A method for preparing light calcium carbonate with controllable morphology and particle size
By controlling the mineralization reaction conditions, light calcium carbonate with controllable morphology and particle size was prepared, which solved the problems of crystal form inhibitor use and high-temperature calcination in traditional methods, and achieved high purity and high dispersion light carbonic acid Calcium preparation reduces production costs and environmental impact.
Patent Information
- Application Number
- CN202410597711.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-05-14
AI Technical Summary
The existing preparation methods for light calcium carbonate require a large number of crystalline inhibitors, which are costly to produce, and high-temperature calcination leads to energy consumption and environmental pollution. Traditional methods cannot meet the high requirements for purity and morphology of high-end products.
By adding ammonia water and nano-calcium carbonate solutions to the solution containing calcium chloride, the pH value and gas inflow of mineralization reactions are controlled, the concentration of calcium chloride and nano-calcium carbonate is adjusted, and the low-temperature mineralization reaction is used to prepare the morphology and Lightweight calcium carbonate with controllable particle size, avoid using crystal form control agents.
The stable preparation of lightweight calcium carbonate of different morphology and sizes is achieved, which improves the purity and dispersion of the product, reduces production costs, reduces energy consumption and environmental pollution, and meets the high requirements of high-end products.
Smart Images

Figure CN118479521B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of light calcium carbonate preparation, and in particular to a method for preparing light calcium carbonate with controllable morphology and particle size. Background Art
[0002] Light calcium carbonate is a kind of chemical powder with extremely wide applications in inorganic chemical products. It is widely used in papermaking, plastics, rubber, coatings, medicine, food processing, sealants, adhesives and other fields. Depending on the preparation process, the crystal structure of light calcium carbonate is different, and it can be in different crystal morphologies such as spindle, flake, cube, needle-rod, regular dodecahedron, rose, etc.
[0003] In the papermaking industry, needle-shaped light calcium carbonate can be used as a papermaking filler to improve paper strength and opacity; rose-shaped light calcium carbonate can give paper better bulk and air permeability, improve ink absorption, reduce cutter wear, and improve paper printing adaptability. Regular dodecahedron-shaped light calcium carbonate can improve the mechanical properties of the matrix material, effectively improve the fluidity and processing performance of the system, and also improve the surface finish and filling performance of the product.
[0004] At present, the industrial method for preparing needle-shaped, rose-shaped, regular dodecahedral and other light calcium carbonate is mainly based on carbonization, which requires high-temperature calcination of limestone to obtain calcium oxide, add water to prepare lime slurry, and add an appropriate amount of crystal control agent to the lime slurry before carbonization to obtain the desired crystal form of light calcium carbonate. Commonly used crystal inhibitors include magnesium chloride, magnesium hydroxide, strontium chloride, sodium hexametaphosphate, sodium pyrophosphate, sodium tripolyphosphate, sodium polyacrylate, polyacrylic acid phthalamide, etc. The above method has the following problems: a large amount of crystal inhibitors need to be added, and the production cost is high; during the continuous production process, as the crystal inhibitors continue to accumulate, they will also adhere to the light calcium carbonate, reducing the product quality and whiteness; in addition, high-temperature calcination of limestone requires a lot of energy consumption on the one hand, and on the other hand, it will cause a large amount of greenhouse gas CO2 to be discharged into the air, causing environmental pollution. In addition, since the raw material limestone belongs to mineral resources and is non-renewable, it is urgent to develop a new method for preparing light calcium carbonate to replace the traditional preparation method.
[0005] Publication number is CN113620331A Chinese invention patent discloses a method for preparing nano vaterite calcium carbonate from CO2 mineralized carbide slag, the method uses ammonium sulfate as carbide slag leaching agent, and obtains nano vaterite calcium carbonate with higher purity and whiteness through a step-by-step gentle mineralization process. The nano vaterite calcium carbonate obtained by the method will be doped with calcium sulfate in calcium carbonate due to the addition of ammonium sulfate as leaching agent, reducing the purity of calcium carbonate, and using a flotation agent will increase production costs.
[0006] The Chinese invention patent with publication number CN105800657A discloses a method for preparing rose-shaped precipitated calcium carbonate, which uses medium-burned lime and digestion water with a composite crystal inhibitor added thereto in a ratio of 1:5-10 for digestion, and then filters and removes slag through a 60-120 mesh vibrating screen, dilutes the obtained calcium hydroxide emulsion with water, adds a crystal control agent, and then feeds it into a reaction tower, introduces kiln gas to carbonize it to pH <7.5, and then stops carbonization, dehydrates, dries, crushes, and sieves the precipitated calcium carbonate suspension to obtain a rose-shaped precipitated calcium carbonate. In this method, it is necessary to add a variety of monosaccharides and polysaccharides to prepare digestion water, and a large amount of crystal control agent is also added to the refined slurry, and this method is a traditional method for preparing light calcium carbonate, and the rose-shaped crystal form is caused by the agglomeration of spindle-shaped calcium carbonate.
[0007] The Chinese invention patent with publication number CN110775994A discloses a method for preparing regular cubic light calcium carbonate from carbide slag, which uses carbide slag as raw material, extracts calcium ions in the carbide slag with ammonium chloride solution, then adds a crystal control agent to the carbide slag leaching solution, then drips an ammonium bicarbonate solution, filters the carbonized liquid after reaction, and obtains a cubic light calcium carbonate sample after washing and drying the obtained filter cake. In this method, ammonium bicarbonate is used as a mineralization raw material, which greatly increases the production cost, and a crystal inhibitor needs to be added during the mineralization process, which increases the production cost on the one hand, and reduces the purity and whiteness of the light calcium carbonate on the other hand.
[0008] The Chinese invention patent with publication number CN106430272A discloses a method for preparing rod-shaped aragonite calcium carbonate, which comprises crushing limestone, calcining it, and then digesting it at a ash-water mass ratio of 1:3-8 to obtain lime slurry; screening, filtering and removing slag, adding water to adjust the solid content of the lime slurry, and obtaining refined lime slurry; controlling the temperature of the refined lime slurry to 30-60°C, adding a composite crystal form control agent of 0.5-2.0% of the mass of calcium hydroxide in the lime slurry, and then transporting it to a carbonation tower, starting stirring, introducing kiln gas for carbonation reaction until the pH is 8.0, stopping ventilation, terminating the carbonation reaction, and obtaining a precipitated calcium carbonate suspension; finally, dehydrating and drying according to conventional methods to obtain rod-shaped aragonite calcium carbonate. The method for preparing rod-shaped calcium carbonate is a traditional method for preparing calcium carbonate, and a crystal form inhibitor needs to be added during the mineralization process.
[0009] In view of this, the present invention is proposed. Summary of the invention
[0010] The purpose of the present invention is to provide a method for preparing light calcium carbonate with controllable morphology and particle size, which can not only obtain light calcium carbonate with specific crystal form, morphology and size, but also each prepared crystal form has regular morphology, excellent dispersibility and relatively high purity, thus meeting the high requirements of high-end products for light calcium carbonate.
[0011] The present invention provides a method for preparing light calcium carbonate with controllable morphology and particle size, comprising the following steps:
[0012] Adding ammonia water and nano calcium carbonate solution to the solution containing calcium chloride, and then introducing gas containing CO2 to carry out mineralization reaction, and controlling the pH value of the mineralized solution after mineralization to be 7.8-8.0;
[0013] The mineralized liquid is filtered, washed and dried to obtain light calcium carbonate with controllable morphology and particle size;
[0014] Wherein, in the mineralization reaction system, the concentration of calcium chloride is 0.2-0.85 mol / L, the concentration of nano calcium carbonate is 0.0005-0.01 mol / L, and the concentration of ammonia water is 0.2-2.5 mol / L.
[0015] In the present invention, calcium chloride and ammonia water are the main chemical substances for adjusting the crystal form of calcium carbonate, wherein ammonia water is an alkaline solution that can adjust the pH value of the reaction system, and the selection of the crystal form of calcium carbonate is very sensitive to the pH value of the solution. Therefore, by increasing or decreasing the amount of ammonia water added, the pH value of the solution can be changed, thereby affecting the selection of the crystal form of calcium carbonate; and calcium chloride contains chloride ions and calcium ions, which can affect the formation process of the crystal form of calcium carbonate, and different crystal forms have different sensitivities to the concentration of specific ions. By adjusting the concentration of calcium chloride, the formation of the crystal form of calcium carbonate can be regulated.
[0016] Finally, the present invention also introduces nano calcium carbonate, which has relatively small particles and can guide and control the crystal morphology during the growth of calcium carbonate crystals. Therefore, nano calcium carbonate can be used as a template to control the shape and size of calcium carbonate particles.
[0017] The method of the present invention can be used to prepare light calcium carbonate with different morphologies and sizes, wherein the crystal form of the light calcium carbonate includes any one of vaterite, calcite and aragonite, and the morphology of the light calcium carbonate includes any one of spherical, needle-shaped, regular dodecahedral and rose-shaped; and the particle size of the spherical and needle-shaped light calcium carbonate can be controlled within 0.1-3 μm, the particle size of the regular dodecahedral light calcium carbonate can be controlled within 12-15 μm, and the particle size of the rose-shaped light calcium carbonate can be controlled within 8-10 μm.
[0018] In the technical solution of the invention, the gas used can be power plant flue gas or boiler flue gas with low CO2 concentration, or purified high-purity CO2 gas. Specifically, the volume concentration of CO2 in the gas is 6-100%, and the flow rate of the gas is preferably 150-350m 3 / h.
[0019] In addition, during the mineralization reaction, in order to prevent ammonia water from overflowing and reduce the effective concentration of ammonia water, the temperature of the mineralization reaction can be controlled at 10-30°C. Specifically, the temperature of the mineralization reaction can be controlled by circulating cooling water.
[0020] The present invention does not strictly limit the composition form of the solution containing calcium chloride. It can be a calcium chloride solution obtained by the reaction of calcium hydroxide and ammonium chloride, or a filtrate obtained by the ore dissolution reaction of a calcium-containing mineralizable raw material and an ammonium chloride solution. The calcium-containing mineralizable raw material is specifically any one or more of carbide slag, calcium hydroxide, calcium oxide, steel slag, wollastonite, magnesium slag, forsterite, slag and volcanic ash.
[0021] However, the calcium chloride solution used in the present invention is preferably the filtrate obtained after the calcium-containing mineralizable raw material reacts with the ammonium chloride solution. This is because the filtrate obtained from the above reaction contains trace amounts of impurities such as magnesium hydroxide and silicon dioxide, which, to a certain extent, will act as a crystal form controller to participate in the formation of light calcium carbonate with different crystal structures. The specific principle is as follows:
[0022] The influence of raw material impurities on the crystal form of calcium carbonate is due to their interference and substitution in the crystal growth process. The crystal form of calcium carbonate depends on the ion coordination and arrangement in the crystal structure, and the presence of raw material impurities will change the stability and morphology of the crystal structure.
[0023] First, raw material impurities can interfere with the crystal growth process. During the crystal formation process, impurity ions in the raw materials may compete with the components of calcium carbonate crystals for crystallization sites, thereby affecting the formation of crystals. In addition, impurities may also compete with calcium carbonate ions for crystallization sites, resulting in changes in the crystal growth rate, thereby affecting the formation of the crystal form.
[0024] Secondly, raw material impurities can replace ion positions in the crystal. The size, charge, and electron cloud density of impurity ions may be different from those of calcium carbonate ions, and these differences will change the coordination environment and unit cell parameters in the crystal structure. Moreover, this substitution effect will also cause lattice distortion and changes in the crystal structure, thereby affecting the formation of the crystal form.
[0025] In addition, raw material impurities may also form impurity solid solutions in the crystals. If some raw material impurities can form stable solid solutions in calcium carbonate crystals, they will affect the physical properties and structural stability of the crystals. That is, the formation of such solid solutions may change the unit cell parameters, crystal shape and unit cell symmetry, etc., thereby affecting the formation of the crystal form.
[0026] Therefore, the effects of raw material impurities on the crystal form of calcium carbonate include interference with the crystal growth process, ion substitution, and solid solution formation, etc. These effects will change the stability and morphology of the crystal structure, resulting in the formation of different crystal forms.
[0027] The nano calcium carbonate used in the present invention is preferably nano calcium carbonate with a particle size of 20-100 nm. Before use, it is moistened with a small amount of ethanol and then dissolved in water to prepare a nano calcium carbonate solution.
[0028] In addition, the nano calcium carbonate solution of the present invention can also be calcium carbonate obtained by dry grinding and then tested by a laser particle size analyzer with a particle size of 1-2 μm. The calcium carbonate solution obtained by adding water, stirring and dissolving such calcium carbonate is nanometer-sized under a scanning electron microscope.
[0029] Furthermore, the nano-calcium carbonate solution of the present invention can also use the filtrate obtained by filtering the mineralized liquid. This is because during the filtration process, fine calcium carbonate passes through the filter membrane into the filtrate, and this part of the filtrate also appears in nanometer size under a scanning electron microscope.
[0030] In the present invention, when it is necessary to prepare light calcium carbonate with a spherical morphology, a vaterite crystal form and a size of 0.1-3 μm, the concentration of calcium chloride needs to be controlled to be 0.35-0.5 mol / L, the concentration of nano calcium carbonate needs to be controlled to be 0.002-0.005 mol / L, the concentration of ammonia water needs to be controlled to be 0.3 mol / L, and the concentration of CO2 in the gas needs to be controlled to be 8-9%.
[0031] Under this condition, the calcium concentration and ammonia concentration are relatively low, and calcium carbonate can be obtained in a short time. The amount of nano calcium carbonate added is small, and the particle size of calcium carbonate obtained is also small. Therefore, spherical calcium carbonate can be obtained.
[0032] When it is necessary to prepare light calcium carbonate with a needle-shaped morphology, calcite and aragonite crystal forms, and a size of 0.1-3 μm, the concentration of calcium chloride needs to be controlled at 0.2-0.35 mol / L, the concentration of nano calcium carbonate at 0.0005-0.001 mol / L, the concentration of ammonia water at 1.6-1.8 mol / L, and the concentration of CO2 in the gas at 40-45%.
[0033] Under this condition, the calcium concentration is low, while the concentrations of ammonia and carbon dioxide are relatively high, which is conducive to the preferential growth of needle-shaped calcium carbonate. At this time, the concentration of nano-calcium carbonate added is small, so needle-shaped calcium carbonate with a smaller particle size can be obtained.
[0034] When it is necessary to prepare light calcium carbonate with a regular dodecahedral morphology, a vaterite crystal form and a size of 12-15 μm, the concentration of calcium chloride needs to be controlled at 0.5-0.7 mol / L, the concentration of nano calcium carbonate needs to be controlled at 0.008-0.01 mol / L, the concentration of ammonia water needs to be controlled at 1.8-2.0 mol / L, and the concentration of CO2 in the gas needs to be controlled at 70-72%.
[0035] Under this condition, the concentrations of calcium, ammonia and carbon dioxide are all high, which is conducive to the preferential growth of regular dodecahedral calcium carbonate. At the same time, the concentration of nano-calcium carbonate added is relatively high, therefore, the growth of crystals can be promoted.
[0036] When it is necessary to prepare light calcium carbonate with a rose-shaped morphology, a calcite crystal form, and a size of 8-10 μm, the concentration of calcium chloride needs to be controlled at 0.8-0.85 mol / L, the concentration of ammonia water needs to be controlled at 2.2-2.5 mol / L, and the concentration of CO2 in the gas needs to be controlled at 14-15%.
[0037] The calcium carbonate with this morphology is prepared from calcium hydroxide, and the obtained calcium chloride concentration is relatively high. At the same time, because calcium hydroxide contains more Mg 2+ Ions, when calcium extraction is high, magnesium ions will also be extracted in large quantities. Magnesium ions react with carbonate ions to generate different types of carbonate precipitation, thus affecting the formation of calcium carbonate crystals. At the same time, other impurities in calcium hydroxide will also affect the crystallization process of calcium carbonate, thereby affecting the formation of calcium carbonate crystals, so rose-shaped calcium carbonate can be obtained.
[0038] Compared with the prior art, the method for preparing light calcium carbonate with controllable morphology and particle size of the present invention has at least the following technical effects:
[0039] 1. The present invention can obtain stable light calcium carbonate with specific crystal form, morphology and size by controlling the concentration of calcium chloride, the addition amount of nano calcium carbonate and ammonia water, specifically including three crystal forms of vaterite, calcite and aragonite, and four morphologies of spherical, needle-shaped, regular dodecahedral and rose-shaped. Among them, the particle size of spherical and needle-shaped light calcium carbonate can be controlled between 0.1-3μm, the particle size of rose-shaped light calcium carbonate can be controlled between 8-10μm, and the particle size of regular dodecahedral light calcium carbonate can be controlled between 12-15μm;
[0040] 2. The method for preparing light calcium carbonate with controllable morphology and particle size of the present invention does not require the addition of a crystal control agent, and light calcium carbonate with different crystal forms, morphologies and sizes can be obtained. The prepared light calcium carbonate has high purity and whiteness, which significantly increases the added value of light calcium carbonate. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1This is a SEM photo of the spherical light calcium carbonate prepared in Example 1;
[0043] Figure 2 This is a SEM photo of the needle-shaped light calcium carbonate prepared in Example 2;
[0044] Figure 3 This is a SEM photo of the regular dodecahedron-shaped light calcium carbonate prepared in Example 3;
[0045] Figure 4 This is a SEM photo of the rose-shaped light calcium carbonate prepared in Example 4;
[0046] Figure 5 The X-ray diffraction pattern of vaterite light calcium carbonate of Example 1;
[0047] Figure 6 The X-ray diffraction patterns of calcite and aragonite light calcium carbonate of Example 2;
[0048] Figure 7 The X-ray diffraction pattern of vaterite light calcium carbonate of Example 3;
[0049] Figure 8 The X-ray diffraction pattern of the calcite light calcium carbonate of Example 4;
[0050] Fig. 9 This is a SEM photo of spherical light calcium carbonate prepared in Comparative Example 1;
[0051] Fig.10 This is the SEM photo of the needle-shaped light calcium carbonate prepared in Control Example 2. DETAILED DESCRIPTION
[0052] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0053] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0054] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] Example 1
[0056] Preparation of solutions containing calcium chloride
[0057] The industrial solid waste calcium carbide slag is used as raw material. The calcium carbide slag is discharged from the storage bin and enters the ore dissolution reactor through a weighing feeder. The ammonium chloride solution is introduced from the ammonium chloride storage tank into the ore dissolution reactor. The mixture is stirred and reacted at room temperature. The leached calcium chloride and ammonia water mixture enters the ore dissolution liquid sedimentation tank from the bottom of the ore dissolution reactor. Among them, the mass ratio of calcium carbide slag to ammonium chloride is 1:1.6. The amount of calcium carbide slag added is controlled by a weighing feeder, and the amount of ammonium chloride solution added is controlled by a PLC to control the flow rate.
[0058] The carbide slag leaching liquid overflows from the top of the molten liquid settling tank and enters the leaching liquid storage tank. The sediment at the bottom of the molten liquid settling tank is filtered, and the filtrate returns to the molten liquid settling tank. The filter cake is sent to the desulfurization workshop through a belt conveyor.
[0059] Preparation of light calcium carbonate with spherical morphology and vaterite crystal form
[0060] S11. The leaching liquid is introduced into the mineralization device through a metering pump. At the same time, the nano calcium carbonate solution and ammonia water are introduced into the mineralization device through a metering pump in proportion. In the mineralization reaction system, the concentration of calcium chloride is 0.45 mol / L, the concentration of nano calcium carbonate is 0.005 mol / L, and the concentration of ammonia water is 0.3 mol / L. Flue gas is introduced from the bottom of the mineralization device. The CO2 concentration in the flue gas is 8-9%. The flue gas flow rate is 280m 3 / h, the mineralization temperature is controlled at 22°C by circulating cooling water, and the pH value of the mineralized liquid is 8.0 at the end of the mineralization reaction;
[0061] Among them, the nano calcium carbonate is the filtrate after the mineralization liquid is filtered. Since fine calcium carbonate will pass through the filter membrane into the filtrate during the filtration process, the filtrate can be used as a nano calcium carbonate solution.
[0062] S12, after the reaction, the mineralized liquid enters the calcium carbonate precipitation tank from the outlet of the mineralization device, and the mineralized liquid discharge flow rate is 1.5m 3 / h, the sediment at the bottom of the calcium carbonate sedimentation tank is filtered through a plate and frame, washed, and dried to obtain a light calcium carbonate product;
[0063] Among them, part of the filtrate after plate and frame filtration returns to the nano calcium carbonate solution tank and continues to be used as nano calcium carbonate solution, and the remaining part returns to the calcium carbonate sedimentation tank. The clear liquid on the top of the calcium carbonate sedimentation tank flows back to the ammonium chloride storage tank through overflow and is recycled; this mineralization reaction is a continuous operation.
[0064] Depend on Figure 1 and Figure 5 It can be seen that the light calcium carbonate prepared in this embodiment has a spherical morphology and a vaterite crystal form, and its particle size can be controlled to be 0.8-1 μm.
[0065] Example 2
[0066] Preparation of solutions containing calcium chloride
[0067] Taking industrial solid waste magnesium slag as raw material, magnesium slag is discharged from the storage bin, enters the ore dissolution reactor through the weighing feeder, and then the ammonium chloride solution is introduced from the ammonium chloride storage tank into the ore dissolution reactor. The mixture is stirred and reacted at room temperature, and the leached calcium chloride and ammonia water mixture enters the ore dissolution liquid sedimentation tank from the bottom of the ore dissolution reactor; wherein, the mass ratio of magnesium slag to ammonium chloride is 1:1.8, the amount of magnesium slag added is controlled by the weighing feeder, and the amount of ammonium chloride solution added is controlled by the flow control of PLC;
[0068] The leaching liquid overflows from the top of the molten liquid settling tank and enters the leaching liquid storage tank. The sediment at the bottom of the molten liquid settling tank is filtered, and the filtrate returns to the molten liquid settling tank. The filter cake is sent to the desulfurization workshop through a belt conveyor.
[0069] Preparation of light calcium carbonate with needle-shaped morphology and calcite and aragonite crystal forms
[0070] S21, the leaching liquid is introduced into the mineralization device through the metering pump, and at the same time, the nano calcium carbonate solution and ammonia water are introduced into the mineralization device through the metering pump in proportion. In the mineralization reaction system, the concentration of calcium chloride is 0.3 mol / L, the concentration of nano calcium carbonate is 0.001 mol / L, and the concentration of ammonia water is 1.8 mol / L. Flue gas is introduced from the bottom of the mineralization device, the CO2 concentration in the flue gas is 40-45%, and the flue gas flow rate is 250m 3 / h, the mineralization temperature is controlled at 22°C by circulating cooling water, and the pH value of the mineralized liquid is 7.8 at the end of the mineralization reaction;
[0071] The nano calcium carbonate solution is prepared by adding light calcium carbonate obtained by dry grinding into a nano calcium carbonate solution preparation tank, adding a proper amount of water and then stirring, and the obtained nano calcium carbonate solution is pumped into a nano calcium carbonate solution tank for mineralization use.
[0072] S22, after the reaction, the mineralized liquid enters the calcium carbonate precipitation tank from the outlet of the mineralization device, and the mineralized liquid discharge flow rate is 2.2m 3 / h, the sediment at the bottom of the calcium carbonate sedimentation tank is filtered through a plate and frame, washed, and dried to obtain a light calcium carbonate product;
[0073] Among them, the filtrate after plate and frame filtration is returned to the calcium carbonate sedimentation tank, and the clear liquid on the top of the calcium carbonate sedimentation tank is returned to the ammonium chloride storage tank through overflow for recycling; this mineralization reaction is a continuous operation.
[0074] Depend on Figure 2 and Figure 6 It can be seen that the light calcium carbonate prepared in this embodiment has a needle-shaped morphology, and the crystal form is calcite and aragonite, and its particle size can be controlled to be 0.1-1 μm, and the length is 1-3 μm.
[0075] Example 3
[0076] Preparation of solutions containing calcium chloride
[0077] Industrial solid waste steel slag is used as raw material. The steel slag is discharged from the storage bin and enters the ore dissolution reactor through a weighing feeder. The ammonium chloride solution is introduced from the ammonium chloride storage tank into the ore dissolution reactor. The mixture is stirred and reacted at room temperature. The leached calcium chloride and ammonia water mixture enters the ore dissolution liquid sedimentation tank from the bottom of the ore dissolution reactor. Among them, the mass ratio of steel slag to ammonium chloride is 1:1.2. The amount of steel slag added is controlled by a weighing feeder, and the amount of ammonium chloride solution added is controlled by a PLC to control the flow rate.
[0078] The leaching liquid overflows from the top of the molten liquid settling tank and enters the leaching liquid storage tank. The sediment at the bottom of the molten liquid settling tank is filtered, and the filtrate returns to the molten liquid settling tank. The filter cake is sent to the desulfurization workshop through a belt conveyor.
[0079] Preparation of light calcium carbonate with regular dodecahedron morphology and vaterite crystal form
[0080] S31, the leaching liquid is introduced into the mineralization device through the metering pump, and at the same time, the nano calcium carbonate solution and ammonia water are introduced into the mineralization device through the metering pump in proportion. In the mineralization reaction system, the concentration of calcium chloride is 0.5 mol / L, the concentration of nano calcium carbonate is 0.01 mol / L, and the concentration of ammonia water is 2.0 mol / L. Flue gas is introduced from the bottom of the mineralization device, the CO2 concentration in the flue gas is 70-72%, and the flue gas flow rate is 180m 3 / h, the mineralization temperature is controlled at 16°C by circulating cooling water, and the pH value of the mineralized liquid is 8.0 at the end of the mineralization reaction;
[0081] The nano calcium carbonate solution is prepared by using 50nm calcium carbonate, which is moistened with a small amount of ethanol and then dissolved in water to form the nano calcium carbonate solution. The obtained nano calcium carbonate solution is pumped into a nano calcium carbonate solution tank for mineralization.
[0082] S32, after the reaction, the mineralized liquid enters the calcium carbonate precipitation tank from the outlet of the mineralization device, and the discharge flow rate of the mineralized liquid is 2.5m3 / h, the sediment at the bottom of the calcium carbonate sedimentation tank is filtered through a plate and frame, washed, and dried to obtain a light calcium carbonate product;
[0083] Among them, the filtrate after plate and frame filtration is returned to the calcium carbonate sedimentation tank, and the clear liquid on the top of the calcium carbonate sedimentation tank is returned to the ammonium chloride storage tank through overflow for recycling; this mineralization reaction is a continuous operation.
[0084] Depend on Figure 3 and Figure 7 It can be seen that the light calcium carbonate prepared in this embodiment has a regular dodecahedron morphology and a vaterite crystal form, and its particle size can be controlled to be 12-15 μm.
[0085] Example 4
[0086] Preparation of solutions containing calcium chloride
[0087] Calcium hydroxide is used as the raw material. Calcium hydroxide is discharged from the storage bin and enters the ore dissolution reactor through the weighing feeder. The ammonium chloride solution is introduced from the ammonium chloride storage tank into the ore dissolution reactor. The mixture is stirred and reacted at room temperature. The leached calcium chloride and ammonia water mixture enters the ore dissolution liquid sedimentation tank from the bottom of the ore dissolution reactor. Among them, the mass ratio of calcium hydroxide to ammonium chloride is 1:1.7. The addition amount of calcium hydroxide is controlled by the weighing feeder, and the addition amount of ammonium chloride solution is controlled by the flow rate controlled by PLC.
[0088] The leaching liquid overflows from the top of the molten liquid settling tank and enters the leaching liquid storage tank. The sediment at the bottom of the molten liquid settling tank is filtered, and the filtrate returns to the molten liquid settling tank. The filter cake is sent to the desulfurization workshop through a belt conveyor.
[0089] Preparation of light calcium carbonate with rose-shaped morphology and calcite crystal form
[0090] S41, the leaching solution is introduced into the mineralization device through the metering pump, and at the same time, calcium chloride, nano calcium carbonate solution and ammonia water are introduced into the mineralization device through the metering pump in proportion. In the mineralization reaction system, the concentration of calcium chloride is 0.82 mol / L and the concentration of ammonia water is 2.5 mol / L. Flue gas is introduced from the bottom of the mineralization device, the CO2 concentration in the flue gas is 14-15%, and the flue gas flow rate is 330m 3 / h, the mineralization temperature is controlled at 28°C by circulating cooling water, and the pH value of the mineralized liquid is 7.8 at the end of the mineralization reaction;
[0091] S42, after the reaction, the mineralized liquid enters the calcium carbonate precipitation tank from the outlet of the mineralization device, and the discharge flow rate of the mineralized liquid is 2.0m 3 / h, the sediment at the bottom of the calcium carbonate sedimentation tank is filtered through a plate and frame, washed, and dried to obtain a light calcium carbonate product;
[0092] The filtrate after plate and frame filtration is returned to the mineralization reactor. Nano-scale calcium carbonate exists in the filtrate and is used as calcium carbonate seed. The flow rate of the solution entering the mineralization reactor is 0.2m 3 / h, the clear liquid on the top of the calcium carbonate sedimentation tank flows back to the ammonium chloride storage tank through overflow and is recycled; this mineralization reaction is a continuous operation.
[0093] Depend on Figure 4 and Figure 8 It can be seen that the light calcium carbonate prepared in this embodiment has a rose-shaped morphology and a calcite crystal form, and its particle size can be controlled to be 8-10 μm.
[0094] Example 5
[0095] In the mineralization reaction system, the concentration of calcium chloride is 0.35 mol / L, the concentration of nano calcium carbonate is 0.002 mol / L, and the concentration of ammonia water is 0.4 mol / L;
[0096] The other steps and parameters are basically the same as those in Example 1.
[0097] Example 6
[0098] In the mineralization reaction system, the concentration of calcium chloride is 0.5 mol / L, the concentration of nano calcium carbonate is 0.003 mol / L, and the concentration of ammonia water is 0.35 mol / L;
[0099] The other steps and parameters are basically the same as those in Example 1.
[0100] Example 7
[0101] In the mineralization reaction system, the concentration of calcium chloride is 0.2 mol / L, the concentration of nano calcium carbonate is 0.0005 mol / L, and the concentration of ammonia water is 1.6 mol / L;
[0102] The other steps and parameters are basically the same as those in Example 2.
[0103] Example 8
[0104] In the mineralization reaction system, the concentration of calcium chloride is 0.35 mol / L, the concentration of nano calcium carbonate is 0.0009 mol / L, and the concentration of ammonia water is 1.75 mol / L;
[0105] The other steps and parameters are basically the same as those in Example 2.
[0106] Example 9
[0107] In the mineralization reaction system, the concentration of calcium chloride is 0.55 mol / L, the concentration of nano calcium carbonate is 0.008 mol / L, and the concentration of ammonia water is 1.8 mol / L;
[0108] The other steps and parameters are basically the same as those in Example 3.
[0109] Example 10
[0110] In the mineralization reaction system, the concentration of calcium chloride is 0.7 mol / L, the concentration of nano calcium carbonate is 0.0095 mol / L, and the concentration of ammonia water is 1.95 mol / L;
[0111] The other steps and parameters are basically the same as those in Example 3.
[0112] Embodiment 11
[0113] In the mineralization reaction system, the concentration of calcium chloride is 0.85 mol / L and the concentration of ammonia water is 2.3 mol / L;
[0114] The other steps and parameters are basically the same as those in Example 4.
[0115] Example 12
[0116] In the mineralization reaction system, the concentration of calcium chloride is 0.84 mol / L and the concentration of ammonia water is 2.4 mol / L;
[0117] The other steps and parameters are basically the same as those in Example 4.
[0118] Comparative Example 1
[0119] In the mineralization reaction system, the concentration of calcium chloride is 0.3 mol / L, the concentration of nano calcium carbonate is 0.001 mol / L, and the concentration of ammonia water is 0.5 mol / L;
[0120] The other steps and parameters are basically the same as those in Example 1.
[0121] Depend on Fig. 9 It can be seen that although the morphology and crystal form of the light calcium carbonate prepared in this comparative example are spherical and vaterite, respectively, the crystal form distribution is uneven and the size is also uneven.
[0122] Comparative Example 2
[0123] In the mineralization reaction system, the concentration of calcium chloride is 0.6 mol / L, the concentration of nano calcium carbonate is 0.006 mol / L, and the concentration of ammonia water is 0.2 mol / L;
[0124] The other steps and parameters are basically the same as those in Example 1.
[0125] Comparative Example 3
[0126] In the mineralization reaction system, the concentration of calcium chloride is 0.55 mol / L, the concentration of nano calcium carbonate is 0.006 mol / L, and the concentration of ammonia water is 0.2 mol / L;
[0127] The other steps and parameters are basically the same as those in Example 1.
[0128] Comparative Example 4
[0129] In the mineralization reaction system, the concentration of calcium chloride is 0.1 mol / L, the concentration of nano calcium carbonate is 0.0003 mol / L, and the concentration of ammonia water is 1.9 mol / L;
[0130] The other steps and parameters are basically the same as those in Example 2.
[0131] Depend on Fig.10 It can be seen that the light calcium carbonate prepared in this comparative example is needle-shaped, with a particle size of 0.1-0.5 μm and a length of 0.2-2 μm, but 10-20% is in the form of flakes or cubic crystals.
[0132] Comparative Example 5
[0133] In the mineralization reaction system, the concentration of calcium chloride is 0.4 mol / L, the concentration of nano calcium carbonate is 0.002 mol / L, and the concentration of ammonia water is 1.5 mol / L;
[0134] The other steps and parameters are basically the same as those in Example 2.
[0135] Comparative Example 6
[0136] In the mineralization reaction system, the concentration of calcium chloride is 0.4 mol / L, the concentration of nano calcium carbonate is 0.0004 mol / L, and the concentration of ammonia water is 1.5 mol / L;
[0137] The other steps and parameters are basically the same as those in Example 2.
[0138] Comparative Example 7
[0139] In the mineralization reaction system, the concentration of calcium chloride is 0.4 mol / L, the concentration of nano calcium carbonate is 0.007 mol / L, and the concentration of ammonia water is 2.1 mol / L;
[0140] The other steps and parameters are basically the same as those in Example 3.
[0141] Comparative Example 8
[0142] In the mineralization reaction system, the concentration of calcium chloride is 0.8 mol / L, the concentration of nano calcium carbonate is 0.01 mol / L, and the concentration of ammonia water is 1.7 mol / L;
[0143] The other steps and parameters are basically the same as those in Example 3.
[0144] Comparative Example 9
[0145] In the mineralization reaction system, the concentration of calcium chloride is 0.8 mol / L, the concentration of nano calcium carbonate is 0.006 mol / L, and the concentration of ammonia water is 1.7 mol / L;
[0146] The other steps and parameters are basically the same as those in Example 3.
[0147] Comparative Example 10
[0148] In the mineralization reaction system, the concentration of calcium chloride is 0.7 mol / L and the concentration of ammonia water is 2.0 mol / L;
[0149] The other steps and parameters are basically the same as those in Example 4.
[0150] Comparative Example 11
[0151] In the mineralization reaction system, the concentration of calcium chloride is 0.9 mol / L and the concentration of ammonia water is 2.6 mol / L;
[0152] The other steps and parameters are basically the same as those in Example 4.
[0153] Comparative Example 12
[0154] In the mineralization reaction system, the concentration of calcium chloride is 1.0 mol / L and the concentration of ammonia water is 2.0 mol / L;
[0155] The other steps and parameters are basically the same as those in Example 4.
[0156] Comparative Example 13
[0157] Calcium carbonate is prepared by using a preparation process for carbonizing spherical calcium carbonate using calcium chloride and ammonia solution disclosed in patent CN 112142087 A. The specific steps are as follows:
[0158] (1) Preparation of calcium chloride and ammonia solution: Calcium hydroxide and water at room temperature are fully stirred and dissolved in a mass ratio of 1:4, and ammonium chloride is added in an amount of 1:2.05 in a molar ratio of calcium hydroxide to ammonium chloride, and fully stirred and dissolved, i.e., ammonium chloride is slightly excessive. After sufficient reaction, the obtained calcium chloride and ammonia solution is filtered to remove insoluble matter and impurities to obtain a clear solution, and methanol is added to adjust the calcium chloride concentration to 10%, and the amount of methanol added is 40% of the mass of the prepared calcium chloride and ammonia solution;
[0159] (2) Adding a crystal morphology control agent: Use a pump to pump the calcium chloride and ammonia solution with adjusted concentrations into an intermittent bubbling carbonization tower equipped with a stirring device, add 1.2% polyaluminium sulfate as a crystal morphology control agent by weight of calcium chloride and stir evenly;
[0160] (3) Carbonization: The temperature of the calcium chloride and ammonia solution was adjusted to 20°C, and a mixed gas containing 42% CO2 by volume was introduced to carry out a carbonization reaction. The temperature was not controlled during the reaction process. When the pH of the reaction solution reached 7.8, the gas valve was closed to stop the reaction.
[0161] (4) Dehydration and drying: The calcium carbonate slurry obtained by the carbonization reaction is subjected to processes such as dehydration, washing, drying, crushing, and screening to obtain regular spherical calcium carbonate with a particle size of 450 nanometers. The ammonium chloride solution obtained by dehydration and washing can be recycled for the dissolution reaction of calcium hydroxide to prepare calcium chloride and ammonia solution after precipitation and purification.
[0162] Comparative Example 14
[0163] Calcium carbonate is prepared by using a method for preparing vaterite-type calcium carbonate powder disclosed in patent CN 103553108 A.
[0164] (1) adding 7.5 g of calcium chloride powder into a beaker containing 92.5 g of distilled water, stirring to fully react or dissolve, to obtain a calcium chloride aqueous solution with a concentration of 7.5%;
[0165] (2) adding 13.26 g of aqueous ammonia to a beaker containing an aqueous solution of calcium chloride and stirring to mix thoroughly to obtain a mixed solution having a pH value of 11.2;
[0166] (3) CO2 gas is introduced into the alkaline solution through a gas microporous diffuser to gradually generate calcium carbonate precipitate. Samples are taken within 1-2 minutes after the precipitate is generated, and samples are taken every 10 minutes thereafter. XRD detection is performed on the obtained samples, and the results show that the calcite phase is obtained when the precipitate is just generated, and the vaterite phase is obtained later. At the end of the reaction, the vaterite phase calcium carbonate powder with a negligible calcite content is obtained;
[0167] (4) Due to Ca 2+ The concentration of Ca decreases with the formation of precipitation, so the following conclusions can be drawn: 2+ When the concentration is high, calcite phase is generated. 2+ When the concentration is low, vaterite phase is generated. In order to prove this conclusion, calcium chloride solutions with mass concentrations of 10.5, 4.5 and 1.5% were selected for carbonization. The results showed that the content of vaterite increased with the increase of Ca 2+ The decrease in concentration gradually increases;
[0168] (5) When the concentration of calcium chloride solution is low, pure vaterite phase calcium carbonate powder can be obtained by carbonization.
[0169] Comparative Example 15
[0170] Using patent CN 116375069 A
[0171] Take 1kg of semi-dry desulfurization ash from a steel plant, the particle size is less than 200 mesh, and its chemical composition is 35.2wt.% calcium sulfite, 23.6wt.% calcium sulfate, 28.3wt.% calcium oxide, 5.5wt.% calcium chloride and 7.4wt.% calcium hydroxide;
[0172] The semi-dry desulfurization ash is leached in water according to a solid-liquid mass ratio of 1:1, and the leaching reaction is carried out at room temperature. The leaching stirring rate is 1200r / min, and the leaching time is 30min, to obtain a leaching solution containing calcium chloride and calcium hydroxide, and a leaching residue containing calcium sulfite and calcium sulfate;
[0173] In the ultrasonic field (ultrasonic power of 500W), carbon dioxide is introduced into the leachate, and the carbon dioxide is dispersed into uniform bubbles of 100nm in size through the gas disc stone. After entering the solution and adjusting the pH of the solution to 6.5, a certain amount of ammonia water is added, and the ammonia water is fed according to the molar concentration ratio of ammonium ions to calcium ions in the leachate of 2:1 to adjust the filtrate; then carbon dioxide is introduced for curing reaction, the carbon dioxide content is 5vol.%, the carbon dioxide flow rate is 0.3L / min, and the average size of carbon dioxide bubbles is 100nm; the curing reaction is carried out in the ultrasonic field, the ultrasonic power is 500W, and the heating treatment is carried out during the ultrasonic process to maintain the filtrate temperature at 40°C, and the curing time is 30min;
[0174] After the solidification reaction is completed, the solution containing vaterite calcium carbonate is separated by centrifugation to obtain solid phase vaterite calcium carbonate and ammonium chloride solution. The solid product is dried at 60°C for 5 hours to obtain a vaterite calcium carbonate product, and the ammonium chloride solution is evaporated and crystallized, and then dried at 60°C for 5 hours to obtain an ammonium chloride product.
[0175] The final product vaterite calcium carbonate has a purity of 86%, an ammonium chloride conversion rate of 94%, and an ammonium sulfate conversion rate of 90%.
[0176] In order to study the quality of the calcium carbonate prepared in the above embodiments and control examples, the present invention tested the purity of the obtained calcium carbonate, and the testing method is as follows:
[0177] The determination method is 3.3 of GB / T19281-2014 calcium carbonate analysis method.
[0178] The specific analysis steps are as follows:
[0179] 1) Preparation of test solution
[0180] Weigh 0.6g of the sample that has been dried to a constant mass at 105℃±2℃ in advance, accurate to 0.0002g, and place it in a 250mL beaker, add a little water (a little anhydrous ethanol for activated calcium carbonate products) to moisten it, cover it with a watch glass, and drip hydrochloric acid solution along the mouth of the cup until the sample is completely dissolved, filter it with medium-speed filter paper, wash it thoroughly with water, collect the filtrate and washing liquid in a 250mL (V1) volumetric flask, dilute it to the scale with water, and shake it well. This solution is the test solution A. It is used for the determination of calcium and magnesium content.
[0181] 2) Determination
[0182] Use a pipette to transfer 25mL (V2) of test solution A into a 250mL conical flask, add 5mL triethanolamine solution, 25mL water and a small amount of calcium reagent sodium carboxylate indicator, adjust to wine red with sodium hydroxide solution, and add 0.5mL in excess, and titrate with disodium ethylenediaminetetraacetic acid standard titration solution until pure blue is the end point. Perform a blank test at the same time.
[0183] After testing, the purity of the obtained calcium carbonate is shown in Table 1.
[0184] Table 1 Calcium carbonate purity
[0185]
[0186]
[0187] It can be seen from Examples 1-12 that the present invention can obtain stable light calcium carbonate with specific crystal forms, morphologies and sizes by controlling the concentration of calcium chloride, the addition amounts of nano-calcium carbonate and ammonia water, specifically including three crystal forms of vaterite, calcite and aragonite, and four morphologies of spherical, needle-shaped, regular dodecahedral and rose-shaped. Among them, the particle size of spherical and needle-shaped light calcium carbonate can be controlled between 0.1-3 μm, the particle size of rose-shaped light calcium carbonate can be controlled between 8-10 μm, and the particle size of regular dodecahedral light calcium carbonate can be controlled between 12-15 μm.
[0188] When the reaction conditions in Comparative Examples 1-12 were changed, the crystal form and size of light calcium carbonate were adversely affected.
[0189] Although reference example 13 is also to prepare calcium carbonate by the main reaction of calcium chloride, ammonia and carbon dioxide, it needs to add methanol condition reaction system concentration in the preparation process, and needs to add crystal morphology control agent, can obtain spherical calcium carbonate with uniform particle size and complete spherical shape. Its embodiment part also obviously illustrates that if methanol and crystal morphology control agent are not added, the particle size of the obtained calcium carbonate is very large, and can't be controlled, and the vaterite crystal form calcium carbonate particle of the obtained is unstable and easily converted into cubic crystal form calcium carbonate.
[0190] Comparative Example 14 also prepares calcium carbonate by the main reaction of calcium chloride, ammonia and carbon dioxide, but its research shows that in Ca 2+ When the concentration is high, calcite phase is generated. 2+ When the concentration is low, vaterite phase is generated, and in the presence of Ca 2+ When the concentration is high, the calcite phase generated is unstable. As the reaction proceeds, Ca 2+ As the concentration decreases, vaterite phase calcium carbonate powder with negligible calcite content is finally obtained. It has been verified experimentally that in control example 14, as the stirring time increases, the calcite changes from an initial small amount to a large amount. Vaterite is unstable under this condition and transforms into stable calcite. Whether calcium carbonate is in vaterite phase or calcite phase is not determined solely by the calcium ion concentration, but also by the amount of ammonia added and the carbon dioxide concentration.
[0191] Comparative Example 15 is to soak the semi-dry desulfurization ash in water and leach it at room temperature to obtain a leachate containing calcium chloride and calcium hydroxide. Since the solubility of calcium hydroxide is very low, the leachate is mainly calcium chloride, and the utilization rate of 28.3% of calcium oxide and 7.4% of calcium hydroxide in the raw material is less than 5%, resulting in great waste. At the same time, carbon dioxide is first introduced into the leachate, and the solution pH is adjusted to 6.5. At this time, the calcium exists in the form of calcium bicarbonate and a small amount of calcium carbonate. At this time, the calcium carbonate produced is prone to agglomeration, which in turn affects the particle size and crystal form of the generated calcium carbonate; ammonia water and CO2 gas are added again in the later stage, although calcium carbonate will be generated, a large amount of calcium bicarbonate is coated by calcium carbonate, which affects the purity and whiteness of the generated calcium carbonate. Finally, due to the secondary introduction of CO2, the pH value of the solution changes greatly, and the generated calcium carbonate has a variety of crystal forms, and agglomeration is serious.
[0192] In summary, the present invention can not only obtain light calcium carbonate with specific crystal form, morphology and size, but also each crystal form prepared has regular morphology, excellent dispersibility, high purity and whiteness, which meets the high requirements of high-end products for light calcium carbonate. Among them, spherical calcium carbonate has good air permeability. In high-end cigarette paper, adding spherical calcium carbonate prepared by this method can improve the combustion performance and air permeability compared with calcite calcium carbonate; needle-bar type light calcium carbonate has the characteristics of washability and high stability. In high-end book paper, adding needle-bar type light calcium carbonate prepared by this method can improve paper strength and opacity, reduce cutter wear, improve paper printing adaptability, and be more ductile than the currently used heavy calcium carbonate; rose-shaped light calcium carbonate has a large specific surface area, has the characteristics of large oil absorption, good transparency and high stability. In the printing ink industry, adding this method to prepare ultrafine calcium carbonate can significantly improve ink adhesion, reduce mechanical wear, reduce costs and increase volume. Regular dodecahedral light calcium carbonate can improve the mechanical properties of the matrix material. In the ceramic manufacturing industry, adding regular dodecahedral light calcium carbonate can effectively improve the fluidity and processing performance of the system, and can also improve the surface finish and filling performance of ceramic products.
[0193] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing light calcium carbonate with controllable morphology and particle size, characterized in that: The following steps are involved: S1, adding ammonia water and nano calcium carbonate solution to a solution containing calcium chloride, and then introducing a gas containing CO2 to carry out a mineralization reaction, and controlling the pH value of the mineralized solution after mineralization to be 7.8-8.0; S2, filtering, washing and drying the mineralized liquid to obtain light calcium carbonate with controllable morphology and particle size; During the mineralization reaction, the concentration of calcium chloride is controlled to be 0.5-0.7 mol / L, the concentration of nano calcium carbonate is controlled to be 0.008-0.01 mol / L, the concentration of ammonia water is controlled to be 1.8-2.0 mol / L, and the volume concentration of CO2 in the gas is controlled to be 70-72%, and light calcium carbonate with a regular dodecahedral morphology, a vaterite crystal form, and a size of 12-15 μm is obtained; During the mineralization reaction, the concentration of calcium chloride is controlled to be 0.8-0.85 mol / L, the concentration of nano calcium carbonate is 0.0005-0.01 mol / L, the concentration of ammonia water is 2.2-2.5 mol / L, and the volume concentration of CO2 in the gas is 14-15%, and light calcium carbonate with a rose-shaped morphology, a calcite crystal form, and a size of 8-10 μm is obtained.
2. The method for preparing light calcium carbonate with controllable morphology and particle size according to claim 1, characterized in that: The flow rate of the CO2-containing gas is 150-350m 3 / h.
3. The method for preparing light calcium carbonate with controllable morphology and particle size according to claim 1, characterized in that: During the mineralization reaction, the temperature is controlled at 10-30°C.
4. The method for preparing light calcium carbonate with controllable morphology and particle size according to claim 1, characterized in that: The solution containing calcium chloride is the filtrate obtained after the calcium-containing mineralizable raw material and the ammonium chloride solution undergo a ore dissolution reaction; The calcium-containing mineralizable raw material is any one or more of carbide slag, calcium hydroxide, calcium oxide, steel slag, wollastonite, magnesium slag, forsterite, slag and volcanic ash.
Citation Information
Patent Citations
Method for preparing rosette-like precipitated calcium carbonate
CN105800657A
Rodlike aragonite calcium carbonate preparation method
CN106430272A
Method for preparation of regular cubic light calcium carbonate from carbide slag
CN110775994A
Preparation process for preparing regular spherical calcium carbonate through calcium chloride and ammonia water solution carbonization method
CN112142087A
Method for preparing nano vaterite calcium carbonate by using CO2 mineralized carbide slag