Environmentally friendly unsaturated polyester resin and preparation method thereof

By using raw materials such as specific dibasic acids, alcohols and acrylates in environmentally friendly unsaturated polyester resins, combined with ingredients such as caffeic acid and zinc titanate, the problems of insufficient chemical stability and high content of volatile organic compounds have been solved and achieved Higher oxidation resistance and durability reduce the risk of pollution to the environment and human body caused by environmentally friendly unsaturated polyester resin.

CN118496428BActive Publication Date: 2024-10-01CHENGDU DA GIONEE SYNTHETIC MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410957767.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Existing environmentally friendly unsaturated polyester resins have problems such as insufficient chemical stability, high content of volatile organic compounds, and potential risks to the environment and human health.

Method used

Using itaconic acid, 2,5-furandicarboxylic acid and succinic acid as dibasic acids, 1,3-propanediol, 2-vinylpropane-1,3-diol and isosorbide as diols, combined with epoxy Acrylate, 2-[3-(2H-benzotriazol-2-yl)-4-hydroxyphenyl ] Ethyl-2-methacrylate and 4-hydroxyethyloxybenzophenone methacrylate, adding caffeic acid, zinc titanate and organic acid anhydride-modified tetrabutyl titanate, etc., through specific Molar ratio and reaction steps, adjust curing speed and performance, improve chemical stability and mechanical properties.

Benefits of technology

Significantly improve the chemical stability, oxidation resistance and UV resistance of environmentally friendly unsaturated polyester resin, reduce the content of volatile organic compounds, reduce the risk of pollution to the environment and human body, and improve the reliability and use of materials life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention belongs to the technical field of polyester resins, and specifically relates to an environmentally friendly unsaturated polyester resin and a preparation method thereof. The preparation method comprises the following steps: S1, mixing a dibasic acid and a diol, adding an acrylic compound, a catalyst and a polymerization inhibitor, stirring, and prepolymerization under N2 protection; the dibasic acid comprises itaconic acid, 2,5-furandicarboxylic acid and succinic acid; the diol comprises 1,3-propylene glycol, 2-vinyl propane-1,3-diol and isosorbide; S2, polycondensation reaction under vacuum conditions, cooling, purification, and obtaining a polyester prepolymer; S3, adding a diluting cross-linking agent to the polyester prepolymer prepared in step S2, stirring evenly, then adding an initiator, a accelerator, a plasticizer and an antioxidant, degassing after mixing evenly, curing, and obtaining an environmentally friendly unsaturated polyester resin. The environmentally friendly unsaturated polyester resin provided by the present invention has excellent mechanical properties and chemical stability, and fully meets environmental protection requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyester resins, and particularly relates to an environmentally friendly unsaturated polyester resin and a preparation method thereof. Background Art

[0002] As a thermosetting plastic, unsaturated polyester resin is widely used in artificial stone, skylight tiles, chemical and municipal pipelines, coatings, yachts, aerospace and other industries due to its excellent processing performance, excellent mechanical properties and low price.

[0003] Unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by polycondensation of unsaturated dibasic acids and diols. As global environmental issues become increasingly prominent, people are paying more and more attention to the improvement of environmental awareness. Environmentally friendly unsaturated polyester resin has important significance and value in promoting the development of environmental protection industry, promoting sustainable development, improving human living environment and maintaining ecological balance.

[0004] Existing literature reports, the invention of publication number CN116970130A discloses an environmentally friendly unsaturated polyester resin and its preparation method, replaces phthalic anhydride with polyethylene terephthalate, and through the reasonable compounding of auxiliary materials, can prepare an unsaturated polyester resin with excellent performance, and the preparation raw material price is low, realizes waste recycling, green environmental protection. But the inventor found that the CN116970130A patent uses styrene as a diluent and cross-linking agent, because styrene is volatile and has a large smell, serious environmental pollution, endangers the health of workers, and cannot really achieve the requirements of environmental protection. And the invention patent of authorization announcement number CN105622858B discloses a synthetic method of an environmentally friendly styrene-free unsaturated polyester resin, utilizes non-volatile, colorless and odorless or colorless and low-odor acrylic esters to replace styrene, adopts hydroxy acrylate and isocyanate block copolymerization modified unsaturated polyester resin to carry out crosslinking copolymerization, thereby completely eliminating styrene, and meeting the requirements of environmental protection. However, the inventors have found that the isocyanate used in patent CN105622858B is a toxic compound, and the unsaturated polyester resin prepared in patent CN105622858B still releases a relatively high content of volatile organic compounds (VOCs), posing a potential risk to the environment and human health, and cannot truly achieve environmental protection requirements. In addition, isocyanate has strong activity and is likely to affect the chemical stability of the unsaturated polyester resin, thereby reducing the durability and reliability of the unsaturated polyester resin. Summary of the invention

[0005] In order to improve the chemical stability of an environmentally friendly unsaturated polyester resin, the present application provides an environmentally friendly unsaturated polyester resin and a preparation method thereof.

[0006] In a first aspect, the present application provides a method for preparing an environmentally friendly unsaturated polyester resin, which is achieved by the following technical solution:

[0007] A method for preparing an environmentally friendly unsaturated polyester resin comprises the following steps:

[0008] S1. Mix a dibasic acid and a diol in a molar ratio of 1:(1-1.35), add an acrylic compound, a catalyst and an inhibitor, stir, introduce N2 protection, react at 150-180°C for 1-3h, remove water during the reaction, and complete prepolymerization; the dibasic acid includes itaconic acid, 2,5-furandicarboxylic acid and succinic acid; the diol includes 1,3-propylene glycol, 2-vinylpropane-1,3-diol and isosorbide; the acrylic compound includes epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methylacrylate and 4-hydroxyethyloxybenzophenone methylacrylate; the mass of the acrylic compound, catalyst and inhibitor is 15%-22%, 0.08%-0.12% and 0.08%-0.12% of the mass of the dibasic acid, respectively;

[0009] S2, reacting at 150-180°C for 3-7h under vacuum of 0.05-0.1MPa to complete polycondensation, cooling, and purification to obtain a polyester prepolymer;

[0010] S3. Add a diluted cross-linking agent to the polyester prepolymer prepared in step S2, stir evenly, then add an initiator, a promoter, a plasticizer and an antioxidant, mix evenly and degas, and cure at 100-140°C for 2-4h to obtain an environmentally friendly unsaturated polyester resin; the mass ratio of the polyester prepolymer, the diluted cross-linking agent and the initiator, the promoter, the plasticizer and the antioxidant is 1: (0.6-0.8): (0.04-0.06): (0.006-0.008): (0.03-0.05): (0.03-0.05).

[0011] The present invention uses itaconic acid, 2,5-furandicarboxylic acid and succinic acid as dibasic acids, and uses 1,3-propylene glycol, 2-vinylpropane-1,3-diol and isosorbide as diols. Each substance has low toxicity, low volatility, and little impact on the environment and human health. The above monomers can adjust the curing speed and performance of the environmentally friendly unsaturated polyester resin, improve the mechanical properties of the environmentally friendly unsaturated polyester resin, and can also improve the chemical stability of the environmentally friendly unsaturated polyester resin. This is because succinic acid is a saturated dibasic acid and 1,3-propylene glycol is a saturated diol. Succinic acid and 1,3-propylene glycol can provide a more stable molecular structure and reduce the unsaturation, thereby slowing down the curing speed, increasing the fluidity and operability of the environmentally friendly unsaturated polyester resin, improving the chemical stability of the environmentally friendly unsaturated polyester resin, and extending its service life; while itaconic acid and 2,5-furandicarboxylic acid are unsaturated dibasic acids, and 2-vinylpropane-1,3-diol is an unsaturated diol. Itaconic acid, 2,5-furandicarboxylic acid, and 2-vinylpropane-1,3-diol introduce double bonds to provide cross-linking sites, accelerate the curing speed, and improve the cross-linking ability of the environmentally friendly unsaturated polyester resin. Isosorbide and 2,5-furandicarboxylic acid contain a ring structure and have strong rigidity. 1,3-propylene glycol and succinic acid regulate the rigidity and flexibility of the molecular chain, so that the environmentally friendly unsaturated polyester resin has good tensile strength and tensile elongation at break, and good heat resistance, oxidation resistance and hydrolysis resistance.

[0012] The invention adopts epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate and 4-hydroxyethyloxybenzophenone methacrylate, which can undergo crosslinking reaction with itaconic acid, 2,5-furandicarboxylic acid and 2-vinylpropane-1,3-diol, thereby improving the mechanical properties of the environmentally friendly unsaturated polyester resin. Meanwhile, epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate and 4-hydroxyethyloxybenzophenone methacrylate have synergistic effect, thereby significantly improving the chemical stability of the environmentally friendly unsaturated polyester resin, especially the oxidation resistance and ultraviolet resistance.

[0013] Preferably, the molar ratio of itaconic acid, 2,5-furandicarboxylic acid and succinic acid is 1:(0.05-0.1):(0.1-0.2).

[0014] Preferably, the molar ratio of 1,3-propylene glycol, 2-vinylpropane-1,3-diol and isosorbide is 1:(0.1-0.15):(0.2-0.4).

[0015] Preferably, the mass ratio of the epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methylacrylate and 4-hydroxyethyloxybenzophenone methylacrylate is 1:(0.4-0.6):(0.4-0.6).

[0016] Preferably, the diluting cross-linking agent is dimethyl itaconate and / or 2-methylhexyl epoxidized soybean oil acrylate.

[0017] More preferably, the diluent cross-linking agent is prepared by mixing dimethyl itaconate and 2-methylhexyl epoxidized soybean oil acrylate in a mass ratio of 1:(1-1.5).

[0018] The diluting crosslinking agent compounded with dimethyl itaconate and 2-methylhexyl epoxidized soybean oil acrylate contains active groups, which participate in polymerization reactions or react with other components, thereby improving the flexibility of the environmentally friendly unsaturated polyester resin, increasing the tensile strength and tensile elongation at break of the environmentally friendly unsaturated polyester resin, and also increasing the chemical stability of the environmentally friendly unsaturated polyester resin, especially the resistance to chemical corrosion.

[0019] Preferably, the antioxidant is caffeic acid.

[0020] Caffeic acid is a polyhydroxy aromatic acid. One hydroxyl group in the caffeic acid molecule is connected to the benzene ring, and the other hydroxyl group is connected to the side chain of the acryloyl group (-CH=CH-COOH). The acryloyl group on the side chain of the caffeic acid molecule has a certain activity, which allows caffeic acid to participate in the cross-linking reaction during the curing process of the polyester prepolymer, thereby improving the antioxidant and mechanical properties of the environmentally friendly unsaturated polyester resin.

[0021] Preferably, the plasticizer is cellulose acetate butyrate.

[0022] Cellulose acetate butyrate contains a high content of acetyl and butyryl, which can adjust the curing speed of environmentally friendly unsaturated polyester resin, making the curing process more stable and controllable, and can improve the tensile strength and tensile elongation at break of environmentally friendly unsaturated polyester resin. It can also improve the chemical stability of environmentally friendly unsaturated polyester resin, especially UV resistance, oxidation resistance, heat resistance, and hydrolysis resistance.

[0023] Preferably, the catalyst is zinc titanate and / or tetrabutyl titanate.

[0024] More preferably, the catalyst is a mixture of zinc titanate and tetrabutyl titanate in a mass ratio of 1:(2-3).

[0025] The compounding of zinc titanate and tetrabutyl titanate can improve the catalytic efficiency and also help to adjust the molecular structure and molecular weight distribution of the environmentally friendly unsaturated polyester resin, thereby improving the mechanical properties and heat resistance of the environmentally friendly unsaturated polyester resin.

[0026] Preferably, the tetrabutyl titanate is tetrabutyl titanate modified with organic acid anhydride.

[0027] Organic anhydride-modified tetrabutyl titanate can improve the catalytic activity of tetrabutyl titanate, improve the compatibility of tetrabutyl titanate with polyester prepolymer, and help to adjust the molecular structure and molecular weight distribution of environmentally friendly unsaturated polyester resin, thereby further improving the mechanical properties and heat resistance of environmentally friendly unsaturated polyester resin.

[0028] In the present application, the polymerization inhibitor includes but is not limited to one or more of anisole, hydroquinone, methyl hydroquinone, p-benzoquinone, p-tert-butylcatechol, tert-butylhydroquinone, benzyl alcohol, methanol, ethanol, and diphenyl sulfide.

[0029] In the present application, the initiator includes but is not limited to one or more of cyclohexanone peroxide, benzoyl peroxide, ethyl perbenzoate, tert-butyl peroxide, stilbene peroxide, diisopropyl peroxide, tripropylamine peroxide, potassium persulfate, ammonium persulfate, diacetophenone, and diisopropyl diacetophenone.

[0030] In the present application, the promoter includes but is not limited to one or more of cobalt naphthenate, zinc oxide, barium oxide, and calcium oxide.

[0031] In a second aspect, the present application provides an environmentally friendly unsaturated polyester resin, which adopts the following technical solution:

[0032] An environmentally friendly unsaturated polyester resin is prepared by adopting the preparation method.

[0033] In summary, this application has the following beneficial effects:

[0034] 1. All the raw materials used in the present invention have low volatility and toxicity, which is beneficial to reducing pollution to the environment and human body, and the VOCs content is low, which meets the requirements of environmental protection.

[0035] 2. The present invention uses itaconic acid, 2,5-furandicarboxylic acid and succinic acid as dibasic acids, and uses 1,3-propylene glycol, 2-vinylpropane-1,3-diol and isosorbide as diols, which can adjust the curing speed and performance of the environmentally friendly unsaturated polyester resin, improve the mechanical properties of the environmentally friendly unsaturated polyester resin, and also improve the chemical stability of the environmentally friendly unsaturated polyester resin.

[0036] 3. The present invention adopts epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate and 4-hydroxyethyloxybenzophenone methacrylate, which can undergo cross-linking reaction with itaconic acid, 2,5-furandicarboxylic acid and 2-vinylpropane-1,3-diol to improve the mechanical properties of the environmentally friendly unsaturated polyester resin. At the same time, epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate and 4-hydroxyethyloxybenzophenone methacrylate have a synergistic effect, which significantly improves the chemical stability of the environmentally friendly unsaturated polyester resin, especially the oxidation resistance and UV resistance.

[0037] 4. The present invention uses caffeic acid as an antioxidant. The acryloyl group on the side chain of the caffeic acid molecule has certain activity, which allows the caffeic acid to participate in the reaction during the curing process of the polyester prepolymer, thereby improving the antioxidant and mechanical properties of the environmentally friendly unsaturated polyester resin.

[0038] 5. The compounding of zinc titanate and tetrabutyl titanate can improve the catalytic efficiency and help to adjust the molecular structure and molecular weight distribution of the environmentally friendly unsaturated polyester resin, thereby improving the mechanical properties and heat resistance of the environmentally friendly unsaturated polyester resin.

[0039] 6. Tetrabutyl titanate modified with organic acid anhydride can improve the compatibility between tetrabutyl titanate and polyester prepolymer, and is more helpful to adjust the molecular structure and molecular weight distribution of environmentally friendly unsaturated polyester resin, thereby further improving the mechanical properties and heat resistance of environmentally friendly unsaturated polyester resin. DETAILED DESCRIPTION

[0040] The present application is further described in detail below with reference to the embodiments.

[0041] The raw materials used in this application can all be obtained commercially, and the raw materials not mentioned in the embodiments and comparative examples are purchased from Sinopharm Chemical Reagent Co., Ltd.

[0042] Example:

[0043] Embodiments 1-14 provide an environmentally friendly unsaturated polyester resin, which is described below using Embodiment 1 as an example.

[0044] The environmentally friendly unsaturated polyester resin provided in Example 1 is prepared by the following steps:

[0045] S1. Mix 122.13 g (1 mol) itaconic acid (CAS No. 97-65-4), 7.20 g (0.05 mol) 2,5-furandicarboxylic acid (CAS No. 3238-40-2) and 12.01 g (0.1 mol) succinic acid to obtain a dibasic acid. 1,3-propylene glycol, 10.21g (0.1mol) 2-vinylpropane-1,3-diol (CAS No. 922167-76-8) and 36.44g (0.2mol) isosorbide (CAS No. 652-67-5) were mixed to obtain diol, the dibasic acid and diol were mixed at a molar ratio of 1:1.13, 21.20g acrylic acid compound, 0.11g catalyst and 0.11g polymerization inhibitor were added, a stirrer, a water separator, a thermometer and a condensing device were connected, N2 protection was introduced, the reaction was carried out at 160°C for 2h, and water was removed during the reaction to complete the prepolymerization;

[0046] The acrylic compound is prepared by mixing 2,3-epoxypropyl methacrylate (CAS No. 106-91-2), 2-[3-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate (CAS No. 96478-09-0) and 4-hydroxyethyloxybenzophenone methacrylate (CAS No. 34570-27-9) in a mass ratio of 1:0.4:0.6; the catalyst is tetrabutyl titanate; the inhibitor is hydroquinone;

[0047] S2, connect a water circulation vacuum pump, the system vacuum degree is 0.09MPa, react at 160℃ for 5h to complete polycondensation, cool to 25℃ after the reaction, add deionized water, stir and react at 100℃ for 0.5h, let stand and separate, pour out the upper layer liquid; connect a water circulation vacuum pump, the system vacuum degree is 0.09MPa, remove water from the lower layer liquid at 120℃ for 3h, cool to 25℃ after the reaction to complete purification, and obtain a polyester prepolymer;

[0048] S3, take 100g of the polyester prepolymer prepared in step S2, add 60g of the diluted cross-linking agent to the polyester prepolymer, stir evenly, then add 4g of initiator, 0.6g of accelerator, 3g of plasticizer and 3g of antioxidant, mix evenly and degas, and cure at 120°C for 3h to obtain an environmentally friendly unsaturated polyester resin;

[0049] Among them, the diluting cross-linking agent is dimethyl itaconate (CAS No. 617-52-7); the initiator is cyclohexanone peroxide; the accelerator is cobalt cyclohexaneate; the plasticizer is methyl stearate; and the antioxidant is diphenylamine.

[0050] The environmentally friendly unsaturated polyester resin provided in Examples 2-4 is different from that in Example 1 only in that the amounts of the components used in step S1 are different, as shown in Table 1.

[0051] Table 1 Amount of each component in Examples 1-4

[0052]

[0053] The environmentally friendly unsaturated polyester resin provided in Example 5 is different from that in Example 4 only in that the acrylic compound is a mixture of 2,3-epoxypropyl methacrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate and 4-hydroxyethyloxybenzophenone methacrylate in a mass ratio of 1:0.6:0.4.

[0054] The environmentally friendly unsaturated polyester resin provided in Example 6 is different from that in Example 4 only in that the diluent cross-linking agent is a mixture of dimethyl itaconate and epoxidized soybean oil acrylate-2-methylhexyl ester (CAS No. 8013-07-8) in a mass ratio of 1:1.

[0055] The environmentally friendly unsaturated polyester resin provided in Example 7 is different from that in Example 4 only in that the diluent cross-linking agent is 2-methylhexyl epoxidized soybean oil acrylate.

[0056] The environmentally friendly unsaturated polyester resin provided in Example 8 is different from that in Example 6 only in that the antioxidant is caffeic acid (CAS No. 331-39-5).

[0057] The environmentally friendly unsaturated polyester resin provided in Example 9 is different from that in Example 8 only in that the mass of the antioxidant is 5 g.

[0058] The environmentally friendly unsaturated polyester resin provided in Example 10 is different from that in Example 9 only in that the plasticizer is cellulose acetate butyrate (CAS No. 9004-36-8).

[0059] The environmentally friendly unsaturated polyester resin provided in Example 11 is different from that in Example 10 only in that the mass of the plasticizer is 5 g.

[0060] The environmentally friendly unsaturated polyester resin provided in Example 12 is different from that in Example 11 only in that the catalyst is obtained by mixing zinc titanate and tetrabutyl titanate in a mass ratio of 1:2.

[0061] The environmentally friendly unsaturated polyester resin provided in Example 13 is different from that in Example 11 only in that the catalyst is zinc titanate.

[0062] The environmentally friendly unsaturated polyester resin provided in Example 14 is different from that in Example 12 only in that: the catalyst is obtained by mixing zinc titanate and tetrabutyl titanate modified with an organic acid anhydride in a mass ratio of 1:2;

[0063] The preparation steps of organic anhydride-modified tetrabutyl titanate are as follows:

[0064] Mix 10g of tetrabutyl titanate, 2g of maleic anhydride and 0.1g of p-toluenesulfonic acid, heat to 150°C, and react at 150°C for 12h. After the reaction, add 10mL of water to extract three times, remove the supernatant, add anhydrous magnesium sulfate to the lower liquid and dry for 12h to obtain tetrabutyl titanate modified with organic acid anhydride.

[0065] Comparative Example:

[0066] The environmentally friendly unsaturated polyester resins provided in Comparative Examples 1-4 are different from those in Example 2 only in that the amounts of the components used in step S1 are different, as shown in Table 2 for details.

[0067] Table 2 The dosage of each component in Comparative Examples 1-4

[0068]

[0069] The environmentally friendly unsaturated polyester resin provided in Comparative Example 5 is different from that in Example 2 only in that the acrylic compound is a mixture of 2,3-epoxypropyl methacrylate and 4-hydroxyethyloxybenzophenone methacrylate in a mass ratio of 1:1.

[0070] The environmentally friendly unsaturated polyester resin provided in Comparative Example 6 is different from that in Example 2 only in that the acrylic compound is a mixture of 2,3-epoxypropyl methacrylate and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate in a mass ratio of 1:1.

[0071] The environmentally friendly unsaturated polyester resin provided in Comparative Example 7 is different from that in Example 2 only in that the acrylic compound is prepared by mixing 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate and 4-hydroxyethyloxybenzophenone methacrylate in a mass ratio of 1:1.

[0072] Performance testing:

[0073] The following performance tests were performed on the environmentally friendly unsaturated polyester resins provided in Examples 1-14 and Comparative Examples 1-7 of the present application.

[0074] 1. VOCs content: According to the standard of ASTM D2369, the VOCs content of the environmentally friendly unsaturated polyester resins provided in Examples 1-14 and Comparative Examples 1-7 was tested. Each group of samples was tested five times and the average value was taken. The test results are shown in Table 3.

[0075] 2. Tensile strength and elongation at break: According to ASTM D638, the environmentally friendly unsaturated polyester resins provided in Examples 1-14 and Comparative Examples 1-7 were respectively made into specimens with a size of 20 mm×4 mm×3 mm. At 25°C, the tensile rate was 0.5 mm / min, and the tensile strength and elongation at break of the specimens were tested. Each group of specimens was tested five times and the average value was taken. The test results are shown in Table 3.

[0076] 3. Chemical stability: According to ASTM D638 standard, the environmentally friendly unsaturated polyester resins provided in Examples 1-14 and Comparative Examples 1-7 were respectively made into specimens with a size of 20 mm×4 mm×3 mm, and each group of specimens was treated in the following various environments. After treatment, the tensile strength after treatment was tested at 25°C with a tensile rate of 0.5 mm / min. Each group of samples was tested five times and the average value was taken. The test results are shown in Table 3.

[0077] Environment 1: 5 cm away from the UV lamp and the irradiation intensity is 150 μW / cm 2 Place in ultraviolet environment for 7 days;

[0078] Environment 2: Place in an environment with a temperature of 85°C and a relative humidity of 85% for 30 days;

[0079] Environment 3: Soak in 500 mL of 10 wt% ammonia solution for 1 day.

[0080] Table 3 Performance test data

[0081]

[0082] The following describes the present application in detail with respect to the test data in Table 3.

[0083] The environmentally friendly unsaturated polyester resin provided in this application has a low VOCs content, with a maximum value not exceeding 44 μg / m 3 , and low toxicity, in line with environmental protection requirements, and protect the health of workers.

[0084] From the comparison of the experimental data of Example 2 and Comparative Examples 1-2, it can be seen that the dibasic acid containing itaconic acid, 2,5-furandicarboxylic acid and succinic acid improves the tensile strength of the environmentally friendly unsaturated polyester resin, the tensile strength after wet heat treatment and the tensile strength after chemical treatment.

[0085] From the comparison of the experimental data of Example 2 and Comparative Examples 3-4, it can be seen that the diol containing 1,3-propylene glycol, 2-vinylpropane-1,3-diol and isosorbide improves the tensile strength of the environmentally friendly unsaturated polyester resin, the tensile strength after wet heat treatment and the tensile strength after chemical treatment.

[0086] From the comparison of the experimental data of Example 2 and Comparative Examples 5-7, it can be seen that the acrylic compound containing epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methacrylate and 4-hydroxyethyloxybenzophenone methacrylate undergoes a cross-linking reaction with itaconic acid, 2,5-furandicarboxylic acid and 2-vinylpropane-1,3-diol, thereby improving the mechanical properties of the environmentally friendly unsaturated polyester resin, and also improving the tensile strength of the environmentally friendly unsaturated polyester resin after UV treatment, the tensile strength after wet heat treatment and the tensile strength after chemical treatment.

[0087] From the comparison of the experimental data of Example 6 with Examples 4 and 7, it can be seen that Example 6 uses a diluent cross-linking agent compounded with dimethyl itaconate and 2-methylhexyl epoxidized soybean oil acrylate, which improves the tensile strength and tensile elongation at break of the environmentally friendly unsaturated polyester resin, and also significantly improves the tensile strength of the environmentally friendly unsaturated polyester resin after chemical treatment.

[0088] From the comparison of the experimental data of Example 8 and Example 6, it can be seen that Example 8 uses caffeic acid as an antioxidant, and Example 6 uses diphenylamine as an antioxidant, and the antioxidant property is better. The acryloyl group on the side chain of the caffeic acid molecule has certain activity and can participate in the reaction, thereby improving the mechanical properties of the environmentally friendly unsaturated polyester resin.

[0089] From the comparison of the experimental data of Example 10 and Example 9, it can be seen that Example 10 uses cellulose acetate butyrate as a plasticizer, and Example 9 uses methyl stearate as a plasticizer. Cellulose acetate butyrate contains a relatively high content of acetyl and butyryl groups, which improves the tensile strength and tensile elongation at break of the environmentally friendly unsaturated polyester resin, and also improves the tensile strength of the environmentally friendly unsaturated polyester resin after UV treatment and the tensile strength after wet heat treatment.

[0090] From the comparison of the experimental data of Example 12 with Examples 11 and 13, it can be seen that Example 12 uses a catalyst compounded with zinc titanate and tetrabutyl titanate, which helps to adjust the molecular structure and molecular weight distribution of the environmentally friendly unsaturated polyester resin, and improves the tensile strength and tensile elongation at break of the environmentally friendly unsaturated polyester resin and the tensile strength after wet heat treatment.

[0091] From the comparison of the experimental data of Example 14 and Example 12, it can be seen that Example 14 uses tetrabutyl titanate modified with organic acid anhydride to improve the compatibility of tetrabutyl titanate with polyester prepolymer, and further improves the tensile strength and tensile elongation at break of the environmentally friendly unsaturated polyester resin and the tensile strength after wet heat treatment.

[0092] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing an environmentally friendly unsaturated polyester resin, characterized in that: The steps include: S1. Mix a dibasic acid and a diol in a molar ratio of 1:1-1.35, add an acrylic compound, a catalyst and an inhibitor, stir, introduce N2 protection, react at 150-180°C for 1-3h, remove water during the reaction, and complete prepolymerization; the dibasic acid includes itaconic acid, 2,5-furandicarboxylic acid and succinic acid; the diol includes 1,3-propylene glycol, 2-vinylpropane-1,3-diol and isosorbide; the acrylic compound includes epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methylacrylate and 4-hydroxyethyloxybenzophenone methylacrylate; the acrylic compound, catalyst and The mass of the inhibitor is 15%-22%, 0.08%-0.12% and 0.08%-0.12% of the mass of the dibasic acid respectively; the molar ratio of itaconic acid, 2,5-furandicarboxylic acid and succinic acid is 1:0.05-0.1:0.1-0.2; the molar ratio of 1,3-propylene glycol, 2-vinylpropane-1,3-diol and isosorbide is 1:0.1-0.15:0.2-0.4; the mass ratio of epoxy acrylate, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl-2-methylacrylate and 4-hydroxyethyloxybenzophenone methylacrylate is 1:0.4-0.6:0.4-0.6; S2, reacting at 150-180°C for 3-7h under vacuum of 0.05-0.1MPa to complete polycondensation, cooling, and purification to obtain a polyester prepolymer; S3. Add a diluted cross-linking agent to the polyester prepolymer prepared in step S2, stir evenly, then add an initiator, a accelerator, a plasticizer and an antioxidant, mix evenly and degas, and cure at 100-140° C. for 2-4 hours to obtain an environmentally friendly unsaturated polyester resin; the mass ratio of the polyester prepolymer, the diluted cross-linking agent and the initiator, the accelerator, the plasticizer and the antioxidant is 1:0.6-0.8:0.04-0.06:0.006-0.008:0.03-0.05:0.03-0.

05.

2. The method for preparing an environmentally friendly unsaturated polyester resin according to claim 1, characterized in that: The diluting cross-linking agent is dimethyl itaconate and / or epoxidized soybean oil acrylate-2-methylhexyl ester.

3. The method for preparing an environmentally friendly unsaturated polyester resin according to claim 1, characterized in that: The antioxidant is caffeic acid.

4. The method for preparing an environmentally friendly unsaturated polyester resin according to claim 1, characterized in that: The plasticizer is cellulose acetate butyrate.

5. The method for preparing an environmentally friendly unsaturated polyester resin according to claim 1, characterized in that: The catalyst is zinc titanate and / or tetrabutyl titanate.

6. The method for preparing an environmentally friendly unsaturated polyester resin according to claim 5, characterized in that: The tetrabutyl titanate is tetrabutyl titanate modified by organic acid anhydride.

7. An environmentally friendly unsaturated polyester resin, characterized in that: The environmentally friendly unsaturated polyester resin is prepared by the preparation method of any one of claims 1 to 6.

Citation Information

Patent Citations

  • A method for synthesizing an environmentally friendly styrene-free unsaturated polyester resin

    CN105622858B

  • Environment-friendly unsaturated polyester resin and preparation method thereof

    CN116970130A

  • Double-bond-containing all-bio-based polyesters, and preparation method and application thereof

    CN103483571A

  • Bio-based polyester resin for powder coating and preparation method of bio-based polyester resin

    CN107163234A

  • Photosensitive biodegradable polyester as well as preparation method and application thereof

    CN110615888A