A preparation process of negative oxygen ion crystal breathing brick
Through the preparation process of negative oxygen ion crystal respiratory bricks, the problems of poor water permeability and insufficient purification capacity in heavy rainy weather are solved, and high water permeability, compressive resistance and sterilization functions are achieved, which significantly improves the environment and human health.
Patent Information
- Application Number
- CN202410753999.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-12
AI Technical Summary
The existing breathing bricks have poor water permeability during heavy rainy weather, limited anti-slip and wear resistance, cannot purify the air, cannot eliminate PM2.5 pollution, and lack the function of killing viruses and bacteria.
The preparation process of negative oxygen ion crystal respiratory bricks is adopted. By mixing solid raw materials such as cartilage, quartz sand, basalt fibers with polymer composite materials and nanomaterials, it is compacted, dried, sintered, polished and sprayed to form a high-quality Large pore bricks with water permeability and compressive resistance, and spray negative oxygen ion-generating materials on the surface to enhance their sterilization and purification capabilities.
It achieves high water permeability and compressive resistance, can quickly penetrate rainwater, reduce urban drainage burden, purify air, eliminate PM2.5 pollution, and has powerful sterilization function to improve human health and the environment.
Abstract
Description
[0001] The invention relates to the technical field of breathing brick preparation technology, and in particular to a preparation technology of a negative oxygen ion crystal breathing brick. Background Art
[0002] The functions of traditional breathing bricks on the market are relatively simple. When encountering heavy rain, rainwater cannot quickly penetrate the surface into the ground, resulting in limited anti-slip and wear-resistant effects. They are also unable to purify the air, cannot eliminate PM2.5 pollution, and do not have the function of killing viruses and bacteria. Therefore, there is an urgent need to set up a breathing brick that allows rainwater to penetrate efficiently, has high pressure resistance, noise reduction and anti-slip properties, has the function of regulating the urban heat island effect, is low-carbon and environmentally friendly, and can also regulate human physiological functions, promote metabolism, prevent colds and respiratory diseases, improve cardiovascular and cerebrovascular diseases, kill viruses and bacteria, eliminate PM2.5 pollution, and strongly decompose formaldehyde, so as to improve the functionality of breathing bricks. Summary of the invention
[0003] In order to overcome the problem that during the use of breathing bricks, rainwater cannot quickly penetrate the surface into the ground when encountering heavy rain, resulting in limited anti-slip and wear-resistant effects, and unable to purify the air, unable to eliminate PM2.5 pollution, and at the same time lacking the function of killing viruses and bacteria.
[0004] The technical solution of the present invention is: a preparation process of a negative oxygen ion crystal breathing brick, the steps of which are as follows;
[0005] Step 1: Prepare the ingredients
[0006] Prepare solid raw materials of 30-40 parts of corundum, 25-35 parts of quartz sand, and 22-33 parts of basalt fiber, and also prepare a polymer composite material of 5-10 parts of polyethylene, 6-12 parts of polypropylene, 6-15 parts of polyvinyl chloride, 8-18 parts of polyester, and 5-12 parts of epoxy resin;
[0007] Step 2: Mix the ingredients
[0008] Put the materials of step 1 into a mixing device, gradually add 6-10 parts of tourmaline, 7-12 parts of vermiculite, and 8-15 parts of nanomaterials to generate negative oxygen ions, and continue stirring until completely mixed. The nanomaterials are specifically one or more of nano titanium dioxide, nano zinc oxide, nano silicon dioxide, nano calcium carbonate, nano copper, nano silver, and nano nickel;
[0009] Step 3: Initial Forming
[0010] Pour the mixed material in step 2 into the mold and compact it using a press or vibrating table to form the preliminary shape of the brick;
[0011] Step 4: Drying
[0012] Place the formed bricks in a drying room or oven for drying to remove excess moisture and improve the strength of the bricks;
[0013] Step 5: Sintering
[0014] The dried bricks are placed in a sintering furnace for high-temperature sintering to solidify them and obtain the required strength. The sintering temperature of the bricks during the bricklaying process is between 800°C and 1200°C, the heat preservation time is between 2 hours and 50 hours, and the cooling rate of the bricks is within the range of 1°C / min to 10°C / min;
[0015] Step 6: Surface polishing
[0016] Use a hand-held grinder or electric sandpaper machine to grind the brick surface to remove the rough parts and unevenness of the surface. Gradually use sandpaper or grinding heads of different coarseness and fineness as needed until the required surface smoothness is achieved;
[0017] Step 7: Surface spraying
[0018] Prepare the spray paint in advance, make sure the paint is fully stirred and then prime the brick surface to allow the paint to adhere better. Then use a spray gun to evenly apply the surface paint. After the paint is dry and solidified, spray it multiple times as needed.
[0019] Step 8: Inspection and Packaging
[0020] The prepared negative oxygen ion crystal breathing bricks are quality inspected to ensure compliance with relevant standards. After the inspection is completed, the products are packaged and prepared for sale or use.
[0021] Beneficial effects of the present invention:
[0022] 1. The water permeability of the crystal breathing brick of the present invention is ≥1.5×10^(-2)cm / s. It has a strong water permeability function and a very high porosity. In particular, it has more connecting holes. The water permeability is above 20mm / s, which is more than twice the standard of similar domestic products. It can cope with a rainfall of 60mm / h. Even if it rains heavily, rainwater can quickly penetrate the surface into the ground, which not only reduces the burden on the urban drainage system, but also reduces the pollution to public waters; restore the natural water storage capacity of the earth, and through the construction of sponge cities, minimize the impact of urban development and construction on the ecological environment, and absorb and utilize 70% of the rainfall on the spot, and also achieve the appearance effect of granite stone, and overcome the disadvantages of natural stone with color difference, cracks, radiation, and impermeability. It belongs to green and environmentally friendly building materials. The product with the addition of basalt fiber is formed by high pressure, and its compressive and flexural strengths are higher than other ground paving materials, 8CM Thick crystal breathing bricks can achieve the effect of driving and parking. The bearing strength reaches 8.9MPa, which can absorb the noise generated by running vehicles and create a safe and comfortable traffic environment. Due to the high-strength water-permeable effect, it can instantly absorb floating water and has a good anti-slip effect. The fabric is made of high-strength corundum and polymer composite materials with good wear resistance (wear resistance 31MM, anti-slip 84), there is no water on the road surface on rainy days, which prevents reflection at night and improves the safety and comfort of vehicles and pedestrians. Its excellent water permeability and breathability can regulate the temperature and humidity of the surface, eliminate the "heat island effect" and maintain the ecological balance of the surface. The product has a long life, is weathering-resistant, and can be reused an unlimited number of times. It can regulate human physiological functions, promote metabolism, prevent colds and respiratory diseases, and improve cardiovascular and cerebrovascular diseases. Negative oxygen ions have powerful bactericidal and disinfection functions. Tests by authoritative professional organizations have shown that its sterilization rate is as high as over 99%. PM2.5 particles are tiny and it is difficult to remove them with conventional filters, but negative oxygen ions have unique advantages in dealing with PM2.5. It carries negative ions and is easy to combine with particles, agglomerate into dust and fall to the ground. Negative oxygen ions are very active and will actively capture formaldehyde (CH2O) and then force it to decompose. DETAILED DESCRIPTION
[0023] This specific implementation method is a preparation process of a negative oxygen ion crystal breathing brick, and the steps are as follows:
[0024] Step 1: Prepare the ingredients
[0025] Prepare solid raw materials of 30-40 parts of corundum, 25-35 parts of quartz sand, and 22-33 parts of basalt fiber, and also prepare a polymer composite material of 5-10 parts of polyethylene, 6-12 parts of polypropylene, 6-15 parts of polyvinyl chloride, 8-18 parts of polyester, and 5-12 parts of epoxy resin;
[0026] Step 2: Mix the ingredients
[0027] Put the materials of step 1 into a mixing device, gradually add 6-10 parts of tourmaline, 7-12 parts of vermiculite, and 8-15 parts of nanomaterials to generate negative oxygen ions, and continue stirring until completely mixed. The nanomaterials are specifically one or more of nano titanium dioxide, nano zinc oxide, nano silicon dioxide, nano calcium carbonate, nano copper, nano silver, and nano nickel. The mixing device is a horizontal ribbon mixer or a double-shaft mixer, and the temperature is between room temperature and 70-80 degrees Celsius.
[0028] Step 3: Initial Forming
[0029] Pour the mixed material in step 2 into the mold and compact it using a press or a vibrating table to form the initial shape of the brick body. The pressure of the press during use is between 500 kPa and 1000 kPa.
[0030] Step 4: Drying
[0031] Place the formed bricks in a drying room or oven for drying to remove excess moisture and improve the strength of the bricks. The drying time is between two hours and twenty hours, and the drying temperature is between 60°C and 100°C.
[0032] Step 5: Sintering
[0033] The dried bricks are placed in a sintering furnace for high-temperature sintering to solidify them and obtain the required strength. The sintering temperature of the bricks during the bricklaying process is between 800°C and 1200°C, the heat preservation time is between 2 hours and 50 hours, and the cooling rate of the bricks is within the range of 1°C / min to 10°C / min;
[0034] Step 6: Surface polishing
[0035] Use a hand-held grinder or electric sandpaper machine to grind the brick surface to remove the rough parts and unevenness of the surface. Gradually use sandpaper or grinding heads of different coarseness and fineness as needed until the required surface smoothness is achieved. The grinding speed of the hand-held grinder is between 100 and 600 revolutions per minute. The coarse sandpaper used in the electric sandpaper machine is used to remove larger defects, while the fine sandpaper is used for fine grinding. The coarseness of the sandpaper is between 180 mesh and 2400 mesh.
[0036] Step 7: Surface spraying
[0037] Prepare the spray paint in advance, make sure the paint is fully stirred and then prime the brick surface to make the paint adhere better, then use a spray gun to evenly apply the surface paint, wait for the paint to dry and solidify, and spray multiple times as needed. The distance between the spray gun and the brick surface is between 12 and 24 inches. The spraying speed should be kept uniform, between 20 and 50 square feet per hour, and the spraying pressure is between 20 and 40PSI. After spraying the primer once, the surface paint can be sprayed 1 to 3 times as needed. Wait for the previous coat of paint to dry and solidify between each coat. The primer needs 5 minutes to 6 hours to dry.
[0038] Step 8: Inspection and Packaging
[0039] The prepared negative oxygen ion crystal breathing bricks are quality inspected to ensure compliance with relevant standards. After the inspection is completed, the products are packaged and prepared for sale or use. Example 1
[0040] The preparation process steps of negative oxygen ion crystal breathing bricks are as follows:
[0041] Step 1: Prepare the ingredients
[0042] Prepare solid raw materials of 40 parts of corundum, 35 parts of quartz sand, and 30 parts of basalt fiber, and also prepare a polymer composite material of 10 parts of polyethylene, 11 parts of polypropylene, 12 parts of polyvinyl chloride, 15 parts of polyester, and 12 parts of epoxy resin;
[0043] Step 2: Mix the ingredients
[0044] Put the materials from step 1 into a mixing device, gradually add 10 parts of tourmaline, 10 parts of vermiculite, and 12 parts of nanomaterials for generating negative oxygen ions, and continue stirring until completely mixed;
[0045] Step 3: Initial Forming
[0046] Pour the mixed material in step 2 into the mold and compact it using a press or vibrating table to form the preliminary shape of the brick;
[0047] Step 4: Drying
[0048] Place the formed bricks in a drying room or oven for drying to remove excess moisture and improve the strength of the bricks;
[0049] Step 5: Sintering
[0050] The dried bricks are placed in a sintering furnace for high-temperature sintering to solidify them and obtain the required strength;
[0051] Step 6: Surface polishing
[0052] Use a hand-held grinder or electric sandpaper machine to grind the brick surface to remove the rough parts and unevenness of the surface. Gradually use sandpaper or grinding heads of different coarseness and fineness as needed until the required surface smoothness is achieved;
[0053] Step 7: Surface spraying
[0054] Prepare the spray paint in advance, make sure the paint is fully stirred and then prime the brick surface to allow the paint to adhere better. Then use a spray gun to evenly apply the surface paint. After the paint is dry and solidified, spray it multiple times as needed.
[0055] Step 8: Inspection and Packaging
[0056] The prepared negative oxygen ion crystal breathing bricks are quality inspected to ensure compliance with relevant standards. After the inspection is completed, the products are packaged and prepared for sale or use. Example 2
[0057] The preparation process steps of negative oxygen ion crystal breathing bricks are as follows:
[0058] Step 1: Prepare the ingredients
[0059] Prepare solid raw materials of 35 parts of corundum, 29 parts of quartz sand, and 25 parts of basalt fiber, and also prepare a polymer composite material of 8 parts of polyethylene, 9 parts of polypropylene, 12 parts of polyvinyl chloride, 14 parts of polyester, and 10 parts of epoxy resin;
[0060] Step 2: Mix the ingredients
[0061] Put the materials of step 1 into a mixing device, gradually add 8 parts of tourmaline, 8 parts of vermiculite, and 11 parts of nanomaterials for generating negative oxygen ions, and continue stirring until completely mixed;
[0062] Step 3: Initial Forming
[0063] Pour the mixed material in step 2 into the mold and compact it using a press or vibrating table to form the preliminary shape of the brick;
[0064] Step 4: Drying
[0065] Place the formed bricks in a drying room or oven for drying to remove excess moisture and improve the strength of the bricks;
[0066] Step 5: Sintering
[0067] The dried bricks are placed in a sintering furnace for high-temperature sintering to solidify them and obtain the required strength;
[0068] Step 6: Surface polishing
[0069] Use a hand-held grinder or electric sandpaper machine to grind the brick surface to remove the rough parts and unevenness of the surface. Gradually use sandpaper or grinding heads of different coarseness and fineness as needed until the required surface smoothness is achieved;
[0070] Step 7: Surface spraying
[0071] Prepare the spray paint in advance, make sure the paint is fully stirred and then prime the brick surface to allow the paint to adhere better. Then use a spray gun to evenly apply the surface paint. After the paint is dry and solidified, spray it multiple times as needed.
[0072] Step 8: Inspection and Packaging
[0073] The prepared negative oxygen ion crystal breathing bricks are quality inspected to ensure compliance with relevant standards. After the inspection is completed, the products are packaged and prepared for sale or use. Example 3
[0074] The preparation process steps of negative oxygen ion crystal breathing bricks are as follows:
[0075] Step 1: Prepare the ingredients
[0076] Prepare solid raw materials of 30 parts of corundum, 25 parts of quartz sand, and 22 parts of basalt fiber, and also prepare a polymer composite material of 5 parts of polyethylene, 6 parts of polypropylene, 6 parts of polyvinyl chloride, 8 parts of polyester, and 5 parts of epoxy resin;
[0077] Step 2: Mix the ingredients
[0078] Put the materials from step 1 into a mixing device, gradually add 6 parts of tourmaline, 7 parts of vermiculite, and 8 parts of nanomaterials for generating negative oxygen ions, and continue stirring until completely mixed;
[0079] Step 3: Initial Forming
[0080] Pour the mixed material in step 2 into the mold and compact it using a press or vibrating table to form the preliminary shape of the brick;
[0081] Step 4: Drying
[0082] Place the formed bricks in a drying room or oven for drying to remove excess moisture and improve the strength of the bricks;
[0083] Step 5: Sintering
[0084] The dried bricks are placed in a sintering furnace for high-temperature sintering to solidify them and obtain the required strength;
[0085] Step 6: Surface polishing
[0086] Use a hand-held grinder or electric sandpaper machine to grind the brick surface to remove the rough parts and unevenness of the surface. Gradually use sandpaper or grinding heads of different coarseness and fineness as needed until the required surface smoothness is achieved;
[0087] Step 7: Surface spraying
[0088] Prepare the spray paint in advance, make sure the paint is fully stirred and then prime the brick surface to allow the paint to adhere better. Then use a spray gun to evenly apply the surface paint. After the paint is dry and solidified, spray it multiple times as needed.
[0089] Step 8: Inspection and Packaging
[0090] The prepared negative oxygen ion crystal breathing bricks are quality inspected to ensure compliance with relevant standards. After the inspection is completed, the products are packaged and prepared for sale or use.
Claims
1. A preparation process of a negative oxygen ion crystal breathing brick, characterized in that: The steps are as follows: Step 1: Prepare the ingredients Prepare solid raw materials of 30-40 parts of corundum, 25-35 parts of quartz sand, and 22-33 parts of basalt fiber, and also prepare a polymer composite material of 5-10 parts of polyethylene, 6-12 parts of polypropylene, 6-15 parts of polyvinyl chloride, 8-18 parts of polyester, and 5-12 parts of epoxy resin; Step 2: Mix the ingredients Put the materials of step 1 into a mixing device, gradually add 6-10 parts of tourmaline, 7-12 parts of vermiculite, and 8-15 parts of nanomaterials to generate negative oxygen ions, and continue stirring until completely mixed. The nanomaterials are specifically one or more of nano titanium dioxide, nano zinc oxide, nano silicon dioxide, nano calcium carbonate, nano copper, nano silver, and nano nickel; Step 3: Initial Forming Pour the mixed material in step 2 into the mold and compact it using a press or vibrating table to form the preliminary shape of the brick body; Step 4: Drying Place the formed bricks in a drying room or oven for drying to remove excess moisture and improve the strength of the bricks; Step 5: Sintering The dried bricks are placed in a sintering furnace for high-temperature sintering to solidify them and obtain the required strength. The sintering temperature of the bricks during the bricklaying process is between 800°C and 1200°C, the heat preservation time is between 2 hours and 50 hours, and the cooling rate of the bricks is within the range of 1°C / min to 10°C / min; Step 6: Surface polishing Use a hand-held grinder or electric sandpaper machine to grind the brick surface to remove the rough parts and unevenness of the surface. Gradually use sandpaper or grinding heads of different coarseness and fineness as needed until the required surface smoothness is achieved; Step 7: Surface spraying Prepare the spray paint in advance, make sure the paint is fully stirred and then prime the brick surface to allow the paint to adhere better. Then use a spray gun to evenly apply the surface paint. After the paint is dry and solidified, spray it multiple times as needed. Step 8: Inspection and Packaging The prepared negative oxygen ion crystal breathing bricks are quality inspected to ensure compliance with relevant standards. After the inspection is completed, the products are packaged and prepared for sale or use.
2. The preparation process of a negative oxygen ion crystal breathing brick according to claim 1, characterized in that: The mixing device in step 2 adopts a horizontal ribbon mixer or a double-shaft mixer, and the temperature is between room temperature and 70-80 degrees Celsius.
3. The preparation process of a negative oxygen ion crystal breathing brick according to claim 1, characterized in that: The pressure of the press used in step 3 is between 500 kPa and 1000 kPa during use.
4. The preparation process of a negative oxygen ion crystal breathing brick according to claim 1, characterized in that: In step 4, the drying time is between two hours and twenty hours, and the drying temperature is between 60°C and 100°C.
5. The preparation process of a negative oxygen ion crystal breathing brick according to claim 1, characterized in that: In step six, the grinding speed of the handheld grinder is between 100 and 600 revolutions per minute. The coarse sandpaper used in the electric sandpaper machine is used to remove larger defects, while the fine sandpaper is used for fine grinding. The coarseness of the sandpaper is between 180 mesh and 2400 mesh.
6. The preparation process of a negative oxygen ion crystal breathing brick according to claim 1, characterized in that: In step 7, the distance between the spray gun and the brick surface should be between 12 and 24 inches, the spraying speed should be kept uniform, between 20 and 50 square feet per hour, and the spraying pressure should be between 20 and 40 PSI.
7. The preparation process of a negative oxygen ion crystal breathing brick according to claim 1, characterized in that: In step seven, spray the primer once, and spray the surface paint 1 to 3 times as needed. Between each coat, wait for the previous coat of paint to dry and solidify. The primer needs 5 minutes to 6 hours to dry.