A high-strength barrier nylon 6 nanocomposite material and preparation method thereof

By adding graphene oxide and hydroxypropyl-β-cyclodextrin to nylon 6 to form a cross-linked structure, the problem of insufficient barrier properties and mechanical properties of existing gas storage bottles is solved, and a polymer with high strength and excellent barrier properties is achieved. Amide nanocomposites for hydrogen storage containers.

CN118496664BActive Publication Date: 2024-10-11SUZHOU GANGRUITONG NANO MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410954103.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-11
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Existing plastic gas storage bottles have low barrier properties, poor mechanical strength and low-temperature impact resistance, resulting in low storage density and low safety. Polyols and cyclodextrin are easy to precipitate, affecting their service life.

Method used

Using the preparation method of high-strength barrier nylon 6 nanocomposites, by adding graphene oxide and hydroxypropyl-β-cyclodextrin to nylon 6, using its surface active groups to react with nylon prepolymer to form a cross-linked structure, improving the Density and mechanical properties.

Benefits of technology

The polyamide nanocomposite material that achieves high strength and excellent barrier properties is suitable for hydrogen storage containers, improving the overall performance and processability of the product and extending its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 4LXTD8W5D6UZYKXCQBLIVGHYJS3N3J2S0B08GDQS
    Figure 4LXTD8W5D6UZYKXCQBLIVGHYJS3N3J2S0B08GDQS
  • Figure AWCF63UZDFSBEZCAI9UTJZJWYNRKYZIREYJP52GH
    Figure AWCF63UZDFSBEZCAI9UTJZJWYNRKYZIREYJP52GH
Patent Text Reader

Abstract

The invention discloses a high-strength barrier nylon 6 nanocomposite material and a preparation method thereof, and belongs to the technical field of polymer materials. The invention uses graphene oxide and hydroxypropyl-β-cyclodextrin as composite modification additives, caprolactam as a monomer, and prepares a high-strength barrier nylon 6 nanocomposite material by an in-situ hydrolysis polymerization process. Graphene oxide with more surface active groups and hydroxypropyl-β-cyclodextrin with high water solubility and polar solvent solubility are both conducive to the full dispersion of raw materials in the in-situ polymerization process to prevent material agglomeration; and graphene oxide and hydroxypropyl-β-cyclodextrin can form a cross-linked network structure with each other and with nylon prepolymers, and the interface effect is stronger, which can improve the compactness and mechanical strength of the composite material. Due to its compactness and low permeability, the polyamide nanocomposite material can be used in storage containers for gases such as hydrogen.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials technology, specifically relating to a high-strength barrier nylon 6 nanocomposite material and its preparation method. Background Technology

[0002] Composite material gas cylinders originated in the 1950s, initially based on rocket engine composite material technology. They were made by impregnating glass fiber with epoxy resin and then winding it around a metal shell. While these cylinders are lighter than all-steel cylinders, glass fiber has poor resistance to stress fracture and fatigue, resulting in a lower safety factor. Especially with the increasing sophistication of equipment, traditional metal gas cylinders are becoming increasingly unsuitable due to their weight. Furthermore, the global demand for new energy sources has led to rapid development in the hydrogen fuel cell vehicle and hydrogen storage cylinder industries in recent years. Currently, all gas cylinders are made of carbon fiber fully wound with an aluminum alloy liner; there are no reports of composite cylinders with plastic liner manufacturing.

[0003] A comparison of metal-lined and plastic-lined composite hydrogen storage cylinders with the same outer diameter, volume, and pressure reveals that plastic-lined composite cylinders offer advantages such as low cost, high density, and lightweight, making them more aligned with the development trend of vehicle-mounted hydrogen storage cylinders. Gaseous hydrogen storage, which involves compressing hydrogen and storing it in a high-pressure container, is currently the most mature method for hydrogen energy storage and transportation. The advantages of gaseous hydrogen storage include simple storage conditions, lower required storage temperature and pressure, lower equipment costs suitable for large-scale storage, wide applicability in automobiles, trains, ships, and other transportation vehicles, as well as industrial applications, and convenient transportation via pipelines or long-tube trailers.

[0004] However, existing plastic gas cylinders have low barrier properties, allowing hydrogen to easily escape into the environment within high-pressure containers; poor molding quality results in poor mechanical strength and low-temperature impact resistance, leading to low storage density, limiting large-scale storage, and low safety with a high explosion hazard. CN116987380A provides a polyol and cyclodextrin modified nylon gas barrier material, but it uses a direct blending method to prepare the composite material, resulting in uneven additive dispersion, limited improvement in mechanical properties, and a technical problem of easy precipitation of polyols and cyclodextrins during long-term use, affecting the service life of the gas cylinder. Summary of the Invention

[0005] To address the aforementioned problems, the present invention aims to provide a high-strength barrier nylon 6 nanocomposite material and its preparation method. This high-strength barrier nylon 6 nanocomposite material has a simple preparation process, low production cost, and excellent barrier and mechanical properties, which can meet the requirements of high barrier and high mechanical properties and has good application prospects.

[0006] The objective of this invention is achieved through the following technical solution.

[0007] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0008] (1) Add 4-6 parts of graphene oxide, 1-2 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse size of graphene oxide is 300-500 nm.

[0009] (2) Under the protection of inert gas, the mixed dispersion is transferred to a high-temperature and high-pressure reactor, heated to 250-300℃, and reacted at 0.5-1MPa for 2-4h; then the reaction is continued under vacuum for 0.5-2h to obtain nylon 6 melt;

[0010] (3) After cooling, washing and drying the nylon 6 melt, a high-strength barrier nylon 6 nanocomposite material is obtained.

[0011] This invention uses nylon 6 as the resin matrix, which has better molecular chain regularity and stronger intermolecular interactions compared to nylon 66 and other polymers, thus promoting crystallization and improving mechanical properties and density. However, highly crystalline nylon 6 has lower toughness, making it difficult to meet the requirements for high impact resistance. Adding graphene oxide and hydroxypropyl-β-cyclodextrin, which have high barrier properties, during in-situ polymerization can improve the toughness and density of the nylon composite material. Graphene oxide has numerous surface-active groups such as carboxyl and hydroxyl groups, which can react with carboxyl or amino functional groups on the nylon prepolymer, improving its compatibility with the nylon resin. Compared to β-cyclodextrin and γ-cyclodextrin, hydroxypropyl-β-cyclodextrin has a higher thermal decomposition temperature (hydroxypropyl-β-cyclodextrin decomposes at 360℃, while β-cyclodextrin and γ-cyclodextrin decompose at around 250℃, making it difficult to reach the polymerization temperature of nylon 6), thus preventing degradation during polymerization. Furthermore, hydroxypropyl-β-cyclodextrin exhibits higher water solubility and polar solvent solubility compared to other cyclodextrins, which is beneficial for thorough dispersion during in-situ polymerization. The presence of hydroxypropyl branches facilitates the formation of a cross-linked structure with the nylon backbone, improving density. Both graphene oxide and hydroxypropyl-β-cyclodextrin possess numerous surface-active groups. Cyclodextrin not only prevents the re-agglomeration of graphene oxide sheets, improving its dispersion performance, but also forms a cross-linked network structure between themselves and with nylon prepolymers, enhancing the density and mechanical properties of the composite material and meeting the requirements for gas storage materials.

[0012] Based on the above scheme, in step (1), the water is deionized water, and the amount used is 3-8 parts.

[0013] Based on the above scheme, further, the heating temperature in step (1) is 80-95℃.

[0014] Based on the above scheme, the ultrasonic stirring time in step (1) is further 0.5-1h.

[0015] Based on the above scheme, in step (2), the inert gas is nitrogen or helium.

[0016] Based on the above scheme, further, in step (2), the temperature is raised to 260-280℃.

[0017] Based on the above scheme, further, in step (3), water cooling process is adopted for cooling.

[0018] Based on the above scheme, further, in step (3), the washing is carried out with warm water at 40-50℃.

[0019] Based on the above scheme, further, in step (3), the drying is carried out in a vacuum drying oven; the drying temperature is 70-90℃; and the drying time is 2-4h.

[0020] The beneficial effects of this invention are as follows:

[0021] This invention provides a polyamide nanocomposite material that combines excellent barrier properties and mechanical strength. Due to its low permeability, this polyamide nanocomposite material can be used for storage containers of gases such as hydrogen. Graphene oxide has numerous surface-active groups, and hydroxypropyl-β-cyclodextrin has higher water solubility and polar solvent solubility, both of which are beneficial for thorough dispersion during in-situ polymerization. These components can form cross-linked structures with each other and with nylon prepolymers, improving the density and mechanical properties of the composite material. Compared with physically blended nylon 6 composites, the overall performance is further improved, and the product has good processability, meeting the requirements for gas storage materials. Detailed Implementation

[0022] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0023] The raw material components involved in the following examples and comparative examples are all typical products purchased from the market.

[0024] Example 1

[0025] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0026] (1) Add 4 parts of graphene oxide, 1 part of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 300 nm; the water is deionized water, and the amount used is 3 parts; the heating temperature is 80℃; the sonication time is 0.5 h.

[0027] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 260°C, and reacted at 1 MPa for 4 hours; then the reaction was continued under vacuum for 2 hours to obtain nylon 6 melt;

[0028] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 40℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 70℃; the drying time was 4h.

[0029] Example 2

[0030] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0031] (1) Add 6 parts of graphene oxide, 2 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 500 nm; the water is deionized water, and the amount used is 8 parts; the heating temperature is 95℃; the sonication time is 1 h.

[0032] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 280°C, and reacted at 0.5 MPa for 2 h; then the reaction was continued under vacuum for 0.5 h; nylon 6 melt was obtained;

[0033] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by 50°C warm water; the drying was carried out by vacuum drying oven; the drying temperature was 90°C; the drying time was 2h.

[0034] Example 3

[0035] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0036] (1) Add 4 parts of graphene oxide, 2 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 500 nm; the water is deionized water, and the amount used is 4 parts; the heating temperature is 85℃; the sonication time is 0.7 h.

[0037] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 265°C, and reacted at 0.6 MPa for 2.5 h; then the reaction was continued under vacuum for 1.2 h; nylon 6 melt was obtained;

[0038] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 42℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 86℃; the drying time was 2.8h.

[0039] Example 4

[0040] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0041] (1) Add 6 parts of graphene oxide, 1 part of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 300 nm; the water is deionized water, and the amount used is 7 parts; the heating temperature is 92℃; the sonication time is 0.9 h.

[0042] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 273°C, and reacted at 0.8 MPa for 3.6 h; then the reaction was continued under vacuum for 1.7 h; nylon 6 melt was obtained;

[0043] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 47℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 86℃; the drying time was 2.2h.

[0044] Example 5

[0045] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0046] (1) Add 4.5 parts of graphene oxide, 1.7 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 350 nm; the water is deionized water, and the amount used is 4 parts; the heating temperature is 85℃; the sonication time is 0.8 h.

[0047] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 265°C, and reacted at 0.9 MPa for 2.8 h; then the reaction was continued under vacuum for 1.3 h; nylon 6 melt was obtained;

[0048] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 47℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 72℃; the drying time was 3.4h.

[0049] Example 6

[0050] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0051] (1) Add 5.8 parts of graphene oxide, 1.4 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 450 nm; the water is deionized water, and the amount used is 6 parts; the heating temperature is 87℃; the sonication time is 0.8 h.

[0052] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 274°C, and reacted at 0.6 MPa for 3.3 h; then the reaction was continued under vacuum for 0.9 h; nylon 6 melt was obtained;

[0053] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 48℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 86℃; the drying time was 3.6h.

[0054] Example 7

[0055] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0056] (1) Add 5 parts of graphene oxide, 1.5 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 400 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the sonication time is 0.8 h.

[0057] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 270°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0058] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0059] Example 8

[0060] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0061] (1) Add 5 parts of graphene oxide, 1.5 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 400 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the sonication time is 0.8 h.

[0062] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 250°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0063] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0064] Example 9

[0065] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0066] (1) Add 5 parts of graphene oxide, 1.5 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 400 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the sonication time is 0.8 h.

[0067] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 300°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0068] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0069] Comparative Example 1

[0070] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0071] (1) Add 5 parts of graphene oxide, 1.5 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 200 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the sonication time is 0.8 h.

[0072] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 270°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0073] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0074] Comparative Example 2

[0075] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0076] (1) Add 5 parts of graphene oxide, 1.5 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 700 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the sonication time is 0.8 h.

[0077] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 270°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0078] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0079] Comparative Example 3

[0080] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0081] (1) Add 8 parts of graphene oxide, 1.5 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 400 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the sonication time is 0.8 h.

[0082] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 270°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0083] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0084] Comparative Example 4

[0085] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0086] (1) Add 5 parts of graphene oxide, 0.4 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 400 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the sonication time is 0.8 h.

[0087] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 270°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0088] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0089] Comparative Example 5

[0090] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0091] (1) Add 5 parts of graphene oxide, 4 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heat and sonicate to stir evenly to obtain a mixed dispersion; the transverse dimension of graphene oxide is 400 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the sonication time is 0.8 h.

[0092] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 270°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0093] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0094] Comparative Example 6

[0095] A method for preparing a high-strength barrier nylon 6 nanocomposite material includes the following steps:

[0096] (1) Add 5 parts graphene, 1.5 parts β-cyclodextrin and water to 100 parts caprolactam, heat and ultrasonically stir until uniform to obtain a mixed dispersion; the transverse dimension of graphene oxide is 400 nm; the water is deionized water, and the amount used is 5 parts; the heating temperature is 86℃; the ultrasonic stirring time is 0.8 h.

[0097] (2) Under nitrogen protection, the mixed dispersion was transferred to a high-temperature and high-pressure reactor, heated to 270°C, and reacted at 0.7 MPa for 3 h; then the reaction was continued under vacuum for 1.6 h; nylon 6 melt was obtained;

[0098] (3) The nylon 6 melt was cooled, washed and dried to obtain a high-strength barrier nylon 6 nanocomposite material; the cooling was carried out by water cooling process; the washing was carried out by washing with 45℃ warm water; the drying was carried out by vacuum drying oven; the drying temperature was 80℃; the drying time was 3h.

[0099] The high-strength barrier nylon 6 nanocomposites prepared in Examples 1-9 and Comparative Examples 1-6 were used to prepare samples for testing tensile strength, flexural strength, notched impact strength, and barrier performance. Barrier grades A, B, C, D, and E represent the hydrogen barrier efficiency of the high-strength barrier nylon 6 nanocomposites, with the barrier effect gradually decreasing from A to E.

[0100]

[0101]

[0102] As can be seen from Examples 1-9 and Comparative Examples 1-6 in Table 1, this invention provides a polyamide nanocomposite material with both excellent barrier properties and mechanical properties. During in-situ polymerization, the raw materials are fully dispersed, and cross-linked structures can be formed between themselves and with the nylon prepolymer, improving the density and mechanical properties of the composite material. Compared with physically blended nylon 6 composite materials, the overall performance is further enhanced. As can be seen from Examples 7-9, when the reaction temperature is too low, the activity of hydroxypropyl-β-cyclodextrin is low, chain segment movement is difficult, and the cross-linking reaction is incomplete; when the reaction temperature is too high, it approaches the decomposition temperature of hydroxypropyl-β-cyclodextrin and leads to a violent reaction of caprolactam, which is detrimental to performance improvement.

[0103] As can be seen from Examples 7-9 and Comparative Examples 1-6, the combined addition of graphene oxide and hydroxypropyl-β-cyclodextrin can achieve a synergistic cross-linking effect; when the amount added is too small, it is difficult to achieve the reinforcing and blocking effects. Excessive addition of graphene oxide easily leads to uneven dispersion, affecting performance improvement; excessive addition of hydroxypropyl-β-cyclodextrin leads to over-cross-linking, increased brittleness, hindered molecular chain movement, poor crystallization ability, and low barrier performance. Meanwhile, compared to graphene, graphene oxide has more surface active groups, which is conducive to the formation of cross-linked and dense structures, improving the barrier and mechanical properties of nylon 6. When the average size of graphene oxide is too small, it cannot play a blocking role and is prone to agglomeration; when the size is too large, under the same graphene oxide mass conditions, its effective dispersion concentration decreases, failing to form a barrier network, affecting the barrier effect and mechanical property improvement.

Claims

1. A method for preparing a high-strength barrier nylon 6 nanocomposite material, characterized in that: The following steps are involved: (1) adding 4-6 parts of graphene oxide, 1-2 parts of hydroxypropyl-β-cyclodextrin and water to 100 parts of caprolactam, heating and ultrasonically stirring to obtain a mixed dispersion; the lateral size of the graphene oxide is 300-500 nm; (2) Under the protection of inert gas, transfer the mixed dispersion into a high temperature and high pressure reactor, raise the temperature to 260-280°C, and react at 0.5-1MPa for 2-4h; then evacuate and continue the reaction for 0.5-2h; Obtaining nylon 6 melt; (3) The nylon 6 melt is cooled, washed, and dried to obtain a high-strength barrier nylon 6 nanocomposite material.

2. The method for preparing a high-strength barrier nylon 6 nanocomposite material according to claim 1, characterized in that: The water in step (1) is deionized water, and the amount used is 3-8 parts.

3. The method for preparing a high-strength barrier nylon 6 nanocomposite material according to claim 1, characterized in that: The heating temperature in step (1) is 80-95°C.

4. The method for preparing a high-strength barrier nylon 6 nanocomposite material according to claim 1, characterized in that: The ultrasonic stirring time in step (1) is 0.5-1h.

5. The method for preparing a high-strength barrier nylon 6 nanocomposite material according to claim 1, characterized in that: In step (2), the inert gas is nitrogen or helium.

6. The method for preparing a high-strength barrier nylon 6 nanocomposite material according to claim 1, characterized in that: In step (3), cooling is performed using a water cooling process.

7. The method for preparing a high-strength barrier nylon 6 nanocomposite material according to claim 1, characterized in that: The washing in step (3) is carried out using warm water at 40-50°C.

8. The method for preparing a high-strength barrier nylon 6 nanocomposite material according to claim 1, characterized in that: The drying in step (3) is carried out in a vacuum drying oven; the drying temperature is 70-90° C.; and the drying time is 2-4 hours.

9. A high-strength barrier nylon 6 nanocomposite material, characterized in that: The high-strength barrier nylon 6 nanocomposite material is prepared by the preparation method of any one of claims 1 to 8.