A kind of high temperature resistant mullite brick prepared by using aluminum slag and preparation method thereof

By compounding and modifying aluminum ash with other materials, combined with molding and gradient heating sintering processes, the problem of converting aluminum ash into high-performance mullite bricks is solved, and waste recycling and performance improvement are achieved. .

CN118479868BActive Publication Date: 2024-10-22洛阳智源再生资源有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410949276.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-22
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively convert aluminum waste aluminum ash into mullite bricks with good flexural resistance, alkali erosion resistance and thermal shock resistance, and there are environmental pollution problems.

Method used

By compounding aluminum slag powder with silicon powder, fused white corundum fine powder and α-Al2O3 fine powder, and sintering in a nitrogen environment, β-SiAlON powder is formed, combined with modified hollow glass microspheres and porous silicate , using compression molding and gradient temperature sintering processes to prepare high-temperature resistant mullite bricks with a core-shell structure.

Benefits of technology

The high-temperature performance of aluminum ash has been improved, and mullite bricks with high flexural resistance, strong alkali erosion resistance, and good thermal shock resistance have been prepared. The process can reduce costs and realize waste recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of mullite bricks, and in particular to a high-temperature resistant mullite brick prepared by using aluminum slag and a preparation method thereof. Aluminum ash slag is used as a raw material, aluminum ash slag powder is compounded with silicon powder, fused white corundum fine powder and α-Al2O3 micropowder, and sintered in a nitrogen atmosphere to form β-SiAlON powder on the surface of the aluminum ash slag powder; hollow glass microbeads are sequentially treated with a NaOH solution and dopamine hydrochloride to obtain dopamine-modified hollow glass microbeads, and then the hollow glass microbeads are electrostatically self-assembled with graphene oxide to obtain graphene oxide-coated hollow glass microbeads; a high-elasticity aerogel is prepared as a skeleton of the mullite brick by combining a sol-gel method and normal pressure drying, and amino polydimethylsiloxane is introduced to make it amino; porous silicate, sodium silicate and potassium silicate are compounded as a binder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mullite bricks, in particular to a high-temperature resistant mullite brick prepared by using aluminum slag and a preparation method thereof. Background Art

[0002] With the progress of society, aluminum products are more and more widely used in people's lives, and the production technology of aluminum products is constantly developing. As a result, the amount of aluminum solid waste increases year by year. Simply discarding or burying it will cause pollution to the environment. How to recycle aluminum ash and aluminum ash slag to achieve sustainable development is a research hotspot in this field.

[0003] Mullite bricks are high-alumina refractory bricks with mullite as the main crystal phase. They are the most widely used refractory materials. How to transform aluminum waste aluminum ash slag into mullite bricks with good flexural resistance, alkali corrosion resistance and good thermal shock resistance, so as to turn waste into treasure and reduce costs and increase efficiency, has always been a focus of attention in this field. Summary of the invention

[0004] The object of the present invention is to provide a high temperature resistant mullite brick prepared by using aluminum slag and a preparation method thereof, so as to solve the problems in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing a high temperature resistant mullite brick using aluminum slag comprises the following steps:

[0007] S1: washing, crushing, grinding and sieving the aluminum ash slag to obtain aluminum ash slag powder, compounding the aluminum ash slag powder, silicon powder, fused white corundum fine powder and α-Al2O3 micro powder, and sintering with nitrogen to obtain mixed aluminum ash slag powder;

[0008] S2: dividing the composite silicate into composite silicate A and composite silicate B according to a mass ratio of 9:1, and mixing the composite silicate B with deionized water to obtain a diluted composite silicate;

[0009] S3: Add composite hollow glass microspheres and mixed aluminum ash slag powder, composite silicate A and auxiliary agent mixture, let stand, add diluted composite silicate secondary mixture to keep the moisture content at 2.5-3.2%, mold, gradually increase the temperature and keep warm to obtain a green body, sinter, and obtain a high temperature resistant mullite brick prepared using aluminum slag.

[0010] Furthermore, the size of the aluminum ash powder is 200 µm.

[0011] Furthermore, the mass ratio of aluminum ash slag powder, silicon powder, fused white corundum fine powder and α-Al2O3 fine powder in the mixed aluminum ash slag powder is 4:3.3:1:1.

[0012] Furthermore, the auxiliary agent is one of calcium carbonate, calcium oxide and magnesium oxide.

[0013] Furthermore, the working conditions of the compression molding are: pressure of 2-4 MPa, time of 1-5 min.

[0014] Furthermore, the working conditions of the gradient heating and heat preservation are: 2℃·min -1 Heat to 70-80℃ and keep warm for 22-24h at 4℃·min -1 Raise the temperature to 120-140℃ and keep warm for 44-48h.

[0015] Furthermore, the working conditions of nitrogen sintering in step S1 are: keeping warm at 1400-1450° C. for 9-10 hours in a nitrogen environment; and the working conditions of sintering in step S3 are: keeping warm at 1600-1650° C. for 6-8 hours.

[0016] Furthermore, the composition of the blank is, by weight: 20-22 parts of mixed aluminum ash slag powder, 12-15 parts of additives, 1-5 parts of composite hollow glass microspheres, and 3-8 parts of composite silicate.

[0017] Furthermore, the preparation of the composite hollow glass microspheres comprises the following steps:

[0018] (1) Soaking the hollow glass microspheres in a NaOH solution for 2 hours, filtering and drying to obtain hydroxylated glass microspheres; mixing Tris buffer and dopamine hydrochloride, adding hydroxylated glass microspheres, ultrasonically dispersing for 1-2 hours, stirring at 18-25° C. for 10-12 hours, centrifuging, washing with water, and drying to obtain modified glass microspheres;

[0019] (2) Mixing the modified glass microspheres and distilled water, adding graphene oxide, adjusting the pH to 4, stirring for 1 hour, standing for 2 hours, centrifuging, washing, and drying to obtain graphene oxide-coated glass microspheres;

[0020] (3) Mixing graphene oxide coated glass microbeads and deionized water, adding a mixture of carbon nanotubes and deionized water, ultrasonically stirring, adding L-ascorbic acid and sodium carboxymethyl cellulose, ultrasonically stirring for 1-2 hours, adding a mixture of amino polydimethylsiloxane and n-hexane, ultrasonically stirring, keeping warm at 95-100°C for 9-10 hours, naturally cooling to 18-25°C, transferring to -18°C for freeze-thawing for 2 hours, repeating the operation 2-3 times, heating to 75-80°C for 3 hours, washing with deionized water, replacing the deionized water with anhydrous ethanol, and drying to obtain composite hollow glass microbeads.

[0021] Further, the preparation of the composite silicate comprises the following steps:

[0022] 1) Mix aluminum nitrate nonahydrate, cerium chloride and deionized water, add a mixture of iminodiacetic acid and N,N-dimethylformamide, keep warm at 145-150°C for 4-5 hours, cool, add tetraethyl silicate, keep warm at 145-150°C for 44-48 hours, rinse with N,N-dimethylformamide and deionized water for 3-5 times, dry, grind, heat to 550°C and keep warm for 5-6 hours to obtain an intermediate powder;

[0023] 2) Mix the intermediate powder and ammonium nitrate solution, keep the mixture at 115-120°C for 9-10 hours, wash and dry, and heat to 550°C for 5-6 hours to obtain porous silicate;

[0024] 3) Compounding porous silicate, sodium silicate and potassium silicate in a mass ratio of 1:2:1 to obtain composite silicate.

[0025] Beneficial effects of the present invention:

[0026] The invention provides a high temperature resistant mullite brick prepared by using aluminum slag and a preparation method thereof. The aluminum ash slag is used as a raw material to prepare the high temperature resistant mullite brick with high bending resistance, good alkali corrosion resistance and high thermal shock resistance.

[0027] The invention uses aluminum ash slag as raw material, crushes and sieves, and aims at the problem that the existing aluminum ash slag has complex components. In the invention, aluminum ash slag powder is compounded with silicon powder, electric fused white corundum fine powder and α-Al2O3 micropowder, and sintered in a nitrogen atmosphere to form β-SiAlON powder on the surface of the aluminum ash slag powder to achieve a core-shell structure, and shield and wrap low melting point components in the aluminum ash slag on the microstructure, thereby greatly improving the high temperature resistance of the aluminum ash slag, so that the sintered aluminum ash slag can be granulated, has high strength, and does not generate gas during the re-burning process, thereby realizing the transformation of waste into treasure.

[0028] Hollow glass microspheres are glassy, ​​transparent hollow spheres filled with rarefied nitrogen or inert gas. In the present invention, hollow glass microspheres are used as filling materials and pore-forming agents to prepare high-temperature resistant mullite bricks, giving the mullite bricks properties such as light weight, high strength, low thermal conductivity, and sound insulation. However, directly adding hollow glass microspheres has compatibility problems with the mullite brick base material. In order to improve the uniformity of the dispersion of hollow glass microspheres in mullite bricks, the present invention modifies the hollow glass microspheres.

[0029] In order to improve the dispersibility and high temperature resistance of hollow glass microspheres, the present invention uses graphene oxide to coat the surface of the hollow glass microspheres. Because the hollow glass microspheres are inert to reaction, the hollow glass microspheres are first treated with a NaOH solution and dopamine hydrochloride in sequence to obtain dopamine-modified hollow glass microspheres, and then the hollow glass microspheres are electrostatically self-assembled with graphene oxide to obtain graphene oxide-coated hollow glass microspheres. On the one hand, the agglomeration of the hollow glass microspheres is suppressed by the graphene oxide, and on the other hand, the mutual stacking of graphene oxide sheets is suppressed by the hollow glass microspheres.

[0030] In order to further improve the flexural resistance of mullite bricks, the present invention further performs aerogel treatment on the graphene oxide-coated hollow glass microspheres, prepares high-elasticity aerogel by combining the sol-gel method and normal pressure drying, prepares high specific surface area aerogel using three-dimensional mesh graphene oxide and multi-walled carbon nanotubes on the graphene oxide-coated hollow glass microspheres as the skeleton of the mullite brick, introduces amino polydimethylsiloxane to make it amino, improves the compatibility of the aerogel and the base material, thereby further improving the flexural resistance and thermal shock resistance of the mullite brick.

[0031] The invention adds auxiliary agents to improve the performance of the bricks. The composite hollow glass microspheres are used as pore-forming agents, composite silicates are used as binders, and high-temperature resistant mullite bricks are prepared by compression molding and sintering.

[0032] Traditional inorganic silicates use water as the main dispersant, which causes them to shrink greatly during the solidification process, easily crack and have poor corrosion resistance. Porous silicates, sodium silicate and potassium silicate are compounded as binders to solve the problem of large brittleness of potassium silicate and sodium silicate after solidification. Aluminum nitrate nonahydrate, cerium chloride and organic ligand iminodiacetic acid are used to synthesize aluminum cerium bimetallic organic framework as a template, and silicate is used as a skeleton to synthesize porous aluminum cerium silicate. Its unique configuration changes the particle grading of mullite bricks, thereby effectively improving the density of the bricks. The high reactivity of porous aluminum cerium silicate effectively promotes the densification of mullite bricks. Its higher unit surface area helps to improve the plasticity of molding, activate the formation of mullite, and improve the various properties of mullite bricks. At the same time, cerium ions enter the corundum-mullite lattice during sintering, effectively improving the high-temperature flexural resistance of mullite bricks. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] It should be noted that if the embodiments of the present invention involve directional indications such as up, down, left, right, front, and back, the directional indication is only used to explain a specific posture such as the relative position relationship between the components, the movement status, etc. If the specific posture changes, the directional indication will also change accordingly. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.

[0035] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0036] Embodiment 1: A method for preparing a high temperature resistant mullite brick using aluminum slag, comprising the following steps:

[0037] S1: washing, crushing, grinding and sieving the aluminum ash slag to obtain aluminum ash slag powder, compounding the aluminum ash slag powder, silicon powder, fused white corundum fine powder and α-Al2O3 micro powder, and sintering with nitrogen to obtain mixed aluminum ash slag powder;

[0038] The mass ratio of aluminum ash powder, silicon powder, fused white corundum fine powder and α-Al2O3 micro powder is 4:3.3:1:1; the working conditions of nitrogen sintering are: in nitrogen environment, keep warm at 1400℃ for 10h;

[0039] S2: dividing the composite silicate into composite silicate A and composite silicate B according to a mass ratio of 9:1, and mixing the composite silicate B with deionized water to obtain a diluted composite silicate;

[0040] S3: adding composite hollow glass microspheres and mixed aluminum ash slag powder to composite silicate A and additive mixture, standing, adding diluted composite silicate secondary mixture, keeping the moisture content at 2.5%, molding, gradient heating and heat preservation, obtaining a green body, sintering, and obtaining a high temperature resistant mullite brick prepared using aluminum slag;

[0041] The auxiliary agent is calcium carbonate; the working conditions of compression molding are: pressure 2MPa, time 5min;

[0042] The working conditions of gradient heating and heat preservation are: 2℃·min -1 Heat to 70℃ and keep warm for 24h at 4℃·min -1 Heat to 120℃ and keep warm for 48h;

[0043] The sintering working conditions are: keeping at 1600℃ for 8h;

[0044] In terms of weight, the composition of the blank is: 20 parts of mixed aluminum ash slag powder, 12 parts of additives, 1 part of composite hollow glass microspheres, and 3 parts of composite silicate;

[0045] The preparation of composite hollow glass microspheres includes the following steps:

[0046] (1) Soaking the hollow glass microspheres in a 4% NaOH solution for 2 h, filtering and drying to obtain hydroxylated glass microspheres; mixing 300 mL of Tris buffer with a pH of 8.5 and 0.5 g of dopamine hydrochloride, adding 25 g of hydroxylated glass microspheres, ultrasonically dispersing for 1 h, stirring at 18 ° C for 12 h, centrifuging, washing with water, and drying to obtain modified glass microspheres;

[0047] (2) Mix 1 g of modified glass microspheres and 250 mL of distilled water, add 25 mg of graphene oxide, adjust the pH to 4, stir for 1 h, let stand for 2 h, centrifuge, wash, and dry to obtain graphene oxide-coated glass microspheres;

[0048] (3) 1 g of graphene oxide-coated glass microspheres and 100 mL of deionized water were mixed, and a mixture of 0.13 g of carbon nanotubes and 43 mL of deionized water was added, and ultrasonic stirring was performed. 3 g of L-ascorbic acid and 0.1 g of sodium carboxymethyl cellulose were added, and ultrasonic stirring was performed for 1 h. A mixture of 2 g of amino polydimethylsiloxane and 10 mL of n-hexane was added, and ultrasonic stirring was performed. The mixture was kept at 95 °C for 10 h, cooled naturally to 18 °C, and frozen and thawed at -18 °C for 2 h. The operation was repeated twice, and the mixture was heated to 75 °C and kept for 3 h. The mixture was washed with deionized water, and the deionized water was replaced with anhydrous ethanol, and dried to obtain composite hollow glass microspheres.

[0049] The preparation of composite silicate comprises the following steps:

[0050] 1) Mix 1.6 mmol aluminum nitrate nonahydrate, 6.2 mmol cerium chloride, and 20 mL deionized water, add a mixture of 1 mmol iminodiacetic acid and 20 mL N, N-dimethylformamide, keep warm at 145 ° C for 5 h, cool, add 4.26 g tetraethyl silicate, keep warm at 145 ° C for 48 h, rinse with N, N-dimethylformamide and deionized water three times, dry, grind, heat to 550 ° C and keep warm for 5 h to obtain an intermediate powder;

[0051] 2) Mix 1 g of the intermediate powder and 10 mL of 1 mol / L ammonium nitrate solution, keep the mixture at 115°C for 10 h, wash and dry, and heat the mixture to 550°C for 5 h to obtain porous silicate;

[0052] 3) Compounding porous silicate, sodium silicate and potassium silicate in a mass ratio of 1:2:1 to obtain composite silicate.

[0053] Embodiment 2: A method for preparing a high temperature resistant mullite brick using aluminum slag, comprising the following steps:

[0054] S1: washing, crushing, grinding and sieving the aluminum ash slag to obtain aluminum ash slag powder, compounding the aluminum ash slag powder, silicon powder, fused white corundum fine powder and α-Al2O3 micro powder, and sintering with nitrogen to obtain mixed aluminum ash slag powder;

[0055] The mass ratio of aluminum ash powder, silicon powder, fused white corundum fine powder and α-Al2O3 micro powder is 4:3.3:1:1; the working conditions of nitrogen sintering are: in nitrogen environment, keep at 1420℃ for 10h;

[0056] S2: dividing the composite silicate into composite silicate A and composite silicate B according to a mass ratio of 9:1, and mixing the composite silicate B with deionized water to obtain a diluted composite silicate;

[0057] S3: adding composite hollow glass microspheres and mixed aluminum ash slag powder to a mixture, adding composite silicate A and an additive mixture, standing, adding a diluted composite silicate secondary mixture, keeping the moisture content at 3%, molding, gradient heating and heat preservation, obtaining a green body, sintering, and obtaining a high-temperature resistant mullite brick prepared using aluminum slag;

[0058] The auxiliary agent is calcium oxide; the working conditions of compression molding are: pressure 3MPa, time 3min;

[0059] The working conditions of gradient heating and heat preservation are: 2℃·min -1 Raise the temperature to 75℃ and keep it for 23h at 4℃·min -1 Heat to 130℃ and keep warm for 46h;

[0060] The working conditions for sintering are: keeping at 1620℃ for 7h;

[0061] In terms of weight, the composition of the blank is: 21 parts of mixed aluminum ash slag powder, 14 parts of additives, 3 parts of composite hollow glass microspheres, and 5 parts of composite silicate;

[0062] The preparation of composite hollow glass microspheres includes the following steps:

[0063] (1) Soaking the hollow glass microspheres in a 4% by mass NaOH solution for 2 h, filtering and drying to obtain hydroxylated glass microspheres; mixing 300 mL of Tris buffer with a pH of 8.5 and 0.5 g of dopamine hydrochloride, adding 25 g of hydroxylated glass microspheres, ultrasonically dispersing for 1.5 h, stirring at 20 ° C for 11 h, centrifuging, washing with water, and drying to obtain modified glass microspheres;

[0064] (2) Mix 1 g of modified glass microspheres and 250 mL of distilled water, add 25 mg of graphene oxide, adjust the pH to 4, stir for 1 h, let stand for 2 h, centrifuge, wash, and dry to obtain graphene oxide-coated glass microspheres;

[0065] (3) 1 g of graphene oxide-coated glass microspheres and 100 mL of deionized water were mixed, and a mixture of 0.13 g of carbon nanotubes and 43 mL of deionized water was added, and ultrasonic stirring was performed. 3 g of L-ascorbic acid and 0.1 g of sodium carboxymethyl cellulose were added, and ultrasonic stirring was performed for 1.5 h. A mixture of 2 g of amino polydimethylsiloxane and 10 mL of n-hexane was added, and ultrasonic stirring was performed. The mixture was kept at 98 °C for 9.5 h, cooled naturally to 20 °C, and frozen and thawed at -18 °C for 2 h. The operation was repeated twice, and the mixture was heated to 78 °C and kept for 3 h. The mixture was washed with deionized water, and the deionized water was replaced with anhydrous ethanol, and dried to obtain composite hollow glass microspheres.

[0066] The preparation of composite silicate comprises the following steps:

[0067] 1) Mix 1.6 mmol aluminum nitrate nonahydrate, 6.2 mmol cerium chloride, and 20 mL deionized water, add a mixture of 1 mmol iminodiacetic acid and 20 mL N, N-dimethylformamide, keep the mixture at 148°C for 4.5 h, cool, add 4.26 g tetraethyl silicate, keep the mixture at 148°C for 46 h, rinse with N, N-dimethylformamide and deionized water four times, dry, grind, heat to 550°C and keep the mixture for 5.5 h to obtain an intermediate powder;

[0068] 2) Mix 1 g of the intermediate powder and 10 mL of 1 mol / L ammonium nitrate solution, keep the mixture at 118°C for 9.5 h, wash and dry, and heat to 550°C for 5.5 h to obtain porous silicate;

[0069] 3) Compounding porous silicate, sodium silicate and potassium silicate in a mass ratio of 1:2:1 to obtain composite silicate.

[0070] Embodiment 3: A method for preparing a high temperature resistant mullite brick using aluminum slag, comprising the following steps:

[0071] S1: washing, crushing, grinding and sieving the aluminum ash slag to obtain aluminum ash slag powder, compounding the aluminum ash slag powder, silicon powder, fused white corundum fine powder and α-Al2O3 micro powder, and sintering with nitrogen to obtain mixed aluminum ash slag powder;

[0072] The mass ratio of aluminum ash powder, silicon powder, fused white corundum fine powder and α-Al2O3 micro powder is 4:3.3:1:1; the working conditions of nitrogen sintering are: in nitrogen environment, keep warm at 1450℃ for 10h;

[0073] S2: dividing the composite silicate into composite silicate A and composite silicate B according to a mass ratio of 9:1, and mixing the composite silicate B with deionized water to obtain a diluted composite silicate;

[0074] S3: adding composite hollow glass microspheres and mixed aluminum ash slag powder to composite silicate A and additive mixture, standing, adding diluted composite silicate secondary mixture, keeping the moisture content at 3.2%, molding, gradient heating and heat preservation, obtaining a green body, sintering, and obtaining a high temperature resistant mullite brick prepared using aluminum slag;

[0075] The auxiliary agent is magnesium oxide; the working conditions of compression molding are: pressure 4MPa, time 1min;

[0076] The working conditions of gradient heating and heat preservation are: 2℃·min -1 Heat to 80℃ and keep warm for 22h at 4℃·min -1 Heat to 140℃ and keep warm for 44h;

[0077] The sintering working conditions are: keeping at 1650℃ for 6h;

[0078] In terms of weight, the composition of the blank is: 22 parts of mixed aluminum ash slag powder, 15 parts of additives, 5 parts of composite hollow glass microspheres, and 8 parts of composite silicate;

[0079] The preparation of composite hollow glass microspheres includes the following steps:

[0080] (1) Soaking the hollow glass microspheres in a 4% by mass NaOH solution for 2 h, filtering and drying to obtain hydroxylated glass microspheres; mixing 300 mL of Tris buffer with a pH of 8.5 and 0.5 g of dopamine hydrochloride, adding 25 g of hydroxylated glass microspheres, ultrasonically dispersing for 2 h, stirring at 25 ° C for 10 h, centrifuging, washing with water, and drying to obtain modified glass microspheres;

[0081] (2) Mix 1 g of modified glass microspheres and 250 mL of distilled water, add 25 mg of graphene oxide, adjust the pH to 4, stir for 1 h, let stand for 2 h, centrifuge, wash, and dry to obtain graphene oxide-coated glass microspheres;

[0082] (3) 1 g of graphene oxide-coated glass microspheres and 100 mL of deionized water were mixed, and a mixture of 0.13 g of carbon nanotubes and 43 mL of deionized water was added, and ultrasonic stirring was performed. 3 g of L-ascorbic acid and 0.1 g of sodium carboxymethyl cellulose were added, and ultrasonic stirring was performed for 2 h. A mixture of 2 g of amino polydimethylsiloxane and 10 mL of n-hexane was added, and ultrasonic stirring was performed. The mixture was kept at 100 °C for 10 h, cooled naturally to 25 °C, and frozen and thawed at -18 °C for 2 h. The operation was repeated 3 times, and the mixture was heated to 80 °C and kept for 3 h. The mixture was washed with deionized water, and the deionized water was replaced with anhydrous ethanol, and dried to obtain composite hollow glass microspheres.

[0083] The preparation of composite silicate comprises the following steps:

[0084] 1) Mix 1.6 mmol aluminum nitrate nonahydrate, 6.2 mmol cerium chloride, and 20 mL deionized water, add a mixture of 1 mmol iminodiacetic acid and 20 mL N, N-dimethylformamide, keep the mixture at 150°C for 4 h, cool, add 4.26 g tetraethyl silicate, keep the mixture at 150°C for 44 h, rinse with N, N-dimethylformamide and deionized water for 5 times, dry, grind, heat to 550°C and keep the mixture for 6 h to obtain an intermediate powder;

[0085] 2) Mix 1 g of the intermediate powder and 10 mL of 1 mol / L ammonium nitrate solution, keep the mixture at 120 °C for 9 h, wash and dry, and heat to 550 °C for 6 h to obtain porous silicate;

[0086] 3) Compounding porous silicate, sodium silicate and potassium silicate in a mass ratio of 1:2:1 to obtain composite silicate.

[0087] Comparative Example 1: Taking Example 3 as the control group, aluminum ash slag powder was used to replace the mixed aluminum ash slag powder, and other processes were normal.

[0088] Comparative Example 2: Taking Example 3 as the control group, the composite hollow glass microspheres were replaced with graphene oxide-coated glass microspheres, and the other processes were normal.

[0089] Comparative Example 3: Taking Example 3 as the control group, hollow glass microspheres were used to replace the composite hollow glass microspheres, and other processes were normal.

[0090] Comparative Example 4: Example 3 was used as a control group, in which porous silicate was not prepared, and other processes were normal.

[0091] Source of raw materials:

[0092] Aluminum ash slag (200µm): Yichuan Yugang Longquan Aluminum Co., Ltd.; Fused white corundum fine powder 325F (99.3%): Xinxing Fused Corundum Factory, Xingyang City, Henan Province; α-Al2O3 micropowder: by mass fraction, the main raw material composition is: 99.86% Al2O3, 0.072% Na2O, 0.018% Fe2O3, 0.05% SiO2; Hollow glass microspheres K1: 3M Company, USA; Amino polydimethylsiloxane RED (98%): Haorui Chemical (Shanghai) Co., Ltd.; Graphene oxide 777676, L-ascorbic acid A92902: Merck Reagents; Tris buffer: Beijing Huakesheng Fine Chemical Products Trading Co., Ltd.; silicon powder S401567, dopamine hydrochloride D103111, carbon nanotubes C313046, sodium carboxymethyl cellulose C104984, aluminum nitrate nonahydrate S492260, cerium chloride C196218, iminodiacetic acid I104451, N,N-dimethylformamide D111999, tetraethyl silicate T110593, ammonium nitrate A117719: Aladdin reagent; n-hexane, calcium carbonate, calcium oxide, magnesium oxide, NaOH, sodium silicate, potassium silicate, analytical grade: Sinopharm Group reagent.

[0093] Performance test: The performance test of the mullite bricks prepared in Examples 1-3 and Comparative Examples 1-4 was performed:

[0094] The size of the mullite brick in the embodiment and the comparative example is 228mm×114mm×75mm; volume density and porosity: detected with reference to GB / T2997-2015; compressive strength: detect the compressive strength at 25°C with reference to GB / T5072-2023, and test with reference to the padless test method, with a loading rate of 1.1MPa / s; thermal shock resistance: put the sample into a resistance furnace, heat it to 1100°C and keep it warm for 15min, take it out and air cool it to 25°C, complete a thermal shock, cycle 10 times, test the flexural strength before and after the test, and characterize the thermal shock resistance of the mullite brick with the flexural strength retention rate; alkali crack resistance: drill a circular hole with a depth of 50mm and a diameter of 20mm on the sample, put in 10g of potassium carbonate, heat it to 1200°C and keep it warm for 4h, cool it naturally to 25°C, and detect whether cracks are generated. No cracks are qualified, and cracks are unqualified; the results are shown in Table 1 below;

[0095] Table 1

[0096] The present invention provides a high temperature resistant mullite brick prepared by using aluminum slag and a preparation method thereof. It can be seen from the above table that the porosity of the mullite brick prepared according to the present invention is 33.5-34.3%, the compressive strength is 186-191MPa, the flexural strength retention rate is 72-74%, and no cracks appear in the alkali-soluble crucible method, indicating that the present invention uses aluminum ash slag as a raw material to prepare high temperature resistant mullite bricks with high flexural resistance, good alkali corrosion resistance and high thermal shock resistance. In Table 1, / indicates that the item has not been measured.

[0097] Example 3 is compared with Comparative Example 1. The present invention uses aluminum ash slag as raw material, crushes and sieves it, and aims at the problems that the existing aluminum ash slag has complex components and the colored glaze is difficult to clean. In the present invention, aluminum ash slag powder is compounded with silicon powder, electric fused white corundum fine powder, and α-Al2O3 micropowder, and sintered in a nitrogen atmosphere to form β-SiAlON powder on the surface of the aluminum ash slag powder to achieve a core-shell structure, and shield and wrap the low melting point components in the aluminum ash slag on the microstructure, thereby greatly improving the high temperature resistance of the aluminum ash slag, so that the sintered aluminum ash slag can be granulated, high in strength, and does not generate gas during the re-firing process, thereby realizing the transformation of waste into treasure.

[0098] Example 3 is compared with Comparative Example 2 and Comparative Example 3. In order to improve the dispersibility and high temperature resistance of the hollow glass microspheres, graphene oxide is used to coat the surface of the hollow glass microspheres. Because the hollow glass microspheres are inert to reaction, the hollow glass microspheres are first treated with NaOH solution and dopamine hydrochloride in sequence to obtain dopamine-modified hollow glass microspheres, and then the hollow glass microspheres are electrostatically self-assembled with graphene oxide to obtain graphene oxide-coated hollow glass microspheres. On the one hand, the agglomeration of the hollow glass microspheres is inhibited by graphene oxide, and on the other hand, the hollow glass microspheres inhibit the formation of graphene oxide. The graphene sheets are stacked with each other; in order to further improve the flexural resistance of the mullite brick, the present invention further performs aerogel treatment on the graphene oxide-coated hollow glass microspheres, prepares a high-elastic aerogel by combining the sol-gel method and normal pressure drying, and prepares a high specific surface area aerogel with three-dimensional mesh graphene oxide and multi-walled carbon nanotubes on the graphene oxide-coated hollow glass microspheres as the skeleton of the mullite brick, introduces amino polydimethylsiloxane to make it amino, improves the compatibility of the aerogel and the base material, thereby further improving the flexural resistance and thermal shock resistance of the mullite brick.

[0099] Example 3 is compared with Comparative Example 4. The traditional inorganic silicate uses water as the main dispersant, which causes it to shrink greatly during the solidification process, is prone to cracks, and has poor corrosion resistance. A porous silicate, sodium silicate, and potassium silicate are compounded as a binder to solve the problem that potassium silicate and sodium silicate are relatively brittle after solidification. Aluminum nitrate nonahydrate, cerium chloride, and an organic ligand iminodiacetic acid are used to synthesize an aluminum-cerium bimetallic organic framework as a template, and silicate is used as a skeleton to synthesize porous aluminum-cerium silicate. Its unique configuration changes the particle grading of mullite bricks, thereby effectively improving the density of the brick blank. The high reactivity of porous aluminum-cerium silicate effectively promotes the densification of mullite bricks. Its higher unit surface area helps to improve the plasticity of molding and activate the formation of mullite. At the same time, cerium ions enter the corundum-mullite lattice during sintering, thereby effectively improving the high-temperature flexural resistance of mullite bricks.

[0100] The above descriptions are only embodiments of the present invention and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the present invention specification under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A method for preparing high temperature resistant mullite bricks using aluminum slag, characterized in that: The following steps are involved: S1: washing, crushing, grinding and sieving the aluminum ash slag to obtain aluminum ash slag powder, compounding the aluminum ash slag powder, silicon powder, fused white corundum fine powder and α-Al2O3 micro powder, and sintering with nitrogen to obtain mixed aluminum ash slag powder; S2: dividing the composite silicate into composite silicate A and composite silicate B according to a mass ratio of 9:1, and mixing the composite silicate B with deionized water to obtain a diluted composite silicate; S3: adding composite hollow glass microspheres and mixed aluminum ash slag powder to a mixture, adding composite silicate A and an additive mixture, standing, adding a diluted composite silicate secondary mixture to keep the moisture content at 2.5-3.2%, molding, gradient heating and heat preservation to obtain a green body, sintering, and obtaining a high-temperature resistant mullite brick prepared using aluminum slag; The preparation of composite hollow glass microspheres includes the following steps: (1) Soaking the hollow glass microspheres in a NaOH solution for 2 hours, filtering and drying to obtain hydroxylated glass microspheres; mixing Tris buffer and dopamine hydrochloride, adding the hydroxylated glass microspheres, ultrasonically dispersing for 1-2 hours, stirring at 18-25° C. for 10-12 hours, centrifuging, washing with water, and drying to obtain modified glass microspheres; (2) mixing the modified glass microspheres and distilled water, adding graphene oxide, adjusting the pH to 4, stirring for 1 hour, standing for 2 hours, centrifuging, washing, and drying to obtain graphene oxide-coated glass microspheres; (3) mixing graphene oxide coated glass microspheres and deionized water, adding a mixture of carbon nanotubes and deionized water, ultrasonically stirring, adding L-ascorbic acid and sodium carboxymethyl cellulose, ultrasonically stirring for 1-2 hours, adding a mixture of amino polydimethylsiloxane and n-hexane, ultrasonically stirring, keeping warm at 95-100° C. for 9-10 hours, naturally cooling to 18-25° C., transferring to -18° C. for freeze-thawing for 2 hours, repeating the operation 2-3 times, heating to 75-80° C. for 3 hours, washing with deionized water, replacing the deionized water with anhydrous ethanol, and drying to obtain composite hollow glass microspheres; The preparation of composite silicate comprises the following steps: 1) Aluminum nitrate nonahydrate, cerium chloride and deionized water are mixed, a mixed solution of iminodiacetic acid and N,N-dimethylformamide is added, the mixture is kept at 145-150° C. for 4-5 hours, cooled, tetraethyl silicate is added, the mixture is kept at 145-150° C. for 44-48 hours, the mixture is rinsed with N,N-dimethylformamide and deionized water for 3-5 times, dried, ground, heated to 550° C. and kept for 5-6 hours to obtain an intermediate powder; 2) mixing the intermediate powder and the ammonium nitrate solution, keeping the mixture at 115-120° C. for 9-10 hours, washing, drying, and heating to 550° C. for 5-6 hours to obtain a porous silicate; 3) Compounding porous silicate, sodium silicate and potassium silicate in a mass ratio of 1:2:1 to obtain composite silicate; The mass ratio of aluminum ash slag powder, silicon powder, fused white corundum fine powder and α-Al2O3 fine powder in the mixed aluminum ash slag powder is 4:3.3:1:1; The composition of the blank is as follows, by weight: 20-22 parts of mixed aluminum ash slag powder, 12-15 parts of auxiliary agent, 1-5 parts of composite hollow glass microspheres, and 3-8 parts of composite silicate.

2. The method for preparing high temperature resistant mullite bricks using aluminum slag according to claim 1, characterized in that: The auxiliary agent is one of calcium carbonate, calcium oxide and magnesium oxide.

3. The method for preparing high temperature resistant mullite bricks using aluminum slag according to claim 1, characterized in that: The working conditions of compression molding are: pressure of 2-4MPa and time of 1-5min.

4. The method for preparing high temperature resistant mullite bricks using aluminum slag according to claim 1, characterized in that: The working conditions of gradient heating and heat preservation are: 2℃·min -1 Heat to 70-80℃ and keep warm for 22-24h at 4℃·min -1 Raise the temperature to 120-140℃ and keep warm for 44-48h.

5. The method for preparing high temperature resistant mullite bricks using aluminum slag according to claim 1, characterized in that: The working conditions of nitrogen sintering in step S1 are: keeping warm at 1400-1450° C. for 9-10 hours in a nitrogen environment; the working conditions of sintering in step S3 are: keeping warm at 1600-1650° C. for 6-8 hours.

6. A high temperature resistant mullite brick prepared by using aluminum slag, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 5.