of the auxiliary member, allowing the softened laminate layer to penetrate between the fibers of the spunbond nonwoven fabric layer, thus integrating the auxiliary member and the spunbond nonwoven fabric layer. At this time, since the polylactic acid resin contained in the spunbond nonwoven fabric layer does not soften even at the softening temperature of the polylactic acid resin contained in the laminate layer, the spunbond nonwoven fabric layer is not damaged and its function as a filter is maintained. Furthermore, since the adhesive force between the spunbond nonwoven fabric layer and the auxiliary member is appropriately controlled, there is no concern about damaging the spunbond nonwoven fabric layer even when the auxiliary member is peeled off. Attached Figure Description

[0041] Figure 1 This is a cross-sectional view illustrating the stacked structure of the extraction bag (drip filter bag) according to the first embodiment of the present invention.

[0042] Figure 2 This is a cross-sectional view illustrating the stacked structure of the extraction bag (drip filter bag) according to the second embodiment of the present invention.

[0043] Figure 3 This is a cross-sectional view illustrating the stacked structure of the extraction bag (tea bag) according to the third embodiment of the present invention. Detailed Implementation

[0044] The following describes in detail embodiments of the extraction bag and its manufacturing method, as well as the sheet material for the extraction bag and its manufacturing method. It should be noted that, for ease of understanding, the shape and size relationships of the layered structures of the extraction bag shown in the figures are appropriately simplified and exaggerated, and do not directly reflect the actual shape and size relationships. Furthermore, the present invention is not intended to be limited to the configuration described below.

[0045] [Sheet material for extraction bags]

[0046] In its basic structure, the extraction bag sheet of the present invention comprises a laminate obtained by laminating a spunbond nonwoven fabric layer containing polylactic acid resin and an auxiliary member. The auxiliary member has a polylactic acid resin-containing material laminated on its surface (at least the surface in contact with the spunbond nonwoven fabric layer). As lamination methods, extrusion lamination, dry lamination, hot lamination, wet lamination, etc., are known; however, if the crystallinity of the polylactic acid resin contained in the laminated layer is less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer, then any processing method is acceptable. Examples of auxiliary members include, for instance, hooks for attaching extraction bags made from the extraction bag sheet of the present invention to containers such as cups, labels with strings attached to the extraction bags, and thin plate-like members for moving the extraction bags up and down in hot water. A meltblown nonwoven fabric layer containing polylactic acid resin is provided on the spunbond nonwoven fabric layer, if necessary.

[0047] [Extraction bag]

[0048] The extraction bag of the present invention is obtained by processing the extraction bag of the present invention from sheet material into a bag shape. Examples of bag-making methods include welding using heat or ultrasound, joining using adhesives, and sewing using thread. Three representative embodiments of the extraction bag of the present invention will be described below.

[0049] <First Implementation Method>

[0050] Figure 1This is a cross-sectional view schematically illustrating the laminated structure of the extraction bag according to the first embodiment of the present invention. The extraction bag is used in the form of a drip filter bag 100, which is obtained by joining a spunbond nonwoven fabric layer 10 with a cardboard 20 as an accessory component.

[0051] [Spunbond nonwoven layer]

[0052] The spunbond nonwoven layer 10 functions as a filter for extracting target components. The spunbond nonwoven layer 10 is formed by blowing a high-speed airflow through molten resin extruded from a spinning nozzle to draw and stretch it, while simultaneously cooling and solidifying it to form fibers. These fibers are then aggregated on a collector to form a mesh. In the drip filter bag 100 of the first embodiment, polylactic acid resin, a biodegradable resin, is used as the resin constituting the spunbond nonwoven layer 10. The area weight of the spunbond nonwoven layer 10 is preferably set to 8–20 g / m². 2 More preferably 12-20 g / m 2 .

[0053] [cardboard]

[0054] The cardboard 20 is a component used to form a hook for attaching the drip filter bag 100 to containers such as cups. Therefore, in order to have a certain degree of rigidity, the weight per unit area of ​​the cardboard is preferably set to 150-300 g / m². 2 .

[0055] For the cardboard 20, a laminated layer 21, formed by coating a laminating material mainly composed of a thermoplastic resin, is provided on the surface that is in contact with at least the spunbond nonwoven fabric layer 10. In the drip filter bag 100 of the first embodiment, polylactic acid resin, a biodegradable resin, is used as the resin for forming the laminated layer 21, similar to that used for the spunbond nonwoven fabric layer 10. The thickness of the laminated layer 21 is preferably set to 20 to 80 μm, more preferably 40 to 80 μm.

[0056] Polylactic acid resin

[0057] The drip filter bag 100 of the first embodiment is obtained by bonding a cardboard 20 to a spunbond nonwoven fabric layer 10. The bonding is achieved by stacking the spunbond nonwoven fabric layer 10 and the cardboard 20 together and heating them to soften the polylactic acid resin contained in the laminate layer 21 on the surface of the cardboard 20, allowing the softened polylactic acid resin to penetrate into the gaps of the spunbond nonwoven fabric layer 10. Therefore, in order to effectively bond the cardboard 20 to the spunbond nonwoven fabric layer 10, it is important to understand the mechanism of polylactic acid resin softening and to perform the bonding (heating) under appropriate conditions. Here, polylactic acid resin is a crystalline polymer capable of phase transition between a crystalline phase and an amorphous phase. Like other common polymer materials, polylactic acid resin has the following properties: it gradually softens above its glass transition temperature; it softens easily if it has a large amorphous portion; and it does not soften easily in its crystalline state. Moreover, the higher the crystallinity of the polylactic acid resin, the higher its heat resistance.

[0058] The inventors believe that when a paperboard 20 having a laminate layer 21 containing polylactic acid resin is bonded to a spunbond nonwoven fabric layer 10 containing polylactic acid resin, the crystallinity of the polylactic acid resin is closely related to the quality of the left-right bonding. They have found that by appropriately setting the relationship between the crystallinity of the polylactic acid resin on the spunbond nonwoven fabric layer 10 side and the crystallinity of the polylactic acid resin on the paperboard 20 (laminate layer 21) side, the paperboard 20 can be bonded to the spunbond nonwoven fabric layer 10 without damaging the spunbond nonwoven fabric layer 10.

[0059] The crystallinity of polylactic acid (PLA) resin is determined as follows. First, test pieces cut from spunbond nonwoven fabric layer 10 and laminate layer 21 are placed in a differential scanning calorimeter (DSC) and heated at a specific rate from a temperature lower than the glass transition temperature Tg (approximately 50–60 °C) of PLA resin to a temperature exceeding the melting point Tm (approximately 150–170 °C). For example, the temperature is increased from 30 °C to 240 °C at a rate of 10 °C / min. During this heating process, the amorphous portion of PLA resin temporarily transitions to crystals, and if the temperature is further increased, the crystals melt and eventually become molten. Here, the heat of crystallization when the amorphous portion of PLA resin transitions to crystals is denoted as ΔHc, and the heat of melting when the crystals of PLA resin melt is denoted as ΔHm. The crystallinity χc (%) of PLA resin is calculated by the following formula (1).

[0060] χc(%)=(ΔHm-ΔHc) / Q×100···(1)

[0061] It should be noted that Q is the heat of fusion of the complete crystal, and in the case of polylactic acid resin, Q = 93 J / g.

[0062] According to the novel insights obtained by the inventors, in order to ensure that the paperboard 20 bonds smoothly to the spunbond nonwoven fabric layer 10, it is important to set the crystallinity of the polylactic acid resin contained in the laminate layer 21 of the paperboard 20 to be less than the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer 10. For example, the crystallinity of the polylactic acid resin contained in the laminate layer 21 is set to 1-40%, and the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer 10 is set to 30-60%. Here, the difference between the crystallinity of the polylactic acid resin contained in the laminate layer 21 and the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer 10 is preferably set to 10% or more. In this case, the polylactic acid resin contained in the laminate layer 21 of the paperboard 20 softens easily, while the polylactic acid resin contained in the spunbond nonwoven fabric layer 10 is difficult to soften. In this way, if a temperature higher than the glass transition temperature Tg of polylactic acid resin (e.g., Tg + 30°C to 100°C) is applied when bonding the spunbond nonwoven fabric layer 10 to the paperboard 20, only the polylactic acid resin contained in the laminate layer 21 of the paperboard 20, which has a lower crystallinity, softens. The softened laminate layer 21 then bites into the fibers of the spunbond nonwoven fabric layer 10, thereby firmly bonding the paperboard 20 to the spunbond nonwoven fabric layer 10 as an integral unit. At this time, the polylactic acid resin contained in the spunbond nonwoven fabric layer 10 has a higher crystallinity than the polylactic acid resin contained in the laminate layer 21, and therefore does not soften even at the softening temperature of the polylactic acid resin contained in the laminate layer 21, thus maintaining the structure of the spunbond nonwoven fabric layer 10. Thus, if the crystallinity of the polylactic acid resin contained in the laminate layer 21 of the paperboard 20 is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer 10, it is possible to achieve the bonding of the spunbond nonwoven fabric layer 10 and the paperboard 20 (laminate layer 21), which were previously considered difficult to achieve, and the spunbond nonwoven fabric layer 10 can maintain its function as a filter without being damaged. In addition, since the drip filter bag 100 uses polylactic acid resin as its main raw material, it also greatly contributes to reducing the environmental impact when it is discarded after use.

[0063] <Second Implementation Method>

[0064] Figure 2 This is a cross-sectional view schematically illustrating the laminated structure of the extraction bag according to the second embodiment of the present invention. The extraction bag is used in the form of a coffee drip bag 200, obtained by laminating a spunbond nonwoven fabric layer 10 and a meltblown nonwoven fabric layer 15, and then bonding a cardboard 20 to the laminate. The drip bag 200 of the second embodiment is obtained by providing a meltblown nonwoven fabric layer 15 on the spunbond nonwoven fabric layer 10 in the drip bag 100 of the first embodiment. Therefore, in the following description, only the meltblown nonwoven fabric layer 15 will be described, and detailed descriptions of structures identical to those of the drip bag 100 of the first embodiment will be omitted.

[0065] [Meltblown nonwoven fabric layer]

[0066] The meltblown nonwoven layer 15 functions as a layer to prevent the leakage of adhesive and contents powder during bag making. The meltblown nonwoven layer 15 is formed by blowing a high-temperature, high-speed airflow through molten resin extruded from a spinning nozzle, thereby stretching and fiberizing the molten resin and causing it to disperse, then collecting it on a collector and solidifying it into a sheet. In the drip filter bag 200 of the second embodiment, polylactic acid resin, a biodegradable resin, is preferably used as the resin constituting the meltblown nonwoven layer 15, similar to that of the spunbond nonwoven layer 10. Thus, by including polylactic acid resin in all nonwoven layers, the environmental impact of the entire drip filter bag 200 is reduced, and the laminated structure of the spunbond nonwoven layer 10 and the meltblown nonwoven layer 15 provides excellent filter functionality. The weight per unit area of ​​the meltblown nonwoven layer 15 is preferably set to 1 to 10 g / m². 2 More preferably 6-10 g / m 2 .

[0067] The crystallinity of the polylactic acid resin contained in the meltblown nonwoven layer 15 is not particularly limited, but it is known to be less than that of the polylactic acid resin contained in the spunbond nonwoven layer 10. For example, when the crystallinity of the polylactic acid resin contained in the spunbond nonwoven layer 10 is set to 30-60% as described above, the crystallinity of the polylactic acid resin contained in the meltblown nonwoven layer 15 is 20-40%. In this case, if the laminate of the meltblown nonwoven layer 15 and the spunbond nonwoven layer 10 is folded with the meltblown nonwoven layer 15 as the inside and then heated, the meltblown nonwoven layer 15 functions as an adhesive, making bag making easier.

[0068] <Third Implementation Method>

[0069] Figure 3 This is a cross-sectional view illustrating the laminated structure of the extraction bag according to the third embodiment of the present invention. The extraction bag is used in the form of a tea bag 300 obtained by joining a spunbond nonwoven fabric layer 10 with a label 30 as an accessory component. It should be noted that the tea bag 300 of this third embodiment may also be configured such as the drip filter bag 200 of the second embodiment, with a meltblown nonwoven fabric layer 15 laminated on the spunbond nonwoven fabric layer 10. The tea bag 300 of the third embodiment is obtained by replacing the cardboard 20 with the label 30 in the drip filter bag 100 of the first embodiment. Therefore, in the following description, only the label 30 will be described, and detailed descriptions of configurations identical to those of the drip filter bag 100 of the first embodiment will be omitted.

[0070] [Label]

[0071] Label 30 is a component that is pinched with fingers when the tea bag 300 is suspended by a thread. It is adhered to the surface of the bag when not in use and peeled off when in use. The weight per unit area of ​​the label is preferably set to 50-150 g / m². 2 .

[0072] For label 30, a laminated layer 31, formed by coating a laminating material mainly composed of thermoplastic resin, is provided on the surface that is in contact with at least the spunbond nonwoven fabric layer 10. In the tea bag 300 of the third embodiment, polylactic acid resin, a biodegradable resin, is used as the resin for forming the laminated layer 31, similar to that used for the spunbond nonwoven fabric layer 10. The thickness of the laminated layer 31 is preferably set to 10 to 80 μm, more preferably 40 to 80 μm.

[0073] The crystallinity of the polylactic acid resin contained in the laminate layer 31 of the label 30 is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer 10. For example, the crystallinity of the polylactic acid resin contained in the laminate layer 31 is set to 1-20%, and the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer 10 is set to 30-60%. Here, the difference between the crystallinity of the polylactic acid resin contained in the laminate layer 31 and the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer 10 is preferably set to 10% or more. In this case, the polylactic acid resin contained in the laminate layer 31 of the label 30 softens easily, while the polylactic acid resin contained in the spunbond nonwoven fabric layer 10 is difficult to soften. Therefore, the label 30 can be adhered to the spunbond nonwoven fabric layer 10 with an appropriate adhesive force. As a result, the label 30 does not fall off when the extract is filled into the tea bag 300, and there is no concern about damaging the tea bag 300 when peeling off the label 30 from the tea bag 300 during use.

[0074] [Manufacturing method of extraction bag (sheet material for extraction bag)]

[0075] The extraction bag (sheet material for extraction bag) of the present invention can be manufactured, for example, using heated clamping rollers. It should be noted that heated clamping rollers are conventionally known manufacturing devices and are not shown in the figure.

[0076] When manufacturing the drip filter bag 100 of the first embodiment, a cardboard 20 having a laminated layer 21 formed by extrusion lamination is laminated onto the spunbond nonwoven fabric layer 10, and the laminate is passed through a pair of heated clamping rollers. When manufacturing the drip filter bag 200 of the second embodiment, a meltblown nonwoven fabric layer 15 is formed on the spunbond nonwoven fabric layer 10, and then a cardboard 20 having a laminated layer 21 formed by extrusion lamination is laminated onto the side of the spunbond nonwoven fabric layer 10, and the laminate is passed through a pair of heated clamping rollers. When manufacturing the tea bag 300 of the third embodiment, a label 30 having a laminated layer 31 formed by dry lamination is laminated onto the spunbond nonwoven fabric layer 10, and the laminate is passed through a pair of heated clamping rollers.

[0077] Here, if the heating temperature from the heated rollers is set to a temperature higher than the glass transition temperature Tg of polylactic acid resin (e.g., Tg + 30°C to 100°C), then, for example, in the drip filter bag 100 of the first embodiment, when the laminate passes through a pair of heated rollers, the polylactic acid resin contained in the laminate layer 21 on the surface of the cardboard 20 softens and bites into the gap of the spunbond nonwoven fabric layer 10, thereby integrally bonding the spunbond nonwoven fabric layer 10 with the cardboard 20. At this time, since the polylactic acid resin contained in the spunbond nonwoven fabric layer 10 does not soften at the temperature at which the polylactic acid resin contained in the laminate layer 21 softens, the spunbond nonwoven fabric layer 10 is not damaged and can maintain its function as a filter. For the drip filter bag 200 of the second embodiment and the tea bag 300 of the third embodiment, the same phenomenon can be used to bond the spunbond nonwoven fabric layer 10 to the cardboard 20 or the label 30.

[0078] Regarding the pair of heating clamping rollers used in the manufacturing method of the extraction bag (sheet material for extraction bag) of the present invention, they can be configured as a pair of clamping rollers obtained by combining two flat rollers, or they can be a pair of clamping rollers obtained by configuring one as an embossing roller and the other as a flat roller.

[0079] Example

[0080] The following describes embodiments of the extraction bag of the present invention. However, the present invention is not limited to the following embodiments.

[0081] Extraction bags having the characteristic structure of the present invention (Examples 1-14) and extraction bags not having the characteristic structure of the present invention (Comparative Examples 1-2) were prepared and evaluated.

[0082] [Crystallization (%)]

[0083] Test pieces were collected from nonwoven fabric and placed on a differential scanning calorimeter (DSC) (TA INSTRUMENTS, product number 2920MDSC V2.6A). The temperature was then increased to 240°C at a rate of 10°C / min, and the heat of crystallization ΔHc and the heat of fusion ΔHm were measured. The crystallinity of the nonwoven fabric was then calculated based on equation (1) above.

[0084] Weight per unit area (g / m²) 2 )]

[0085] According to "JIS L 1913 General Test Method for Nonwoven Fabrics", a 10cm square test piece was collected from the nonwoven fabric, the mass was measured, and the weight per unit area of ​​the nonwoven fabric was calculated.

[0086] [evaluate]

[0087] The condition of the extraction bag after heat sealing is evaluated visually based on the following criteria.

[0088] Good: The spunbond nonwoven layer is undamaged and the cardboard is bonded.

[0089] Defect: The spunbond nonwoven fabric layer is damaged, or the cardboard is not bonded.

[0090] <Example 1>

[0091] like Figure 1 As shown, in a spunbond nonwoven fabric containing polylactic acid resin with a crystallinity of 50% (weight per unit area: 15 g / m²), 2 On top of this, a paperboard with a laminated layer (thickness: 40μm) (weight per unit area: 200g / m²) is stacked. 2 The extraction bag of Example 1 was produced by heating the clamping rollers as a heat-sealing process. The heat-sealing process was carried out for 0.5 seconds at a temperature of 110°C and a pressure of 0.5 MPa. The laminate was formed by extrusion lamination of polylactic acid resin in a flowing state onto a paperboard. A polylactic acid resin with a crystallinity of 3% was used. It should be noted that the extraction bag of Example 1 was actually a sheet material for extraction bags before being made into a bag shape, but since the characteristics of the raw materials themselves were not changed, it was evaluated as an extraction bag.

[0092] <Examples 2-14, Comparative Examples 1-2>

[0093] Except for having the configuration shown in Table 1, extraction bags for Examples 2-14 and Comparative Examples 1-2 were manufactured in the same manner as the extraction bag of Example 1. It should be noted that in the extraction bags of Examples 9-11, as... Figure 2 As shown, a meltblown nonwoven fabric layer is stacked on top of a spunbond nonwoven fabric layer. Furthermore, in the extraction bags of Examples 13 and 14, and Comparative Examples 1-2, a laminate is formed by dry lamination of a stretched polylactic acid film.

[0094] The composition of the extraction bags of Examples 1 to 14 and the extraction bags of Comparative Examples 1 to 2, as well as the evaluation results, are shown in Table 1.

[0095] [Table 1]

[0096]

[0097] SB: Spunbond nonwoven fabric layer

[0098] MB: Meltblown nonwoven fabric layer

[0099] In Examples 1-14, where the crystallinity of the polylactic acid resin in the laminate was set to be less than that in the spunbond nonwoven fabric layer, the extraction bags did not damage the spunbond nonwoven fabric layer and could all be heat-sealed. Furthermore, in the extraction bags of Examples 1-14, only the polylactic acid resin in the laminate layer of the cardboard, which has a lower crystallinity, softened. The softened laminate layer then penetrated between the fibers of the spunbond nonwoven fabric layer, thus firmly bonding the cardboard to the spunbond nonwoven fabric layer, resulting in an integrated structure between the cardboard and the spunbond nonwoven fabric layer.

[0100] In contrast, regarding the extraction bag of Comparative Example 1, where the heat-sealing temperature was set to 130°C and the crystallinity of the polylactic acid resin contained in the laminate was set to be equal to that of the polylactic acid resin contained in the spunbond nonwoven fabric layer (i.e., the crystallinity of the polylactic acid resin contained in the laminate was not set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer), the resin in the laminate did not soften, and the spunbond nonwoven fabric layer did not bond with the cardboard. Furthermore, regarding the extraction bag of Comparative Example 2, which had the same structure as the extraction bag of Comparative Example 1 and where the heat-sealing temperature was set to 150°C, although the polylactic acid resin in the laminate softened, the fibers contained in the spunbond nonwoven fabric layer also softened, and the spunbond nonwoven fabric layer was damaged.

[0101] Industrial availability

[0102] The extraction bag and sheet material for extraction bags of the present invention can be used as drip bags for coffee extraction, tea bags for tea extraction, and soup bags for extracting the broth of bonito flakes, kelp, etc. Furthermore, the manufacturing method of the extraction bag and sheet material for extraction bags of the present invention can be used in the manufacture of filters for the above-mentioned applications.

[0103] Explanation of reference numerals in the attached figures

[0104] 10 layers of spunbond nonwoven fabric

[0105] 15 layers of meltblown nonwoven fabric

[0106] 20 cardboard pieces (attached components)

[0107] 21-layer laminate

[0108] 30 Labels (Attached Components)

[0109] 31-layer laminate

[0110] 100-drop filter bag (extraction bag)

[0111] 200-drop filter bag (extraction bag)

[0112] 300 tea bags (extraction bags)

Claims

1. An extraction bag, comprising a spunbond nonwoven fabric layer containing polylactic acid resin bonded to an auxiliary component. A laminate containing polylactic acid resin is provided on at least the surface of the auxiliary member that contacts the spunbond nonwoven fabric layer, in such a way that it bites into the gaps of the spunbond nonwoven fabric layer. The crystallinity of the polylactic acid resin contained in the laminate is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer.

2. The extraction bag according to claim 1, wherein, The difference between the crystallinity of the polylactic acid resin contained in the laminate layer and the crystallinity of the polylactic acid resin contained in the spunbond nonwoven fabric layer is set to be 10% or more.

3. The extraction bag according to claim 1 or 2, wherein, A meltblown nonwoven fabric layer containing polylactic acid resin is disposed on the spunbond nonwoven fabric layer.

4. A method for manufacturing an extraction bag, comprising bonding a spunbond nonwoven fabric layer containing polylactic acid resin to an auxiliary component to form the extraction bag. A laminate containing polylactic acid resin is provided on at least the surface of the auxiliary member that contacts the spunbond nonwoven fabric layer, in such a way that it bites into the gaps of the spunbond nonwoven fabric layer. The crystallinity of the polylactic acid resin contained in the laminate layer is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer. When bonding the spunbond nonwoven fabric layer to the auxiliary component, a heating process is performed to impart a temperature 30°C to 100°C higher than the glass transition temperature Tg of polylactic acid resin.

5. A sheet for extraction bags, comprising a spunbond nonwoven fabric layer containing polylactic acid resin bonded to an auxiliary component. A laminate containing polylactic acid resin is provided on at least the surface of the auxiliary member that contacts the spunbond nonwoven fabric layer, in such a way that it bites into the gaps of the spunbond nonwoven fabric layer. The crystallinity of the polylactic acid resin contained in the laminate is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer.

6. A method for manufacturing a sheet for an extraction bag, comprising bonding a spunbond nonwoven fabric layer containing polylactic acid resin to an auxiliary component to form the sheet for the extraction bag. A laminate containing polylactic acid resin is provided on at least the surface of the auxiliary member that contacts the spunbond nonwoven fabric layer, in such a way that it bites into the gaps of the spunbond nonwoven fabric layer. The crystallinity of the polylactic acid resin contained in the laminate layer is set to be less than that of the polylactic acid resin contained in the spunbond nonwoven fabric layer. When bonding the spunbond nonwoven fabric layer to the auxiliary component, a heating process is performed to impart a temperature 30°C to 100°C higher than the glass transition temperature Tg of polylactic acid resin.

Citation Information

Patent Citations

  • Biodegradable sheet material for coffee extraction

    JP2000336570A

  • Sheet for extraction, filter for extraction, and bag for extraction

    JP2016168569A

  • Sheet for extraction, extraction filter, and extraction bag

    CN107427737A

  • Method for producing biodegradable laminate

    JP2006341616A