A kind of clay stabilizer and preparation method thereof

By preparing a zwitterionic clay stabilizer with a dendritic network structure, the problem of clay stabilizer resistance under high temperature and water flushing is solved, and stable anti-swelling effect and durability are achieved, which is suitable for high-permeability and low-permeability oil and gas layers.

CN118480342BActive Publication Date: 2024-10-22QARAMAY ZIGUANG TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410941145.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-22
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

Existing clay stabilizers have poor resistance to high temperature environments and water flushing, and their anti-swelling effects are unstable. Especially in low-permeability oil layers, they may aggravate the negative impact on permeability.

Method used

Polyethylene glycol derivatives, modified siloxanes, quaternary ammonium salts, organic metal salts, amides and other materials are used to prepare a dendritic network structure zwitterionic clay stabilizer through multi-step reactions to enhance the temperature resistance of the clay stabilizer. properties and anti-swelling properties, and builds a three-dimensional structure through silane coupling and hyperbranching modification technology to improve adsorption capacity.

Benefits of technology

Significantly improve the water resistance, high temperature resistance and anti-swelling properties of the clay stabilizer, allowing it to maintain a stable effect in harsh environments, avoid clay swelling and migration, extend the service life, and do not affect the permeability in low-permeability oil layers .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_15
    Figure SMS_15
  • Figure SMS_16
    Figure SMS_16
  • Figure SMS_17
    Figure SMS_17
Patent Text Reader

Abstract

The present invention belongs to the technical field of stabilizers, and specifically relates to a clay stabilizer and a preparation method thereof. The method comprises: (1) uniformly mixing polyethylene glycol derivatives, modified siloxanes, quaternary ammonium salts, organic metal salts, amides and ammonium sulfate salts in proportion to obtain a substrate through reaction; (2) uniformly mixing the substrate, aliphatic carboxylic acid esters, hydrocarbon compounds and polyamine derivatives in proportion to prepare a pre-modified substrate, and uniformly mixing the pre-modified substrate, acyclic alcohols and guanidine salts in proportion to obtain a modified substrate through reaction; (3) uniformly mixing the modified substrate, siloxanes and organic metal salts in proportion to obtain a clay stabilizer through reaction. The clay stabilizer of the present invention has a good adsorption effect on particulate matter, strengthens the anti-swelling property of the clay stabilizer, and enables the clay stabilizer to maintain a good stabilization effect after being flushed with water, so that it can still maintain its working ability in a relatively harsh working environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of stabilizers, and particularly relates to a clay stabilizer and a preparation method thereof. Background Art

[0002] The expansion and migration of clay minerals when encountering fresh water, which damages the permeability of the formation, has become a major problem in the process of oil production. To solve this problem, the application of clay stabilizers is particularly important. The stabilizer can effectively adhere to the surface of clay, effectively inhibit the expansion and dispersion migration of water-sensitive minerals caused by hydration, thereby reducing the damage to the oil and gas layer. At present, the main method of water injection development is used in the field of oil production in my country. However, in the actual production process, the clay minerals in the formation are prone to expansion and dispersion after contact with water-based substances, which will not only directly lead to a significant decrease in the permeability of the reservoir, but also cause irreversible damage to the oil and gas reservoir. In order to effectively deal with this problem and protect the permeability of the oil and gas layer, we specially add clay stabilizers to various water-based working fluids. When these stabilizers work, the electrolyzed cations are firmly adsorbed on the surface of clay particles through electrostatic action, thereby reducing the negative charge of clay particles and further wrapping them on the surface of particles, thereby achieving the effect of inhibiting clay expansion.

[0003] The clay stabilizers commonly used in oilfield operations in the existing public technology are mainly divided into two categories: inorganic salt stabilizers and organic cationic clay stabilizers. Among them, inorganic salt clay stabilizers have high anti-swelling ability in the early stage, but the anti-swelling ability is gradually weakened due to the impact of scouring during use, and the effect only exists in a short time; organic cationic clay stabilizers have a more lasting effect and can maintain the stability of clay for a long time. However, it should be pointed out that for low permeability oil layers, the use of cationic polymers with larger molecular weight may aggravate the negative impact on the permeability of the oilfield. Summary of the invention

[0004] The technical solution of the present invention aims at the technical difficulties that the clay stabilizer in the existing public technical solution has poor temperature resistance, poor water washing resistance and unstable anti-swelling effect during actual use, and provides a clay stabilizer and a preparation method thereof.

[0005] The main purposes of the present invention are: 1. To improve the thermal stability of the clay stabilizer so that it can still maintain its working ability in a harsh working environment.

[0006] 2. Clay stabilizer can still maintain the stabilizing effect on clay after being flushed with water.

[0007] 3. Strengthen the anti-swelling property of clay stabilizer.

[0008] To achieve the above objectives, the present invention adopts the following technical solutions.

[0009] A method for preparing a clay stabilizer comprises: (1) uniformly mixing polyethylene glycol derivatives, modified siloxane, quaternary ammonium salt, organic metal salt, amide and ammonium sulfate in proportion, and reacting to obtain a base material.

[0010] (2) The substrate, aliphatic carboxylic acid ester, hydrocarbon compound and polyamine derivative are mixed uniformly in proportion to prepare a pre-modified substrate, and the pre-modified substrate, acyclic alcohol and guanidine salt are mixed uniformly in proportion to react to obtain a modified substrate.

[0011] (3) The modified substrate, siloxane and organic metal salt are mixed in proportion and reacted evenly to obtain a clay stabilizer.

[0012] Preferably, the polyethylene glycol derivative in step (1) is polyoxyethylene propylene glycol ether.

[0013] The modified siloxane in step (1) is polyether-modified trisiloxane.

[0014] The quaternary ammonium salt in step (1) is a diquaternary ammonium salt.

[0015] The organic metal salt in step (1) is sodium hydroxymethane sulfonate.

[0016] The amide in step (1) is acrylamide.

[0017] The ammonium sulfate salt in step (1) is ammonium persulfate.

[0018] In step (1), the polyethylene glycol derivative, modified siloxane, quaternary ammonium salt, organic metal salt, amide and ammonium sulfate are uniformly mixed in a mass ratio of 10: (0.8-1.2): (3.7-4.1): (3.8-4.2): (0.9-1.1): (0.5-1.5).

[0019] Preferably, the preparation method of the modified siloxane in step (1) is: uniformly mixing allyloxy polyoxyethylene ether, hexadecyl cyclooctasiloxane and trimethyl platinum iodide in a mass ratio of (0.8-1.2):1:(0.008-0.012), stirring and reacting at a temperature of 90-105°C for 4-7 hours to prepare polyether-modified trisiloxane.

[0020] The preparation method of the diquaternary ammonium salt in step (1) is as follows: polyetheramine and dimethyl sulfite are uniformly mixed in a mass ratio of 1: (2.5-3.5), stirred for reaction at a temperature of 80-95°C for 2-5 hours, and dried in an oven to obtain the diquaternary ammonium salt.

[0021] Preferably, the reaction in step (1) is carried out by stirring for 2.5 to 4 hours at a temperature of 40 to 90°C and a pH of 7 to 9, and the pH is adjusted by using a 0.01 to 1.0 mol / L sodium hydroxide solution.

[0022] Preferably, the aliphatic carboxylic acid ester in step (2) is ethyl hexanoate.

[0023] The hydrocarbon compound in step (2) is diethylenetriamine.

[0024] The polyamine derivative in step (2) is hexamethylenediamine.

[0025] In step (2), the substrate, aliphatic carboxylic acid ester, hydrocarbon compound and polyamine derivative are uniformly mixed in a mass ratio of 3:1:(1.1-1.4):(0.5-0.7).

[0026] The preparation of the pre-modified substrate in step (2) is carried out by reaction in an environment with a temperature of 120 to 160° C. for 2 to 5 hours.

[0027] Preferably, the acyclic alcohol in step (2) is n-butanol.

[0028] The guanidine salt in step (2) is guanidine hydrochloride.

[0029] In step (2), the pre-modified substrate, acyclic alcohol and guanidine salt are uniformly mixed in a mass ratio of 5: (1.8-2.2): 0.5.

[0030] The reaction in step (2) is as follows: stirring at a temperature of 80 to 105°C for 3 to 4.5 hours.

[0031] Preferably, the siloxane in step (3) is vinyltriethoxysilane.

[0032] The organic metal salt in step (3) is sodium methanesulfonate.

[0033] In step (3), the modified substrate, siloxane and organic metal salt are uniformly mixed in a mass ratio of 5: (1.8-2.2): (2.2-2.5).

[0034] Preferably, the reaction in step (3) is carried out in a protective atmosphere at a constant temperature of 110 to 125° C. for 3.5 to 5 hours.

[0035] A clay stabilizer.

[0036] The clay stabilizer provided in the scheme of the present invention is a composite clay stabilizer, which has multiple molecular links and contains multiple cationic groups. It can increase the number of strong adsorption exchange points by virtue of the dendritic network structure, and can be adsorbed on the surface of the adsorbed particles through intermolecular forces and hydrogen bonds. The clay stabilizer provided by the present invention has an appropriate molecular weight and can be widely used in high-permeability and low-permeability oil and gas layers. Its unique rigid structure can easily penetrate into the clay mineral layers, and under the joint action of various chemical forces, it ensures that the efficient and stable performance can be fully exerted.

[0037] In the technical solution of the present invention, the core lies in providing a zwitterionic clay stabilizer with propylene alcohol polyoxyethylene ether as the main base material and capable of producing a dendritic network structure by means of hyperbranching and silane coupling. In the field of oil production in my country, water injection development is a common technical means. However, in this process, clay minerals in the formation are prone to expansion and dispersion after contacting with water-based substances, resulting in a significant decrease in reservoir permeability, posing a serious threat to oil and gas reservoirs. In order to effectively ensure the permeability of oil and gas layers, clay stabilizers are often added to various water-based working fluids in actual operations. The addition of clay stabilizers can significantly inhibit the potential damage of clay to oil and gas layers. The cations electrolyzed in the water-based substance are tightly adsorbed on the surface of clay particles through electrostatic action, which can not only effectively reduce the negative charge of clay particles, but also inhibit the expansion trend of clay through encapsulation. At present, clay stabilizers widely used in oil fields are mainly divided into two categories: inorganic salts and organic cations. Among them, inorganic salt clay stabilizers show a high anti-swelling effect in the initial stage, but their scour resistance is relatively weak, and the anti-swelling effect is often only temporary. Relatively speaking, organic cationic clay stabilizers have a more lasting effect and can maintain the stability of clay for a long time. However, it is worth noting that in the application of low permeability oil layers, cationic polymers with larger relative molecular weight may aggravate the negative impact on oil field permeability.

[0038] In the technical solution of the present invention, through the final modification of the substrate, the hyperbranched substrate has a special three-dimensional structure, there are cavities in the internal molecular structure, and a large number of terminal amino groups are present on the surface of the hyperbranched substrate, which can be functionally modified to construct a dendritic network structure, which can effectively improve the anti-swelling performance of the clay stabilizer. At the same time, since the clay stabilizer prepared by the present invention has a small molecular weight, it will not have a negative impact on the permeability of the oil field.

[0039] In the technical solution of the present invention, the modified trisiloxane in the substrate has two intermolecular bonding methods, silicon-oxygen-carbon type and silicon-carbon type, among which the silicon-carbon type bonding method exists in large quantities in the substrate. Inside the substrate, the terminal hydroxyl group reaction activity in the polyether-modified trisiloxane is greater than the carbon-carbon double bond, resulting in the priority of the silicon-oxygen-carbon condensation reaction. The polyether-modified trisiloxane is used for methyl end-capping inside the substrate, so that the carbon-carbon double bond is preferentially subjected to silicon-hydrogen addition, forming a silicon-carbon bond with good water stability, thereby ensuring that the final prepared clay stabilizer has strong water resistance. At the same time, when the polyether-modified trisiloxane is introduced into the substrate, the probability of the propylene alcohol polyoxyethylene ether molecular chain contacting with water molecules can be reduced, further enhancing the water resistance of the stabilizer.

[0040] Quaternary ammonium salt clay stabilizers are common chemical additives in the process of oil field water injection and exploitation in the prior art. In the scheme of the present invention, a double quaternary ammonium salt structure is formed by polyetheramine and dimethyl sulfite. The structure has a positively charged polymer cation in water and can adsorb multiple clay particles at the same time. After the adsorption is completed, the polyether molecules can form an adsorption protective layer on the surface of the adsorbed particles, which can effectively prevent the swelling and migration of the adsorbed particles. In addition, the clay stabilizer provided by the present invention can react in water under the interaction of double quaternary ammonium bonds to form a silanol intermediate with reaction ability, and the intermediate is further The polymer is polycondensed to form a polymer, which is then hydrolyzed. The product thereof initiates dehydration condensation with the hydroxyl groups on the surface of the adsorbed particles, thereby modifying the surface of the adsorbed particles, changing the hydrophilic surface characteristics into a lipophilic surface to further inhibit the swelling of the adsorbed particles in water. The polyether silicon forms chemical bonds on the surface of the adsorbed particles, which can effectively improve the temperature resistance of the clay stabilizer during use. At the same time, the introduction of quaternary ammonium groups into the substrate makes the material molecules have the characteristics of multi-point adsorption of double quaternary ammonium salts, and improves the chemical adsorption capacity of the material through chemical modification, while improving the high temperature resistance of the material and expanding the application range of the stabilizer.

[0041] In the technical scheme of the present invention, ethyl hexanoate and hexamethylenediamine can generate multiple coordination bonds in a high temperature environment to form a cross-linked small molecule complex. Under the action of high temperature reaction, the small molecule cross-linked complex is dispersed in polyoxyethylene propylene alcohol ether, diquaternary ammonium salt and sodium hydroxymethyl sulfonate. Under the initiation of diethylenetriamine, a micro-particle pre-cross-linked body is formed. The structure can be adsorbed on the surface of clay particles and embedded in the particle lattice to achieve the inhibition of the expansion and migration of the adsorbed particles. At the same time, the clay stabilizer provided by the present invention can produce different adsorption effects according to the pH change in the environment. Under the synergistic effect with polyether-modified trisiloxane, acrylamide and ammonium persulfate, it can form permanent multi-point adsorption on the surface of the adsorbed particles, and generate chemical bonds with the clay to separate the water molecules in the adsorbed clay, so that the adsorbed clay shrinks and expands, thereby reinforcing the firmness between the adsorbed particles, reducing the migration of the adsorbed clay, and helping to improve the water resistance of the clay stabilizer during use.

[0042] In the technical solution of the present invention, allyl alcohol polyoxyethylene ether, polyether-modified trisiloxane, and diquaternary ammonium salt are guided by hexamethylenediamine, and ethyl hexanoate and diethylenetriamine are externally connected on the molecular side chain to form a three-dimensional structure of a hyperbranched polymer, so that the stabilizer molecular chain is lengthened, and sodium hydroxymethyl sulfonate is added to the reaction to form a network-like small molecule compound and a chelate structure, which has a variety of cationic properties and can be adsorbed at multiple points. When the clay stabilizer meets water, the polymer micelles of the intermediate are uniformly dispersed in the solution system due to electrostatic and hydrogen bond adsorption, and the clay stabilizer forms a monomolecular adsorption layer in the soil layer due to the charge repulsion effect, expanding the surface treatment area of ​​the clay stabilizer during the treatment process. At the same time, the chelate structure constructed by the clay stabilizer prepared by the present invention can also retain metal ions in the soil layer, reduce the interference of metal ions on the stabilizer, and enable the clay stabilizer to penetrate into the soil layer crystals more conveniently, and also have the surface adsorption of the stabilizer to be easy, and extend the effective service life of the clay stabilizer.

[0043] In the technical solution of the present invention, after hyperbranched modification, the clay stabilizer of the present invention successfully incorporates the excellent properties of organic clay stabilizers. On the basis of the existing, the present invention further introduces vinyl triethoxysilane and sodium methanesulfonate for modification, thereby successfully achieving a significant synergistic effect in the present technology. This synergistic effect not only greatly enhances the performance of the clay stabilizer, but also broadens its scope of application in practical applications, so that the present invention shows a higher practical value in the relevant field. In the key shrinkage and expansion treatment process of the clay stabilizer, sodium methanesulfonate becomes an indispensable component with its excellent strong cationic properties. Under the precise synergistic effect of vinyl triethoxysilane, it undergoes a silane coupling reaction with the modified substrate, so that a stable and efficient combination of strong cationic groups and active adsorption groups is successfully formed inside the modified substrate. The reshaped strong cationic group can be firmly adsorbed on the clay particles with its strong positive charge characteristics, thereby significantly inhibiting the expansion trend of the clay. At the same time, the active adsorption group, with its unique adsorption capacity, tightly connects the surrounding particles, further improving the stability and anti-migration of the clay. After modification and rearrangement, the clay stabilizer of the present invention exhibits excellent performance in controlling clay expansion and inhibiting particle migration. These groups are adsorbed on clay particles to ensure that the particles maintain a tight, non-dispersed state, thereby effectively preventing cracks and particles that may be caused by external pressure or water flushing. At the same time, sodium methanesulfonate fully provides the required cation concentration in this process, effectively preventing leaching that may be caused by cation exchange, thereby preventing the dispersion of clay particles. In addition, thanks to the modification of silane coupling, the stacking morphology of clay particles is maintained, presenting a stable state of condensation and concentration.

[0044] The advantages of the present invention are: (1) through the selection of the substrate and subsequent chemical modification, the present invention enables the clay stabilizer to have a good adsorption effect on both cationic particles and anionic particles, and modifies the structure of the adsorbed particles to enhance the anti-swelling property of the clay stabilizer.

[0045] (2) The present invention constructs a hyperbranched three-dimensional structure, which can not only construct an adsorption exchange space, but also modify the surface of the adsorbed particles, so that the clay stabilizer can still maintain a good stabilizing effect after being washed with water.

[0046] (3) The present invention reconstructs the internal structure of the stabilizer by silane coupling, so that it can provide sufficient adsorption exchange points under different pH conditions and different temperature conditions, so that it can still maintain its working ability in a relatively harsh working environment. DETAILED DESCRIPTION

[0047] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0048] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0049] Unless otherwise specified, in the embodiments of the present invention, the preparation methods of polyether-modified trisiloxane and diquaternary ammonium salt are as follows: The preparation method of polyether-modified trisiloxane is: allyloxypolyoxyethylene ether, hexadecylcyclooctasiloxane and trimethylplatinum iodide are uniformly mixed in a mass ratio of 1:1:0.01, and stirred for reaction at a temperature of 95°C for 6 h to prepare polyether-modified trisiloxane.

[0050] The preparation method of the diquaternary ammonium salt is as follows: polyetheramine and dimethyl sulfite are uniformly mixed in a mass ratio of 1:3, stirred and reacted at a temperature of 85°C for 4 hours, and dried in an oven to obtain the diquaternary ammonium salt.

[0051] Example 1: A method for preparing a clay stabilizer, the method comprising: (1) uniformly mixing polyoxyethylene propylene alcohol ether, polyether-modified trisiloxane, diquaternary ammonium salt, sodium hydroxymethyl sulfonate, acrylamide and ammonium persulfate in a mass ratio of 10:0.8:3.7:4:1:0.5, stirring for 4 h at a temperature of 40°C and adjusting the pH to 7 with a sodium hydroxide solution having a concentration of 0.05 mol / L, to prepare a substrate.

[0052] (2) The substrate, ethyl hexanoate, diethylenetriamine and hexamethylenediamine were mixed uniformly in a mass ratio of 3:1:1.1:0.5, and reacted in an environment at a temperature of 120°C for 5 hours to prepare a pre-modified substrate. The pre-modified substrate, n-butanol and guanidine hydrochloride were mixed uniformly in a mass ratio of 5:1.8:0.5, and stirred and reacted in an environment at a temperature of 80°C for 4.5 hours to prepare a modified substrate.

[0053] (3) The modified substrate, vinyl triethoxysilane and sodium methane sulfonate were uniformly mixed in a mass ratio of 5:1.8:2.2, and reacted in a nitrogen atmosphere at a temperature of 110 °C for 5 h to prepare a clay stabilizer.

[0054] The clay stabilizer prepared in the example was subjected to performance testing, and the specific characterization results are as follows.

[0055] Anti-swelling rate test: weigh 0.5 g bentonite, add 10 mL deionized water, shake to volume, let stand at room temperature for 2 hours, centrifuge at 1500 r / min for 15 minutes, and record the volume of bentonite. ; Weigh 0.5 g bentonite and 0.025 g clay stabilizer, add 10 mL deionized water, shake to volume, let stand at room temperature for 2 h, centrifuge at 1500 r / min for 15 min, and record the volume of bentonite ; Weigh 0.5 g of bentonite, add 10 mL of kerosene, shake to volume, let stand at room temperature for 2 h, centrifuge at 1500 r / min for 15 min, and record the volume of bentonite , and calculate the anti-swelling rate of clay stabilizer according to the following formula.

[0056]

[0057] Where: ——Anti-swelling rate of clay stabilizer, %.

[0058] ——The volume of bentonite in kerosene, mL.

[0059] ——The volume of bentonite in clay stabilizer, mL.

[0060] ——The volume of bentonite in clean water, mL.

[0061] Washing resistance test: Take out the clay stabilizer test sample group in the above test, pour out the supernatant in the centrifuge tube, add deionized water to 10 mL, stir well, let it stand at room temperature for 2 hours, centrifuge it in a centrifuge at 1500 r / min for 15 minutes, and finally measure and record the volume of bentonite in the centrifuge tube. , and the water resistance of clay stabilizer is calculated using the following formula.

[0062]

[0063] Where: ——Water resistance of clay stabilizer, %.

[0064] ——The volume of bentonite in clay stabilizer, mL.

[0065] ——The expansion volume of bentonite after washing, mL.

[0066] ——The volume of bentonite in clean water, mL.

[0067]

[0068] In addition, referring to the detection method in SY / T 5370-2018, the surface and interfacial tension of the clay stabilizer prepared in the embodiment were measured at room temperature using the ring method. At the same time, the surface and interfacial tension of the clay stabilizer prepared in the embodiment were measured in an environment with a temperature of 120°C and a pressure of 24 MPa. The specific characterization results are as follows.

[0069]

[0070] Analysis of the above characterization results shows that the clay stabilizer prepared in the embodiment has excellent anti-swelling performance and outstanding water washing resistance due to the presence of multiple adsorption sites, and can still maintain more than 50% of the stabilizer properties in a high temperature and high pressure environment.

[0071] Example 2: A method for preparing a clay stabilizer, the method comprising: (1) uniformly mixing polyoxyethylene propylene alcohol ether, polyether-modified trisiloxane, diquaternary ammonium salt, sodium hydroxymethyl sulfonate, acrylamide and ammonium persulfate in a mass ratio of 10:1:3.9:4:1:1, stirring for 3.25 h at a temperature of 65°C and adjusting the pH to 8 with a sodium hydroxide solution with a concentration of 0.05 mol / L, to prepare a substrate.

[0072] (2) The substrate, ethyl hexanoate, diethylenetriamine and hexamethylenediamine were mixed uniformly in a mass ratio of 3:1:1.2:0.6, and reacted in an environment at a temperature of 140°C for 3.5 hours to prepare a pre-modified substrate. The pre-modified substrate, n-butanol and guanidine hydrochloride were mixed uniformly in a mass ratio of 5:2:0.5, and stirred and reacted in an environment at a temperature of 95°C for 3.75 hours to prepare a modified substrate.

[0073] (3) The modified substrate, vinyl triethoxysilane and sodium methane sulfonate were uniformly mixed in a mass ratio of 5:2:2.3, and reacted in a nitrogen atmosphere at a temperature of 115°C for 4.5 h to prepare a clay stabilizer.

[0074] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.

[0075]

[0076]

[0077] Analysis of the above characterization results shows that the clay stabilizer prepared in the embodiment has excellent anti-swelling performance and outstanding water washing resistance due to the presence of multiple adsorption sites, and can still maintain more than 50% of the stabilizer properties in a high temperature and high pressure environment.

[0078] Example 3: A method for preparing a clay stabilizer, the method comprising: (1) uniformly mixing polyoxyethylene propylene alcohol ether, polyether-modified trisiloxane, diquaternary ammonium salt, sodium hydroxymethyl sulfonate, acrylamide and ammonium persulfate in a mass ratio of 10:1.1:4:4:1:1, stirring for 3 hours at a temperature of 70°C and adjusting the pH to 9 with a sodium hydroxide solution with a concentration of 0.05 mol / L, to prepare a substrate.

[0079] (2) The substrate, ethyl hexanoate, diethylenetriamine and hexamethylenediamine were mixed uniformly in a mass ratio of 3:1:1.3:0.6, and reacted at a temperature of 140 °C for 3 h to prepare a pre-modified substrate. The pre-modified substrate, n-butanol and guanidine hydrochloride were mixed uniformly in a mass ratio of 5:2.1:0.5, and stirred at a temperature of 100 °C for 3.5 h to prepare a modified substrate.

[0080] (3) The modified substrate, vinyl triethoxysilane and sodium methane sulfonate were uniformly mixed in a mass ratio of 5:2.1:2.4, and reacted in a nitrogen atmosphere at a temperature of 120 °C for 4 h to prepare a clay stabilizer.

[0081] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.

[0082]

[0083]

[0084] Analysis of the above characterization results shows that the clay stabilizer prepared in the embodiment has excellent anti-swelling performance and outstanding water washing resistance due to the presence of multiple adsorption sites, and can still maintain more than 50% of the stabilizer properties in a high temperature and high pressure environment.

[0085] Example 4: A method for preparing a clay stabilizer, the method comprising: (1) uniformly mixing polyoxyethylene propylene alcohol ether, polyether-modified trisiloxane, diquaternary ammonium salt, sodium hydroxymethyl sulfonate, acrylamide and ammonium persulfate in a mass ratio of 10:1.2:4.1:4:1:1.5, stirring for 2.5 h at a temperature of 90°C and adjusting the pH to 9 with a sodium hydroxide solution having a concentration of 0.05 mol / L, to prepare a substrate.

[0086] (2) The substrate, ethyl hexanoate, diethylenetriamine and hexamethylenediamine were mixed uniformly in a mass ratio of 3:1:1.4:0.7, and reacted in an environment at a temperature of 160°C for 2 h to prepare a pre-modified substrate. The pre-modified substrate, n-butanol and guanidine hydrochloride were mixed uniformly in a mass ratio of 5:2.2:0.5, and stirred and reacted in an environment at a temperature of 105°C for 3 h to prepare a modified substrate.

[0087] (3) The modified substrate, vinyl triethoxysilane and sodium methane sulfonate were uniformly mixed in a mass ratio of 5:2.2:2.5, and reacted in a nitrogen atmosphere at a temperature of 125°C for 3.5 h to prepare a clay stabilizer.

[0088] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.

[0089]

[0090]

[0091] Analysis of the above characterization results shows that the clay stabilizer prepared in the embodiment has excellent anti-swelling performance and outstanding water washing resistance due to the presence of multiple adsorption sites, and can still maintain more than 50% of the stabilizer properties in a high temperature and high pressure environment.

[0092] Example 5: A method for preparing a clay stabilizer, the method comprising: (1) uniformly mixing polyoxyethylene propylene alcohol ether, polyether-modified trisiloxane, diquaternary ammonium salt, sodium hydroxymethyl sulfonate, acrylamide and ammonium persulfate in a mass ratio of 10:1.2:3.7:4:1:0.5, stirring for 3 h at a temperature of 70°C and adjusting the pH to 9 with a sodium hydroxide solution having a concentration of 0.05 mol / L, to prepare a substrate.

[0093] (2) The substrate, ethyl hexanoate, diethylenetriamine and hexamethylenediamine were mixed uniformly in a mass ratio of 3:1:1.3:0.6, and reacted at a temperature of 140 °C for 3 h to prepare a pre-modified substrate. The pre-modified substrate, n-butanol and guanidine hydrochloride were mixed uniformly in a mass ratio of 5:2.1:0.5, and stirred at a temperature of 100 °C for 3.5 h to prepare a modified substrate.

[0094] (3) The modified substrate, vinyl triethoxysilane and sodium methane sulfonate were uniformly mixed in a mass ratio of 5:2.1:2.4, and reacted in a nitrogen atmosphere at a temperature of 120 °C for 4 h to prepare a clay stabilizer.

[0095] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.

[0096]

[0097]

[0098] Analysis of the above characterization results shows that the clay stabilizer prepared in the embodiment has excellent anti-swelling performance and outstanding water washing resistance due to the presence of multiple adsorption sites, and can still maintain more than 50% of the stabilizer properties in a high temperature and high pressure environment.

[0099] At the same time, a comprehensive analysis of the data of Example 3 and Example 5 shows that in Example 5, due to the relatively increased content of the polyether-modified trisiloxane component in the substrate, under the influence of the silicon-carbon bonds between the molecules inside the material, the end-capping of the polymerized molecules inside the substrate accounts for a relatively high proportion. Although the water resistance of the prepared clay stabilizer is further improved, some three-dimensional molecular cavities are incomplete during the hyperbranching process, resulting in a decrease in the number of adsorption points. In summary, increasing the content of the polyether-modified trisiloxane component in the substrate cannot effectively enhance the overall performance of the clay stability. The substrate components can be modified according to actual conditions during specific use.

[0100] Example 6: A method for preparing a clay stabilizer, the method comprising: (1) uniformly mixing polyoxyethylene propylene alcohol ether, polyether-modified trisiloxane, diquaternary ammonium salt, sodium hydroxymethyl sulfonate, acrylamide and ammonium persulfate in a mass ratio of 10:0.8:4.1:4:1:0.5, stirring for 3 h at a temperature of 70°C and adjusting the pH to 9 with a sodium hydroxide solution with a concentration of 0.05 mol / L, to prepare a substrate.

[0101] (2) The substrate, ethyl hexanoate, diethylenetriamine and hexamethylenediamine were mixed uniformly in a mass ratio of 3:1:1.3:0.6, and reacted at a temperature of 140 °C for 3 h to prepare a pre-modified substrate. The pre-modified substrate, n-butanol and guanidine hydrochloride were mixed uniformly in a mass ratio of 5:2.1:0.5, and stirred at a temperature of 100 °C for 3.5 h to prepare a modified substrate.

[0102] (3) The modified substrate, vinyl triethoxysilane and sodium methane sulfonate were uniformly mixed in a mass ratio of 5:2.1:2.4, and reacted in a nitrogen atmosphere at a temperature of 120 °C for 4 h to prepare a clay stabilizer.

[0103] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.

[0104]

[0105]

[0106] Analysis of the above characterization results shows that the clay stabilizer prepared in the embodiment has excellent anti-swelling performance and outstanding water washing resistance due to the presence of multiple adsorption sites, and can still maintain more than 50% of the stabilizer properties in a high temperature and high pressure environment.

[0107] At the same time, a comprehensive analysis of the preparation processes and data of Example 3 and Example 6 shows that the content of the diquaternary ammonium salt component in step 1) of Example 6 is relatively increased, the number of pre-crosslinked microparticles produced in the substrate increases, and the ability to inhibit the expansion and migration of adsorbed particles is enhanced. However, due to the increased chemical bonding effect of the diquaternary ammonium salt inside the substrate, defects appear in the dendritic network structure, and the activity of the adsorption crosslinking points is slightly reduced in an environment with a pH greater than 10. In summary, increasing the content of the diquaternary ammonium salt component in the substrate cannot effectively enhance the overall performance of the clay stability. The substrate component can be modified according to actual conditions during specific use.

[0108] Example 7: A method for preparing a clay stabilizer, the method comprising: (1) uniformly mixing polyoxyethylene propylene alcohol ether, polyether-modified trisiloxane, diquaternary ammonium salt, sodium hydroxymethyl sulfonate, acrylamide and ammonium persulfate in a mass ratio of 10:1.1:4:4:1:1, stirring for 3 hours at a temperature of 70°C and adjusting the pH to 9 with a sodium hydroxide solution having a concentration of 0.05 mol / L, to prepare a substrate.

[0109] (2) The substrate, ethyl hexanoate, diethylenetriamine and hexamethylenediamine were mixed uniformly in a mass ratio of 3:1:1.3:0.6, and reacted in an environment at a temperature of 140°C for 3 h to prepare a pre-modified substrate. The pre-modified substrate, n-butanol and guanidine hydrochloride were mixed uniformly in a mass ratio of 5:2.1:0.5, and stirred and reacted in an environment at a temperature of 100°C for 4.5 h to prepare a modified substrate.

[0110] (3) The modified substrate, vinyl triethoxysilane and sodium methane sulfonate were uniformly mixed in a mass ratio of 5:2.1:2.4, and reacted in a nitrogen atmosphere at a temperature of 120 °C for 4 h to prepare a clay stabilizer.

[0111] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.

[0112]

[0113]

[0114] Analysis of the above characterization results shows that the clay stabilizer prepared in the embodiment has excellent anti-swelling performance and outstanding water washing resistance due to the presence of multiple adsorption sites, and can still maintain more than 50% of the stabilizer properties in a high temperature and high pressure environment.

[0115] At the same time, comprehensive analysis of the data of Example 3 and Example 7 shows that the hyperbranching reaction time is extended in Example 7, so that the degree of hyperbranching increases, a denser dendritic network can be produced, and more molecular cavities are provided, so that the clay stabilizer prepared by the embodiment has more strong adsorption cross-linking points, and the anti-swelling rate is improved. At the same time, more water-resistant carbon-silicon bonds will be produced in the silane coupling modification, so that the water resistance of the clay stabilizer is also enhanced. However, due to the limited adsorption that can be produced inside the substrate, the molecular cavities without cross-linking points will appear in the overly dense network, so that under high temperature conditions, these cavities will produce other side reactions, thereby affecting the use of the clay stabilizer in a high temperature environment. In summary, extending the hyperbranching reaction time cannot effectively enhance the overall performance of clay stability, and the hyperbranching time can be changed according to actual conditions during specific use.

[0116] Example 8: A method for preparing a clay stabilizer, the method comprising: (1) uniformly mixing polyoxyethylene propylene alcohol ether, polyether-modified trisiloxane, diquaternary ammonium salt, sodium hydroxymethyl sulfonate, acrylamide and ammonium persulfate in a mass ratio of 10:1.1:4:4:1:1, stirring for 3 hours at a temperature of 70°C and adjusting the pH to 9 with a sodium hydroxide solution with a concentration of 0.05 mol / L, to prepare a substrate.

[0117] (2) The substrate, ethyl hexanoate, diethylenetriamine and hexamethylenediamine were mixed uniformly in a mass ratio of 3:1:1.3:0.6, and reacted at a temperature of 140 °C for 3 h to prepare a pre-modified substrate. The pre-modified substrate, n-butanol and guanidine hydrochloride were mixed uniformly in a mass ratio of 5:2.1:0.5, and stirred at a temperature of 100 °C for 3.5 h to prepare a modified substrate.

[0118] (3) The modified substrate, vinyl triethoxysilane and sodium methane sulfonate were uniformly mixed in a mass ratio of 5:2.1:2.4, and reacted in a nitrogen atmosphere at a temperature of 120 °C for 5 h to prepare a clay stabilizer.

[0119] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.

[0120]

[0121]

[0122] Analysis of the above characterization results shows that the clay stabilizer prepared in the embodiment has excellent anti-swelling performance and outstanding water washing resistance due to the presence of multiple adsorption sites, and can still maintain more than 50% of the stabilizer properties in a high temperature and high pressure environment.

[0123] At the same time, a comprehensive analysis of the data of Example 3 and Example 8 shows that the silane coupling reaction time is extended in Example 8. Due to the full progress of the silane coupling reaction, the heat resistance of the clay stabilizer prepared by the example is enhanced, but with the increase of the degree of silane coupling, the Zeta potential gradually increases, and the particle size composed of the adsorbed particles first increases and then decreases, and the bentonite particles cannot be tightly connected, and the water cannot be completely squeezed out, resulting in a shrinkage rate lower than the anti-swelling rate, resulting in a decrease in the anti-swelling rate of the clay stabilizer. In summary, extending the silane coupling reaction time cannot effectively enhance the overall performance of the clay stability, and the degree of silane coupling can be modified according to actual conditions during specific use.

[0124] Comparative Example 1: A method for preparing a clay stabilizer. The specific preparation method is the same as that of Example 1. In the comparative example, only the substrate unique to the present invention is changed. An equal amount of polymethacryloyloxyethyltrimethylammonium chloride is used to replace the substrate prepared in step (1) to prepare the clay stabilizer. The clay stabilizer prepared in the comparative example is tested for performance in the same manner as in Example 1. The characterization results are as follows.

[0125]

[0126]

[0127] Analysis of the above characterization results shows that the clay stabilizer prepared in the comparative example has good anti-swelling rate and water resistance. However, due to the small intermolecular interaction force of the clay stabilizer prepared in the comparative example, the surface tension and interfacial tension of the stabilizer are smaller than those of the embodiment, especially in an environment with a temperature of 120°C and a pressure of 24 MPa, high-temperature cross-linking occurs, causing a vicious rheological phenomenon of gelation.

[0128] Comparative Example 2: A method for preparing a clay stabilizer, wherein the specific preparation method is the same as that of Example 1. In the comparative example, only the substrate modification process unique to the present invention is changed, and the substrate is not subjected to hyperbranching modification. That is, the pre-modified substrate prepared in step (2) is simply mixed with n-butanol and guanidine hydrochloride but not reacted, and then an equal amount of the mixture is used to replace the modified substrate to carry out the reaction in step (3) to prepare the clay stabilizer. The clay stabilizer prepared in the comparative example is subjected to performance testing in the same manner as in Example 1, and the characterization results are as follows.

[0129]

[0130]

[0131] Analysis of the above characterization results shows that the clay stabilizer prepared in the comparative example has only little change in relative water resistance and heat resistance, while the other properties are significantly reduced. The purpose of hyperbranching the substrate in the technical scheme of the present invention is to construct the internal structure of the material through branched chains and to provide strong adsorption cross-linking points. At the same time, the molecular cavity is used to ensure that the clay stabilizer has a small molecular weight while having a good internal stable structure.

[0132] Comparative Example 3: A method for preparing a clay stabilizer, wherein the specific preparation method is the same as that of Example 1. In the comparative example, only the substrate modification process unique to the present invention is changed, and the substrate is not subjected to silane coupling modification. That is, the modified substrate obtained in step (2) is directly used as a clay stabilizer, and vinyltriethoxysilane and sodium methanesulfonate are no longer used for modification to prepare the clay stabilizer. The clay stabilizer prepared in the comparative example is subjected to performance testing in the same manner as in Example 1, and the characterization results are as follows.

[0133]

[0134]

[0135] Analyzing the above characterization results, the clay stabilizer prepared in the comparative example has decreased in various test data, especially water resistance and heat resistance, because it has not been modified by silane to produce a synergistic effect. In the technical solution of the present invention, the interaction between sodium methane sulfonate and vinyl triethoxysilane enables the substrate to have strong cationic groups and active adsorption groups. The presence of these two types of groups is macroscopically manifested as condensation inside the substrate and better mutual adsorption between the adsorbed particles, thereby improving the stability between various molecules in the clay stabilizer system.

[0136] Comparative Example 4: A commercially available inorganic clay stabilizer, wherein the main material of the commercially available inorganic clay stabilizer is sodium chloride. The commercially available clay stabilizer was subjected to partial performance testing in the same manner as in Example 1, and the characterization results are as follows.

[0137]

[0138] Analysis of the above characterization results shows that the crystal structure of the commercially available clay stabilizer presents a silicon-oxygen tetrahedron structure, which can form a tight bond with the negatively charged clay surface. The clay stabilizer inhibits clay expansion by exchanging sodium ions on the clay surface. However, in actual operation, some ions will be replaced by sodium ions in the formation water again, and the clay will be converted into a swellable or dispersible form again, making its role in stabilizing the clay only time-limited and the long-term effect poor.

Claims

1. A method for preparing a clay stabilizer, characterized in that: The method comprises: (1) mixing polyethylene glycol derivatives, modified siloxane, quaternary ammonium salt, organic metal salt, amide and ammonium sulfate in proportion and reacting to obtain a substrate; (2) uniformly mixing a substrate, an aliphatic carboxylic acid ester, a hydrocarbon compound and a polyamine derivative in proportion to prepare a pre-modified substrate, and uniformly mixing the pre-modified substrate, an acyclic alcohol and a guanidine salt in proportion to react to obtain a modified substrate; (3) The modified substrate, siloxane and organic metal salt are mixed in proportion and reacted evenly to obtain a clay stabilizer; The polyethylene glycol derivative in step (1) is polyoxyethylene propylene glycol ether; The modified siloxane in step (1) is polyether-modified trisiloxane; The quaternary ammonium salt in step (1) is a diquaternary ammonium salt; The organic metal salt in step (1) is sodium hydroxymethane sulfonate; The amide in step (1) is acrylamide; The ammonium sulfate salt in step (1) is ammonium persulfate; The polyethylene glycol derivative, modified siloxane, quaternary ammonium salt, organic metal salt, amide and ammonium sulfate in step (1) are uniformly mixed in a mass ratio of 10: (0.8-1.2): (3.7-4.1): (3.8-4.2): (0.9-1.1): (0.5-1.5); The preparation method of the modified siloxane in step (1) is: The allyloxy polyoxyethylene ether, hexadecyl cyclooctasiloxane and trimethyl platinum iodide are uniformly mixed in a mass ratio of (0.8-1.2):1:(0.008-0.012), and stirred for reaction at a temperature of 90-105°C for 4-7 hours to prepare polyether-modified trisiloxane; The preparation method of the diquaternary ammonium salt in step (1) is: The polyetheramine and dimethyl sulfite are uniformly mixed in a mass ratio of 1: (2.5-3.5), stirred and reacted at a temperature of 80-95°C for 2-5 hours, and dried in an oven to obtain a diquaternary ammonium salt; The reaction in step (1) is as follows: stirring for 2.5 to 4 hours at a temperature of 40 to 90°C and a pH of 7 to 9; The aliphatic carboxylic acid ester in step (2) is ethyl hexanoate; The hydrocarbon compound in step (2) is diethylenetriamine; The polyamine derivative in step (2) is hexamethylenediamine; Step (2) The substrate, aliphatic carboxylic acid ester, hydrocarbon compound and polyamine derivative are uniformly mixed in a mass ratio of 3:1:(1.1-1.4):(0.5-0.7); The pre-modified substrate in step (2) is prepared by reaction in an environment with a temperature of 120 to 160° C. for 2 to 5 hours; The acyclic alcohol in step (2) is n-butanol; The guanidine salt in step (2) is guanidine hydrochloride; Step (2) The pre-modified substrate, acyclic alcohol and guanidine salt are uniformly mixed in a mass ratio of 5: (1.8-2.2): 0.5; The reaction in step (2) is as follows: stirring for 3 to 4.5 hours in an environment at a temperature of 80 to 105°C; The siloxane in step (3) is vinyltriethoxysilane; The organic metal salt in step (3) is sodium methanesulfonate; Step (3) The modified substrate, siloxane and organic metal salt are uniformly mixed in a mass ratio of 5: (1.8-2.2): (2.2-2.5); The reaction in step (3) is carried out at a constant temperature of 110 to 125° C. in a protective atmosphere for 3.5 to 5 hours.

2. A clay stabilizer obtained by the method of claim 1.

Citation Information

Patent Citations

  • Clay control additive for wellbore fluids

    CA2550834A1

  • Process for preparing sic-bonded polyethersiloxanes

    CA3007808A1

  • Method for producing high-purity quaternary ammonium compounds

    CN101039913A

  • Preparation method of aliphatic amine polyoxyethylene ether biquaternary surfactant

    CN102382292A

  • Composite modified hectorite, preparation method thereof and application in oil-based drilling fluid

    CN110183596A