A coal tar pitch-based silicon-carbon composite precursor material, a silicon-carbon negative electrode material prepared therefrom, and a preparation method thereof

By using strong oxidizer to modify coal asphalt to prepare coal asphalt-based silicon-carbon composite precursor materials in lithium-ion battery negative electrode materials, the poor conductivity and volume expansion of silicon-carbon composite materials are solved, and silicon with high load capacity and good cycle stability is achieved Carbon negative electrode material improves battery performance and process safety.

CN118495536BActive Publication Date: 2024-11-08XINGTAI RISUN NEW ENERGY TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410962520.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The existing silicon-carbon composite materials have poor conductivity and volume expansion problems in the negative electrode applications of lithium-ion batteries, resulting in a degradation of circulation performance. The domestic porous carbon manufacturing process route and raw material selection lead to a low skeleton strength, affecting the capacity and first effect.

Method used

The coal asphalt is carbonized and modified under a strong oxidant system to prepare coal asphalt-based silicon-carbon composite precursor material. The particle size and pore size distribution that meets the requirements of precipitation of silicon are obtained through alkali activation, thereby improving silicon binding and skeleton strength, and further passing through the CVD furnace. Medium silicon deposition forms silicon-carbon anode material with high load and good cycle stability.

Benefits of technology

High load, excellent first-time Coulomb efficiency and good cycle stability are achieved, limiting silicon expansion, increasing cycle life, and simplifying the process, improving safety and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495536B_ABST
    Figure CN118495536B_ABST
Patent Text Reader

Abstract

The present invention discloses a coal tar pitch-based silicon-carbon composite precursor material, a silicon-carbon negative electrode material prepared therefrom, and a preparation method thereof. The present invention carbonizes and modifies coal tar pitch in a strong oxidant system to improve its curing ability in a high temperature environment, and further prepares a coal tar pitch-based silicon-carbon composite precursor material by activation. The precursor material has a particle size and pore size distribution that meet the requirements of silicon precipitation, thereby having high silicon binding and skeleton strength. The silicon-carbon composite negative electrode material prepared from the precursor material has a high silicon loading, and can effectively inhibit the physical expansion of silicon during the lithiation process, showing a high first coulomb efficiency and good cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of silicon-carbon negative electrode materials, and in particular to a coal tar pitch-based silicon-carbon composite precursor material, a silicon-carbon negative electrode material prepared therefrom, and methods for preparing the same. Background Art

[0002] The field of new energy vehicles is gradually entering the 1-N stage, which has also driven the upstream power battery industry into the high-quality product-driven stage, and put forward higher requirements for the fast charging performance and endurance of power batteries. The "Action Plan for Promoting the Development of the Automotive Power Battery Industry" issued by the Ministry of Industry and Information Technology and other four ministries and commissions proposed that in 2020, the specific energy of new lithium-ion power batteries will exceed 300 Wh / kg, and the system specific energy will reach 260 Wh / kg; by 2025, the specific energy of the monomer will reach 500 Wh / kg. To achieve this goal, traditional graphite negative electrodes are almost impossible to achieve. Among the known negative electrode materials, silicon has a theoretical specific capacity of up to 4200 mAh / g, which is more than 10 times that of graphite materials, and can provide channels for lithium ion embedding and extraction from all directions. It has excellent fast charging performance and is expected to become the mainstream direction of the research and development of the next generation of negative electrode materials.

[0003] Although silicon materials have a high theoretical lithium storage capacity, low lithium insertion potential and abundant reserves, pure silicon powder has poor conductivity and produces a large volume expansion when forming Li-Si compounds. During the charge and discharge process, the electrode structure collapses due to the drastic change in volume, and the active material falls off, which leads to a decrease in the cycle performance of the electrode, making it impossible to use it in practice. The use of silicon-carbon composite materials as negative electrode materials for lithium-ion batteries can make up for the lack of low energy density of carbon materials through silicon materials, and at the same time, make up for the poor conductivity of silicon materials and inhibit the volume expansion of silicon through carbon materials. At present, the domestic porous carbon manufacturing process routes are basically the same, and the raw material selection varies greatly, mainly biomass, resin, and coal. When the above raw materials are used for preparation, the skeleton strength of the product is low, the overall yield is not high, and the final synthesized silicon-carbon composite material performs poorly in terms of gram capacity and first effect, affecting downstream use. Summary of the invention

[0004] Based on the problems existing in the above-mentioned prior art, the present invention proposes a method for preparing a silicon-carbon composite precursor material, which carbonizes coal tar under a strong oxidant system to improve its curing ability in a high temperature environment, and further prepares a coal tar-based silicon-carbon composite precursor material by alkali activation. The precursor material has a particle size and pore size distribution that meet the requirements of silicon precipitation, and thus has high silicon binding capacity and skeleton strength. The silicon-carbon negative electrode material prepared from this precursor material has a high silicon loading capacity, a high first coulomb efficiency and good cycle stability.

[0005] In view of this, the first object of the present invention is to provide a method for preparing a coal tar pitch-based silicon-carbon composite precursor material.

[0006] The second object of the present invention is to provide a coal tar pitch-based silicon-carbon composite precursor material prepared by the above preparation method.

[0007] The third object of the present invention is to provide a method for preparing a silicon-carbon negative electrode material, which is prepared using the above-mentioned coal tar-based silicon-carbon composite precursor material.

[0008] The fourth object of the present invention is to provide a silicon-carbon negative electrode material prepared by the above preparation method.

[0009] In order to achieve the above object, the present invention adopts the following technical solution:

[0010] In a first aspect, the present invention provides a method for preparing a coal tar pitch-based silicon-carbon composite precursor material, comprising the following steps:

[0011] (1) mixing the high temperature modified coal tar powder with an oxidant, and performing a high temperature modified carbonization reaction under the protection of an inert gas to obtain a modified carbonized product;

[0012] (2) crushing the modified carbonized product obtained in step (1) and mixing it with an activator, heating it to a reaction temperature, and performing an activation reaction under the protection of an inert gas;

[0013] (3) washing and drying the reaction product obtained in step (2), and then deashing and removing impurities;

[0014] (4) demagnetizing the product obtained in step (3) to obtain demagnetized carbon;

[0015] (5) The demagnetized carbon obtained in step (4) is dried and crushed to obtain the coal tar pitch-based silicon-carbon composite precursor material.

[0016] In some embodiments, in step (1), the high temperature modified coal tar pitch refers to the tar distillation residue of coal high temperature dry distillation (1000±50°C), with an ash content of ≤0.1% and a softening point of 106~108°C.

[0017] In some embodiments, in step (1), the particle size of the high temperature modified coal tar powder is less than 100 μm. The high temperature modified coal tar powder having a particle size that meets the requirements can be obtained by crushing and grinding the high temperature modified asphalt and then sieving it.

[0018] In some embodiments, in step (1), the oxidant is one or more oxidizing substances selected from KNO3, NaNO3, HNO3, K2SO4, H2SO4, H2O2, etc., preferably H2SO4. The present invention promotes the lateral activation of high-temperature modified coal tar pitch by introducing a strong oxidant, in particular, by introducing oxygen-containing functional groups (such as NO3 - 、SO4 2- The introduction of this functional group allows the oxidized asphalt molecules to further cross-link during the later carbonization process, effectively preventing the escape of volatile components in the asphalt balls, ensuring that the overall morphology of the asphalt is not destroyed during the carbonization process, further improving the high-temperature thermosetting properties of the carbon source, and regulating the appropriate pore volume, pore size distribution and particle size.

[0019] In some embodiments, in step (1), the mass ratio of the high temperature modified coal tar powder to the oxidant is 1:0.1-0.4, and preferably the mass ratio is 1:0.25-0.3.

[0020] In some embodiments, in step (1), the temperature of the high temperature modification carbonization reaction is 400°C to 900°C, and the time is 2h to 6h; preferably, the temperature is 500°C to 700°C, and the preferred time is 3h to 5h.

[0021] In some embodiments, in step (2), the modified carbonized product obtained in step (1) is crushed to a particle size of less than 100 μm.

[0022] In some embodiments, in step (2), the activator is selected from one or more of KOH, NaOH, KCNS, H3PO4, H2SO4, etc., which can undergo redox reactions with carbon-based substances to generate gaseous substances during the activation reaction to complete the pore opening.

[0023] In some embodiments, in step (2), the mass ratio of the modified carbonized product to the activator is 1:1 to 1:4, preferably 1:2 to 1:3.

[0024] In some embodiments, in step (2), the reaction temperature is 700°C to 900°C, preferably 800°C to 900°C; the activation reaction time is 6h to 8h, preferably 7h to 8h. When the reaction temperature exceeds this range, or the reaction time is too long, the open porosity will be too large and the skeleton strength will be weakened.

[0025] In some embodiments, the high-temperature carbonization modification reaction of step (1) and / or the activation reaction of step (2) can be carried out in a high-temperature rotary furnace.

[0026] In some embodiments, the inert gas used in step (1) and step (2) may be nitrogen, argon or other protective gases.

[0027] In some embodiments, in step (3), the washing is performed using deionized water.

[0028] In some embodiments, in step (4), the content of magnetic substances in the demagnetized carbon after demagnetization is less than 50 ppm.

[0029] In some embodiments, in step (5), the particle size of the coal tar pitch-based silicon-carbon composite precursor material after crushing is less than 1 μm.

[0030] In some embodiments, the drying in steps (3) and (5) is a conventional operation that can achieve material drying, such as oven drying, which is not limited here.

[0031] In a second aspect, the present invention provides a coal tar pitch-based silicon-carbon composite precursor material prepared by the above-mentioned preparation method.

[0032] The coal tar pitch-based silicon-carbon composite precursor material has a suitable particle size and pore size distribution. 50 >6 nm, preferably >7 nm, microporosity greater than 75%, preferably greater than 90%, specific surface area>1750 m 2 / g, preferably>1900 m 2 / g, thus having higher silicon binding properties.

[0033] In a third aspect, the present invention provides a method for preparing a silicon-carbon negative electrode material, which is prepared from the coal tar pitch-based silicon-carbon composite precursor material described in the second aspect, comprising the following steps:

[0034] The coal tar-based silicon-carbon composite precursor material is mixed with a silicon source and a gaseous hydrocarbon in a mass ratio of 1:1:(0.3-0.5). The mixed materials are placed in a CVD furnace for silicon deposition at a reaction temperature of 500-600°C and a reaction time of 5-8h to obtain the silicon-carbon negative electrode material.

[0035] The core of the formation of silicon-carbon negative electrode materials is to store silicon through a porous carbon skeleton. The principle is: silane gas is introduced into the pores of porous carbon particles, and the gas is precipitated into silicon nanoparticles through high-temperature pyrolysis and dispersed in the pores of porous carbon. The silicon-carbon material produced by deposition has uniform components and a relatively dense structure. The voids inside the porous carbon are used to buffer the volume expansion and improve the cycle performance of the negative electrode material.

[0036] In some embodiments, the silicon source is selected from one or more of SiH4, trichlorosilane, and silicon tetrachloride.

[0037] The gaseous hydrocarbon is selected from C 1-3Hydrocarbons such as acetylene, ethylene, propylene, propyne, etc.

[0038] In a fourth aspect, the present invention provides a silicon-carbon negative electrode material prepared by the preparation method described in the third aspect.

[0039] The silicon-carbon negative electrode material has a high silicon content (40% to 55%) while maintaining a high first coulombic efficiency (>80%, even >90%) and good cycle stability. The cycle process efficiency is >97.4%, even >99%, and the gram capacity can reach 1500-2000 mA·h / g.

[0040] It should be understood that the foregoing general description and the following detailed description are only exemplary and illustrative, and are not intended to limit the present invention. The present invention document provides an overview of various implementations or examples of the technology described in the present invention, and is not a comprehensive disclosure of the full scope or all features of the disclosed technology.

[0041] Beneficial Effects

[0042] 1. The preparation method of the coal tar pitch-based silicon-carbon composite precursor material provided by the present invention adopts the carbonization modification of the asphalt raw material by introducing an oxidant to assist in modification. The process is simple, safe and has a high yield, which can make the carbon source easier to handle and the operation process safer.

[0043] 2. The coal tar pitch-based silicon-carbon composite precursor material prepared by the above method has a particle size and pore size distribution that meet the requirements of silicon precipitation, thereby having high silicon binding and skeleton strength. The silicon-carbon negative electrode material prepared from this precursor material has a high silicon loading, a high first coulombic efficiency and good cycle stability.

[0044] 3. The carbon-coated silicon material commonly used in the prior art has low mechanical strength and poor effect in limiting the expansion of silicon-based materials, which can easily cause battery deformation and bulging, and reduce cycle stability. The silicon structure deposited and embedded in the carbon voids used in the present invention has high mechanical strength, and the cracks generated are bent along the direction of the layer, with many branches and large cross-sections. It requires more energy to crack, so it is not easy to crack, or even if it cracks, it is easy to stop, which hinders the formation of large cracks. The silicon expansion can be limited to 20-30%, increasing the cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is the pore size distribution diagram of the coal tar pitch-based silicon-carbon composite precursor material prepared in Example 4.

[0046] Figure 2 This is a scanning electron microscope image of the coal tar pitch-based silicon-carbon composite precursor material prepared in Example 4.

[0047] Figure 3 This is the isothermal adsorption line of the coal tar pitch-based silicon-carbon composite precursor material prepared in Example 4.

[0048] Figure 4 This is a scanning electron microscope image of the silicon-carbon negative electrode material prepared in Example 4. DETAILED DESCRIPTION

[0049] Example 1

[0050] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with concentrated sulfuric acid (98.3 wt%) (calculated as H2SO4 content) at a mass ratio of 1:0.1, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 400 °C and the time was 2 h;

[0051] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator H3PO4 at a mass ratio of 1:1; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 700°C for 6 hours;

[0052] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0053] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0054] (5) Dry the demagnetized carbon, and place the powder in a grinder for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material are tested, and the specific data are shown in Table 1. The particle size and pore size distribution are suitable and can meet the silicon precipitation requirements of the subsequent process.

[0055] (6) Preparation of silicon-carbon negative electrode material: The coal tar-based silicon-carbon composite precursor material prepared by steps (1) to (5) is mixed with silane and acetylene in a mass ratio of 1:1:0.3. The mixed materials are placed in a CVD furnace for silicon deposition. The reaction temperature is 500°C and the reaction time is 6 hours. The resulting material is the silicon-carbon negative electrode material.

[0056] The obtained silicon-carbon negative electrode material was used as a half-cell for performance testing, and the silicon loading rate, coulombic efficiency, gram capacity, and cycle performance were tested respectively. The data obtained are shown in Table 2.

[0057] Example 2

[0058] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with concentrated sulfuric acid (98.3 wt%) (calculated as H2SO4 content) at a mass ratio of 1:0.2, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 500 °C and the time was 2 h;

[0059] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator H3PO4 at a mass ratio of 1:1; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 800°C and a time of 7 hours;

[0060] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0061] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0062] (5) Dry the demagnetized carbon, and place the powder in a grinder for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material are tested, and the specific data are shown in Table 1. The particle size and pore size distribution are suitable and can meet the silicon precipitation requirements of the subsequent process.

[0063] (6) Preparation of silicon-carbon negative electrode material: The coal tar-based silicon-carbon composite precursor material prepared by steps (1) to (5) is mixed with silane and acetylene in a mass ratio of 1:1:0.3. The mixed materials are placed in a CVD furnace for silicon deposition. The reaction temperature is 500°C and the reaction time is 6 hours. The resulting material is the silicon-carbon negative electrode material.

[0064] The obtained silicon-carbon negative electrode material was used as a half-cell for performance testing, and the silicon loading rate, coulombic efficiency, gram capacity, and cycle performance were tested respectively. The data obtained are shown in Table 2.

[0065] Example 3

[0066] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with concentrated sulfuric acid (98.3 wt%) (calculated as H2SO4 content) at a mass ratio of 1:0.25, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 500 °C and the time was 3 h;

[0067] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator H3PO4 at a mass ratio of 1:2; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 800°C for 7 hours;

[0068] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0069] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0070] (5) Dry the demagnetized carbon, and place the powder in a grinder for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material are tested, and the specific data are shown in Table 1. The particle size and pore size distribution are suitable and can meet the silicon precipitation requirements of the subsequent process.

[0071] (6) Preparation of silicon-carbon negative electrode material: The coal tar-based silicon-carbon composite precursor material prepared by steps (1) to (5) is mixed with silane and acetylene in a mass ratio of 1:1:0.3. The mixed materials are placed in a CVD furnace for silicon deposition. The reaction temperature is 500°C and the reaction time is 6 hours. The resulting material is the silicon-carbon negative electrode material.

[0072] The obtained silicon-carbon negative electrode material was used as a half-cell for performance testing, and the silicon loading rate, coulombic efficiency, gram capacity, and cycle performance were tested respectively. The obtained data on particle size, microporosity, specific surface area, and silicon loading rate are shown in Table 2.

[0073] Example 4

[0074] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with concentrated sulfuric acid (98.3 wt%) (calculated as H2SO4 content) at a mass ratio of 1:0.25, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 600 °C and the time was 3 h;

[0075] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator H3PO4 at a mass ratio of 1:2; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 900°C for 7 hours;

[0076] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0077] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0078] (5) Dry the demagnetized carbon, and place the powder in a pulverizer for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material are tested, and the pore size distribution diagram, scanning electron microscopy diagram, and isothermal adsorption curve are shown in FIG. Figure 1-3 , specific data are shown in Table 1. Its particle size and pore size distribution are suitable and can meet the requirements of silicon deposition in subsequent processes.

[0079] (6) Preparation of silicon-carbon negative electrode material: The coal tar-based silicon-carbon composite precursor material prepared by steps (1) to (5) is mixed with silane and acetylene in a mass ratio of 1:1:0.3. The mixed materials are placed in a CVD furnace for silicon deposition. The reaction temperature is 500°C and the reaction time is 6 hours. The resulting material is the silicon-carbon negative electrode material.

[0080] The obtained silicon-carbon negative electrode material was used as a half-cell for performance testing, and the silicon loading rate, coulombic efficiency, gram capacity, and cycle performance were tested. The obtained scanning electron microscope images are shown in Figure 4 The data obtained are shown in Table 2.

[0081] Example 5

[0082] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with concentrated sulfuric acid (98.3 wt%) (calculated as H2SO4 content) at a mass ratio of 1:0.25, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 600 °C and the time was 3 h;

[0083] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator H3PO4 at a mass ratio of 1:2; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 900°C for 8 hours;

[0084] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0085] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0086] (5) Dry the demagnetized carbon, and place the powder in a grinder for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material are tested, and the specific data are shown in Table 1. The particle size and pore size distribution are suitable and can meet the silicon precipitation requirements of the subsequent process.

[0087] (6) Preparation of silicon-carbon negative electrode material: The coal tar-based silicon-carbon composite precursor material prepared by steps (1) to (5) is mixed with silane and acetylene in a mass ratio of 1:1:0.3. The mixed materials are placed in a CVD furnace for silicon deposition. The reaction temperature is 500°C and the reaction time is 6 hours. The resulting material is the silicon-carbon negative electrode material.

[0088] The obtained silicon-carbon negative electrode material was used as a half-cell for performance testing, and the silicon loading rate, coulombic efficiency, gram capacity, and cycle performance were tested respectively. The data obtained are shown in Table 2.

[0089] Example 6

[0090] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with concentrated sulfuric acid (98.3wt%) (calculated as H2SO4 content) at a mass ratio of 1:0.3, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 700°C and the time was 4 h;

[0091] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator H3PO4 at a mass ratio of 1:2; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 900°C for 7 hours;

[0092] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0093] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0094] (5) Dry the demagnetized carbon, and place the powder in a grinder for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material are tested, and the specific data are shown in Table 1. The particle size and pore size distribution are suitable and can meet the silicon precipitation requirements of the subsequent process.

[0095] (6) Preparation of silicon-carbon negative electrode material: The coal tar-based silicon-carbon composite precursor material prepared by steps (1) to (5) is mixed with silane and acetylene in a mass ratio of 1:1:0.3. The mixed materials are placed in a CVD furnace for silicon deposition. The reaction temperature is 500°C and the reaction time is 6 hours. The resulting material is the silicon-carbon negative electrode material.

[0096] The obtained silicon-carbon negative electrode material was used as a half-cell for performance testing, and the silicon loading rate, coulombic efficiency, gram capacity, and cycle performance were tested respectively. The data obtained are shown in Table 2.

[0097] Example 7

[0098] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with concentrated sulfuric acid (98.3wt%) (calculated as H2SO4 content) at a mass ratio of 1:0.3, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 700°C and the time was 5 h;

[0099] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator H3PO4 at a mass ratio of 1:2; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 900°C for 8 h;

[0100] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0101] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0102] (5) Dry the demagnetized carbon, and place the powder in a grinder for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material are tested, and the specific data are shown in Table 1. The particle size and pore size distribution are suitable and can meet the silicon precipitation requirements of the subsequent process.

[0103] (6) Preparation of silicon-carbon negative electrode material: The coal tar-based silicon-carbon composite precursor material prepared by steps (1) to (5) is mixed with silane and acetylene in a mass ratio of 1:1:0.3. The mixed materials are placed in a CVD furnace for silicon deposition. The reaction temperature is 500°C and the reaction time is 6 hours. The resulting material is the silicon-carbon negative electrode material.

[0104] The obtained silicon-carbon negative electrode material was used as a half-cell for performance testing, and the silicon loading rate, coulombic efficiency, gram capacity, and cycle performance were tested respectively. The data obtained are shown in Table 2.

[0105] Comparative Example 1

[0106] (1) Take 1 kg of high-temperature modified coal tar and place it in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder is less than 100 μm; mix the coal tar powder with the required particle size with the activator H3PO4 at a mass ratio of 1:2; after mixing, the materials enter a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for activation reaction. The activation reaction temperature is 900°C and the time is 7 hours;

[0107] Without the introduction of strong oxidants, the modified coal tar cannot undergo a modification and carbonization reaction. At the set activation temperature, the modified coal tar is in a liquid state and cannot be solidified into a shape.

[0108] Comparative Example 2

[0109] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with H2SO4 at a mass ratio of 1:0.25, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 600 °C and the time was 3 h;

[0110] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator KOH at a mass ratio of 1:2; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 1000°C for 9 hours;

[0111] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0112] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0113] (5) Dry the demagnetized carbon, and place the powder in a pulverizer for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material are tested, and the specific data are shown in Table 1. The porosity is low (34%), and the specific surface area is small (1725.77 m 2 / g) cannot meet the silicon deposition requirements of the subsequent process.

[0114] Comparative Example 3

[0115] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with H2SO4 at a mass ratio of 1:0.25, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 600 °C and the time was 3 h;

[0116] (2) The modified carbonized product is placed in a ball mill for crushing and grinding to a particle size of less than 100 μm; the modified carbonized product with the required particle size is mixed with the activator H3PO4 at a mass ratio of 1:2; the mixed materials are placed in a high-temperature rotary furnace under the protection of an inert gas such as nitrogen or helium for an activation reaction at a temperature of 700°C for 5 h;

[0117] (3) Place the activated material in a corrosion-resistant sealed container and wash it with deionized water. After washing, dry, deash and remove impurities from the material;

[0118] (4) The demagnetized material is placed in a demagnetizer for demagnetization. The content of magnetic substances in the demagnetized carbon after demagnetization is less than 50ppm;

[0119] (5) Dry the demagnetized carbon, and place the powder in a grinder for further crushing to a particle size of <1 μm, thereby obtaining a coal tar pitch-based silicon-carbon composite precursor material. The particle size, pore size distribution, and specific surface area of ​​the obtained coal tar pitch-based silicon-carbon composite precursor material were tested, and the specific data are shown in Table 1. Its porosity is low (48%) and its comparative surface area is small (1187.47 m2 / g), which cannot meet the silicon precipitation requirements of the subsequent process.

[0120] Comparative Example 4

[0121] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with H2SO4 at a mass ratio of 1:0.25, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 200 °C and the time was 3 h;

[0122] Under low-temperature reaction conditions, there is not enough energy for the modification carbonization reaction to proceed. At the set temperature, the modified coal tar will still be in a liquid state and cannot be solidified into shape. The activation reaction cannot be carried out in the subsequent activation stage.

[0123] Comparative Example 5

[0124] (1) 1 kg of high-temperature modified coal tar was placed in a ball mill for crushing and grinding until the particle size of the high-temperature modified coal tar powder was less than 100 μm; the high-temperature modified coal tar powder with the required particle size was mixed with H2SO4 at a mass ratio of 1:0.25, and the mixed materials were placed in a high-temperature rotary furnace under the protection of inert gas such as nitrogen and helium for modification and carbonization reaction to obtain a modified carbonized product; the temperature of the modification and carbonization reaction was 1100°C and the time was 3 h;

[0125] Under the overly high temperature environment, the mixed material undergoes implosion, causing the molecules to rapidly aggregate in a short period of time, forming large polymers with irregular structures, and forming large agglomerates in the high-temperature rotary kiln. The activation reaction cannot be carried out in the subsequent activation step.

[0126] Experimental Example 1

[0127] The particle size of the coal tar pitch-based silicon-carbon composite precursor materials prepared in Examples 1-7 and Comparative Examples 1-3 was measured using a laser particle size analyzer, and the microporosity and specific surface area of ​​the coal tar pitch-based silicon-carbon composite precursor materials prepared in Examples 1-7 and Comparative Examples 1-3 were measured using an adsorption instrument.

[0128] Experimental Example 2

[0129] The silicon loading of the carbon-silicon negative electrode material prepared in Examples 1-7 was measured using a carbon-sulfur meter. The first coulombic efficiency and gram capacity were measured using 91% silicon-carbon negative electrode material, 6% LA132 binder, and 3% Super P conductive agent. The single-cycle attenuation rate of 0.5C was less than 0.1%. The half-battery cycle test was repeated 3 times, and the average value of the test results was taken.

[0130] Table 1

[0131]

[0132] Table 2

[0133]

[0134] As shown in Tables 1 and 2, the product prepared by the method for preparing the coal tar pitch-based silicon-carbon composite precursor material provided by the present invention has a suitable particle size and microporosity, perfectly adapts to the silicon deposition requirements of the silicon-carbon negative electrode material, and has good silicon binding performance. The silicon-carbon negative electrode material prepared based on this precursor material has a gram capacity far exceeding that of existing negative electrode materials, and has good first coulomb efficiency and cycle process efficiency.

[0135] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a coal tar pitch-based silicon-carbon composite precursor material, characterized in that: The preparation method comprises the following steps: (1) mixing the high temperature modified coal tar powder with an oxidant, and performing a high temperature modified carbonization reaction under the protection of an inert gas to obtain a modified carbonized product; (2) crushing the modified carbonized product obtained in step (1) and mixing it with an activator, heating it to a reaction temperature, and performing an activation reaction under the protection of an inert gas; (3) washing and drying the reaction product obtained in step (2), and then deashing and removing impurities; (4) demagnetizing the product obtained in step (3) to obtain demagnetized carbon; (5) drying and crushing the demagnetized carbon obtained in step (4) to obtain the coal tar pitch-based silicon-carbon composite precursor material; Wherein, in step (1): the oxidant is one or more selected from KNO3, NaNO3, HNO3, K2SO4, H2SO4, H2O2; and / or, the mass ratio of the high temperature modified coal tar powder to the oxidant is 1:0.1-0.4; and / or, the temperature of the high temperature modified carbonization reaction is 400°C-900°C, and the time is 2h-6h; In step (2): the activator is selected from one or more of KOH, NaOH, KCNS, H2SO4, H3PO4; and / or the mass ratio of the modified carbonized product to the activator is 1:1 to 1:4; and / or the reaction temperature is 700°C to 900°C, and the reaction time of the activation reaction is 6h to 8h.

2. The method for preparing the coal tar pitch-based silicon-carbon composite precursor material according to claim 1, characterized in that: In step (1): the particle size of the high temperature modified coal tar powder is less than 100 μm.

3. The method for preparing the coal tar pitch-based silicon-carbon composite precursor material according to claim 1, characterized in that: In step (2): the modified carbonized product obtained in step (1) is crushed to a particle size of less than 100 μm.

4. The method for preparing the coal tar pitch-based silicon-carbon composite precursor material according to claim 1, characterized in that: In step (3): the washing is performed using deionized water.

5. The method for preparing the coal tar pitch-based silicon-carbon composite precursor material according to claim 1, characterized in that: In step (4): the content of magnetic material in the demagnetized carbon after demagnetization is less than 50 ppm.

6. The method for preparing the coal tar pitch-based silicon-carbon composite precursor material according to claim 1, characterized in that: In step (5): the particle size of the coal tar pitch-based silicon-carbon composite precursor material after crushing is less than 1 μm.

7. The coal tar pitch based silicon-carbon composite precursor material prepared by the method for preparing the coal tar pitch based silicon-carbon composite precursor material according to any one of claims 1 to 6.

8. A method for preparing a silicon-carbon negative electrode material, characterized in that: The silicon-carbon negative electrode material is prepared from the coal tar pitch-based silicon-carbon composite precursor material according to claim 7, comprising the following steps: The coal tar-based silicon-carbon composite precursor material is mixed with a silicon source and a gaseous hydrocarbon in a mass ratio of 1:1:(0.3-0.5). The mixed materials are placed in a CVD furnace for silicon deposition at a reaction temperature of 500-600°C and a reaction time of 5-8h to obtain the silicon-carbon negative electrode material.

9. The method for preparing the silicon-carbon negative electrode material according to claim 8, characterized in that: The silicon source is selected from one or more of SiH4, trichlorosilane, and silicon tetrachloride; The gaseous hydrocarbon is selected from C 1-3 hydrocarbon.

10. The silicon-carbon negative electrode material prepared by the method for preparing the silicon-carbon negative electrode material according to claim 8 or 9.

Citation Information

Patent Citations

  • Silicon-carbon negative electrode material and preparation method thereof, negative electrode plate and secondary battery

    CN114044516A

  • Silicon-carbon composite negative electrode material and preparation method thereof

    CN115663132A

  • Preparation method of silicon-carbon negative electrode material

    CN116605875A

  • Preparation method of asphalt-based silicon-carbon negative electrode material for lithium ion battery and product of asphalt-based silicon-carbon negative electrode material

    CN116730322A

  • Activated carbon and preparation method and application thereof, demercuration activated carbon and preparation method and application thereof