A high refractive index coating material, preparation method and application thereof

Through the new high-refractive index coating technology of CaTixOy material, the problems of insufficient optical performance of resin substrates and low refractive index of LaTiOx are solved, and the refractive index is improved and the coating performance is stable, reducing equipment requirements and thermal radiation temperature.

CN118497674BActive Publication Date: 2024-11-05GRINM RESOURCES & ENVIRONMENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977451.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-05
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The optical performance of resin substrates on electronic device lenses is insufficient. The existing high-refractive index optical film material LaTiOx has a low refractive index and requires high electron beam power when coating, which can easily lead to deformation of the resin substrate and high equipment requirements.

Method used

A new high-refractive index coating material composed of CaTixOy (0.8

Benefits of technology

The refractive index is improved, the thermal radiation temperature and equipment requirements during coating are reduced, the stability and coating performance of the resin substrate are ensured, and the demand for the number of film layers is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497674B_ABST
    Figure CN118497674B_ABST
Patent Text Reader

Abstract

This application provides a novel coating material with a high refractive index, a preparation method thereof, and an application thereof. The coating material is composed of CaTi x O y (0.8 < x < 2, 2 < y < 4). The preparation method includes: mixing titanium dioxide powder, titanium powder, and calcium oxide in a certain proportion, and then pressing them into a green body; under vacuum conditions, performing high-temperature sintering treatment on the green body to obtain a sintered body; heating the sintered body to melting, and after cooling, crushing, and screening the obtained melt, CaTi x O y , CaTi x O y are formed into the coating material. The novel coating material with a high refractive index provided by this application has stable performance, and its phase structure hardly changes before and after coating. Moreover, CaTi x O y has a specific crystal structure. The refractive index of the coating material composed of CaTi x O y after coating is higher than that of LaTiO x , but the electron beam energy required during coating is similar to that of LaTiO x . It realizes the improvement of the refractive index of the coated film layer without changing the structure of the coating substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new materials, and more specifically, to a novel high refractive index optical coating material, a preparation method thereof, and an application thereof. Background Art

[0002] With the progress of technology, resin substrates are increasingly used on the lenses of some electronic devices. However, the optical properties of resin substrates are average and cannot well meet the shooting requirements. To improve the optical properties of resin substrates, it is necessary to deposit multi-layer optical thin films with alternating low refractive index and high refractive index.

[0003] Among them, the high refractive index optical thin films are mainly LaTiO x (H4) and Ti3O5, and the most widely used is LaTiO x (H4). However, the refractive index of LaTiO x is only 1.9 without an ion source, showing a relatively low refractive index. Summary of the Invention

[0004] To solve the above problems, the present application provides a novel high refractive index coating material, a preparation method thereof, and an application thereof. The electron beam power required for this coating material during coating is similar to that of LaTiO x , but the refractive index is higher than that of LaTiO x , and the coating performance is stable, providing a more applicable material for coating resin substrates.

[0005] In the first aspect, the present application provides a novel high refractive index coating material, which is composed of CaTi x O y (0.8 < x < 2, 2 < y < 4).

[0006] Further, the value range of the number of titanium atoms x in CaTi x O y includes: 0.85 < x < 1.5, and the value range of the number of oxygen atoms y includes: 2.5 < y < 3.5.

[0007] In the second aspect, the present application provides a preparation method of the coating material in the first aspect. The preparation method of the coating material includes:

[0008] Mix a certain proportion of titanium dioxide powder, titanium powder, and calcium oxide evenly and then press them into a green body;

[0009] Under vacuum conditions, perform high-temperature sintering treatment on the green body to obtain a sintered body;

[0010] Heat the sintered body to melting, and after cooling, crushing, and screening the obtained melt, CaTi x Oy , the CaTi x O y Composing the coating material;

[0011] Wherein, by weight, in the green body, the mass fraction of the titanium dioxide powder is 40-60%, the mass fraction of the titanium powder is 5-10%, and the mass fraction of the calcium oxide is 30-45%.

[0012] Furthermore, by weight, in the green body, the mass fraction of the titanium dioxide powder is 48-53%, the mass fraction of the titanium powder is 6-8%, and the mass fraction of the calcium oxide is 35-40%.

[0013] Furthermore, the high temperature sintering treatment includes: heating to 1000-1500° C. at a rate of 2-25° C. / min, and then keeping the temperature for 1-10 h to obtain the sintered body.

[0014] Furthermore, the high temperature sintering treatment includes: heating to 1200-1400° C. at a rate of 4-8° C. / min, and then keeping the temperature for 3-5 hours to obtain the sintered body.

[0015] Furthermore, heating the sintered body to melt includes: heating to 1700-1900° C. at a rate of 1.5-15° C. / min, and then keeping the temperature for 1-10 hours to obtain the melt.

[0016] Furthermore, heating the sintered body until it melts comprises: heating the temperature to 1750-1850° C. at a rate of 2-11° C. / min, and then keeping the temperature for 3-5 hours to obtain the melt.

[0017] In a third aspect, the present application provides an application of the coating material provided in the first aspect or the second aspect above:

[0018] The CaTi x O y Depositing on the cleaned camera resin substrate to form a film layer;

[0019] Among them, the voltage during deposition is 6~8KV, the current is 65~75mA, and the electron beam power is 450~520W.

[0020] Furthermore, the refractive index of the film layer is 1.96-2.10.

[0021] Beneficial effects:

[0022] The present application provides a novel high refractive index coating material composed of CaTi x O ycomposed of (0.8 < x < 2, 2 < y < 4), the compound has stable performance, and its phase structure hardly changes before and after coating; CaTi x O y has a specific crystal structure, and the refractive index of the coating material composed of CaTi x O y after coating is higher than that of LaTiO x , but the electron beam energy required during coating is similar to that of LaTiO x . Without changing the structure of the coating substrate, the refractive index of the deposited film layer is further increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for the description of the embodiments of the present application will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative efforts.

[0024] Figure 1 is the process flow chart of the preparation method of the novel high refractive index coating material proposed in the embodiments of the present application;

[0025] Figure 2 is the comparison diagram of the phase structure of CaTi x O y before and after coating in Embodiment 1 of the present application;

[0026] Figure 3 is the comparison diagram of the thin film transmittance curves of CaTi x O y and LaTiO x under the same conditions in the embodiments of the present application. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0027] The technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the drawings in the embodiments of the present application. Obviously, the described embodiments are some, but not all, of the embodiments of the present application. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present application without creative efforts belong to the scope of protection of the present application.

[0028] In the drawings, sometimes for clarity, the sizes of the components, the thicknesses of the layers, or the regions may be exaggerated. Therefore, any implementation of the present disclosure is not necessarily limited to the sizes shown in the drawings, and the shapes and sizes of the components in the drawings do not reflect the true proportions. In addition, the drawings schematically show ideal examples, and any implementation of the present disclosure is not limited to the shapes or values shown in the drawings.

[0029] In the related technology, in order to meet the requirements of cost saving and lightweight, some electronic equipment cameras and other lenses are increasingly using resin substrates. The resin substrate is mainly made of resin materials, such as CR-39 resin, polycarbonate resin, etc. It is light in weight and lighter than the glass substrate; it has good impact resistance and can better resist external impact and is not easy to break.

[0030] However, when the resin substrate is used in the lens, as an optical element, its optical performance is poor and cannot meet the photography requirements of cameras, mobile phones, etc. In order to improve the optical performance of the substrate, it is generally necessary to coat multiple layers of optical films with alternating high and low refractive indices.

[0031] Optical film is a type of optical medium material composed of thin layered media that propagates light beams through interfaces. It is also a widely used optical element.

[0032] Among them, low refractive index materials are currently generally SiO2, SiAlO x and MgF2, the high refractive material is mainly LaTiO x (H4) and Ti3O5.

[0033] Although the above two materials are commonly used high refractive index optical films, there are still some problems after coating the above two materials. x The refractive index is relatively low, only 1.9 without an ion source. Although Ti3O5 has a higher refractive index, the ion source and electron beam evaporation energy required for coating are relatively high, and the thermal radiation temperature generated is relatively high, which can easily cause deformation of the resin substrate and places high requirements on the coating equipment.

[0034] Based on the above problems, the present application provides a new type of high refractive index coating material, a preparation method and its application. The coating material is composed of CaTi x O y Composition, CaTi x O y The electron beam power required for coating materials composed of LaTiO x Similarly, the ion source and electron beam evaporation energy is relatively low, which makes the generated heat radiation temperature low, avoids deformation of the coating matrix resin substrate, and reduces the requirements for coating equipment. Although the electron beam power required for coating is similar to that of LaTiO x Similar, but CaTi x O y The refractive index of the coating material is compared with LaTiO x The refractive index after coating is better, which helps to use fewer coating layers while meeting the refractive index requirements during application.

[0035] In a first aspect, the present application provides a novel high-refractive-index coating material, which is composed of CaTi x O y (0.8 < x < 2, 2 < y < 4).

[0036] It should be noted that CaTi x O y contains two metal elements, calcium and titanium. The perovskite compound has a relatively high dielectric constant, and the refractive index is equal to the square root of the dielectric constant, which can change the speed of light when propagating in the material, thereby increasing the refractive index of the composition coating material.

[0037] In CaTi x O y , "x" represents the number of oxygen atoms that are unknown or uncertain; the number of oxygen atoms is determined by the masses of the calcium raw material and the titanium raw material used during preparation; "y" represents the number of titanium atoms that are unknown or uncertain, and the number of titanium atoms is determined by the masses of the calcium raw material and the titanium raw material used during preparation.

[0038] Specifically, during implementation, the value range of the number of titanium atoms x in CaTi x O y includes: 0.85 < x < 1.5, and the value range of the number of oxygen atoms y includes: 2.5 < y < 3.5.

[0039] For the coating material composed of CaTi x O y with the number of oxygen atoms within the above range, the phase of the coated material is more stable, and thus the refractive index is more consistent.

[0040] In a second aspect, the present application provides a preparation method for the novel high-refractive-index coating material of the first aspect. Referring to Figure 1 , the preparation method includes:

[0041] Step S1: Mix a certain proportion of titanium dioxide powder, titanium powder, and calcium oxide evenly and then press them into a green body;

[0042] Step S2: Under vacuum conditions, perform high-temperature sintering treatment on the green body to obtain a sintered body;

[0043] Step S3: Heat the sintered body to melting, and after cooling, crushing, and screening the obtained melt, obtain CaTi x O y , and CaTi x O y forms the coating material;

[0044] Among them, by weight, in the green body, the mass fraction of titanium dioxide powder is 40 - 60%, the mass fraction of titanium powder is 5 - 10%, and the mass fraction of calcium oxide is 30 - 45%.

[0045] It should be noted that titanium dioxide is a white solid or powdered amphoteric oxide with stable chemical properties and excellent optical properties, mainly manifested in high refractive index and high reflectivity;

[0046] Titanium powder is a high-strength but low-quality metal with fairly good ductility, stable chemical properties and high corrosion resistance;

[0047] Calcium oxide means a compound which is calcium oxide or is capable of producing calcium oxide at elevated temperatures;

[0048] The calcium oxide may be calcium oxide or calcium carbonate;

[0049] During preparation, the added titanium dioxide, titanium powder and calcium oxide are all in powdery structure.

[0050] CaTi is prepared by combining titanium dioxide, titanium powder and calcium oxide. x O y , CaTi x O y The coating material composed of the above-mentioned materials not only has a high refractive index after coating, but also requires relatively less electron beam energy during coating, thereby reducing the impact on the resin substrate during coating. At the same time, the film layer has a higher refractive index, which helps to reduce the number of film layers required when designing the film system of the base resin substrate.

[0051] It should be noted that CaTiO3 prepared only from titanium dioxide and calcium oxide will lose oxygen to a certain extent during the coating process, resulting in changes in the material phase after coating. However, by adding a small amount of titanium powder, the oxygen content can be controlled in advance, thereby ensuring the stability of the phase before and after coating, and further ensuring the stability of the refractive index of the film layer;

[0052] The second aspect provides a melt-treated post-CaTi x O y As a coating material, it has higher density, more uniform crystal structure and better coating effect.

[0053] In a specific implementation, in the green body, the mass fraction of titanium dioxide powder is 48-53%, the mass fraction of titanium powder is 6-8%, and the mass fraction of calcium oxide is 35-40%.

[0054] The CaTi prepared by the above mass fraction x O y The coating material composed of the above-mentioned materials has a more stable physical structure and a better coating effect.

[0055] In a specific implementation, titanium dioxide powder, titanium powder and calcium oxide in a certain proportion are uniformly mixed, and then pressed into a columnar or sheet-shaped green body by a hydraulic press or cold isostatic pressing, and the green body is placed in a crucible.

[0056] It should be noted that the material of the crucible can be tungsten, molybdenum or tantalum, as long as the material of the crucible meets the high melting point. Therefore, the material of the crucible is not specifically limited in the embodiments of the present application.

[0057] In specific implementation, the material is prepared by segmented heating. First, the green body is placed in a crucible, and the crucible is placed in a furnace. After the furnace is evacuated or protected by an inert gas, the heating power is turned on to start heating.

[0058] When necessary, the furnace body can be a vacuum carbon tube furnace, a vacuum resistance furnace or a vacuum induction furnace, and the furnace body can be evacuated and heated. Therefore, the furnace body is not specifically limited in the embodiments of the present application.

[0059] In a specific implementation, the high temperature sintering treatment includes: heating to 1000-1500°C at a rate of 2-25°C / min, and then keeping the temperature for 1-10 hours. During the heat preservation treatment, the green body undergoes a solid phase synthesis reaction to form a sintered body.

[0060] Alternatively, the temperature is raised to 1000-1500°C within 1-10 hours and then kept at this temperature for 1-10 hours. During the heat preservation treatment, the green body undergoes a solid phase synthesis reaction to form a sintered body.

[0061] Preferably, the high temperature sintering treatment comprises: heating to 1200-1400°C at a rate of 4-8°C / min, and then keeping the temperature for 3-5 hours to obtain a sintered body. During the heat preservation treatment, the green body undergoes a solid phase synthesis reaction to form a sintered body.

[0062] Alternatively, the temperature is raised to 1200-1400°C within 3-5 hours and then kept at this temperature for 3-5 hours to obtain a sintered body. During the heat preservation treatment, a solid phase synthesis reaction occurs in the green body.

[0063] In a specific implementation, heating the sintered body to melt includes: heating the temperature to 1700-1900° C. at a rate of 1.5-15° C. / min, and then keeping the temperature for 1-10 hours to obtain a melt.

[0064] Alternatively, the temperature is raised to 1700-1900°C within 1-10 hours and then kept at this temperature for 1-10 hours to obtain a melt.

[0065] Preferably, heating the sintered body to melt comprises: heating the temperature to 1750-1850° C. at a rate of 2-11° C. / min, and then keeping the temperature for 3-5 hours to obtain a melt.

[0066] Alternatively, the temperature is raised to 1750-1850°C within 3-5 hours and then kept at this temperature for 3-5 hours to obtain a melt.

[0067] In some embodiments, the preparation method comprises:

[0068] Step S11: uniformly mixing titanium dioxide powder, titanium powder and calcium oxide in a certain proportion, and pressing the mixture into a green body;

[0069] Step S12: Under vacuum conditions, the green body is subjected to high temperature sintering treatment to obtain a sintered body. The composition of the obtained sintered body is CaTi x O y , CaTi x O y For coating material.

[0070] It should be noted that compared with the preparation method provided in the second aspect, the density and uniformity of the sintered body are lower, and further melting is required during coating.

[0071] In a third aspect, the present application provides an application of the coating material provided in the first or second aspect above,

[0072] Using a coating device with a diameter of 900 mm, CaTi x O y Deposited on the cleaned camera resin substrate to form a film layer.

[0073] Among them, the voltage during deposition is 6~8KV, the current is 65~75mA, and the electron beam power is 450~520W.

[0074] In a specific implementation, the voltage during deposition is 7 kV and the current is 70 mA.

[0075] The electron beam power in the above coating process is lower than that in Ti3O5 coating, which can avoid damaging the resin substrate and retain the original structure of the resin substrate.

[0076] It should be noted that the preparation technologies of optical thin films mainly include physical vapor deposition (PVD), chemical vapor deposition (CVD) and chemical liquid deposition (CLD). Among them, PVD is one of the most important preparation methods. It requires the use of a vacuum coating machine. Although the manufacturing cost is relatively high, the film thickness can be precisely controlled and the film strength is good. Among the PVD methods, thermal evaporation and ion-assisted coating technologies are more commonly used in precision optical applications.

[0077] In order to enable those skilled in the art to better understand the present invention, a method for preparing a novel high refractive index coating material provided by the present invention is described below through multiple specific embodiments.

[0078] Example

[0079] Example 1

[0080] Preparation of a new type of high refractive index coating material:

[0081] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0082] 2. Under vacuum conditions, the temperature is raised to 1300°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0083] 3. Raise the temperature to 1800℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 Composition coating material.

[0084] Example 2

[0085] The difference between Example 2 and Example 1 is only that the quality of each raw material is different.

[0086] Preparation of a new type of high refractive index coating material:

[0087] 1. Mix 46g of titanium dioxide powder, 5g of titanium powder and 43g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0088] 2. Under vacuum conditions, the temperature is raised to 1300°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0089] 3. Raise the temperature to 1800℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 0.89 O 2.50 , CaTi 0.89 O 2.50 The coating material is composed.

[0090] Example 3

[0091] The only difference between Example 3 and Example 1 is that the quality of each raw material is different.

[0092] Preparation of a new type of high refractive index coating material:

[0093] 1. Mix 52g of titanium dioxide powder, 7g of titanium powder and 42g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0094] 2. Under vacuum conditions, the temperature is raised to 1300°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0095] 3. Raise the temperature to 1800℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 1.06 O 2.74 , CaTi 1.06 O 2.74 The coating material is composed.

[0096] Example 4

[0097] The only difference between Example 4 and Example 1 is that the quality of each raw material is different.

[0098] Preparation of a new type of high refractive index coating material:

[0099] 1. Mix 56g of titanium dioxide powder, 6g of titanium powder and 32g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0100] 2. Under vacuum conditions, the temperature is raised to 1300°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0101] 3. Raise the temperature to 1800℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 1.45 O 3.45 , CaTi 1.45 O 3.45 The coating material is composed.

[0102] Based on the above-mentioned embodiments 1-4, comparative examples 1-2 are provided.

[0103] Comparative Example 1

[0104] The difference between Comparative Example 1 and Example 1 is only that the mass fractions of the raw materials are different.

[0105] Preparation of a new type of high refractive index coating material:

[0106] 1. Mix 36g of titanium dioxide powder, 12g of titanium powder and 52g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0107] 2. Under vacuum conditions, the temperature is raised to 1300°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0108] 3. Heat up to 1800 °C at a rate of 7 °C / min to completely melt the green body. After the obtained melt is successively crushed and screened, CaTi 0.75 O 1.97 is obtained, and CaTi 0.75 O 1.97 forms the coating material.

[0109] Comparative Example 2

[0110] The difference between Comparative Example 2 and Example 1 is only that: the mass fractions of the raw materials are different.

[0111] Prepare a new type of high refractive index coating material:

[0112] 1. Mix 67 g of titanium dioxide powder, 5 g of titanium powder, and 28 g of calcium oxide powder evenly, and use the cold isostatic pressing method to press them into a green body;

[0113] 2. Under vacuum conditions, heat up to 1300 °C at a rate of 6 °C / min and hold for 4 h to cause a solid-phase synthesis reaction of the green body. After high-temperature sintering treatment, a sintered body is obtained;

[0114] 3. Heat up to 1800 °C at a rate of 7 °C / min to completely melt the green body. After the obtained melt is successively crushed and screened, CaTi 1.89 O 4.36 is obtained, and CaTi 1.89 O 4.36 forms the coating material.

[0115] Investigate the phase structure changes of the coating materials composed of CaTi x O y prepared in Examples 1 to 4 and Comparative Examples 1 to 2 before and after coating. The investigation results are shown in Figure 2 and Table 1.

[0116] Figure 2 shows the phase structure of CaTi x O y before and after coating in Example 1, where "1" refers to the phase structure of CaTi x O y before coating, and "2" refers to the phase structure of CaTi x O y after coating (where the detection object is CaTi 1.24 O 2.97 prepared in Example 1. After detection, for CaTi x O y with other atomic number ranges (0.8 < x < 2, 2 < y < 4), the phase structure changes are the same as those in Example 1. Therefore, only CaTi is shown.1.24 O 2.97 ), it can be seen that the phase structure of the coating material remains unchanged before and after coating, proving that the coating material prepared in the embodiment of the present application has stable performance.

[0117] Table 1. Phase structure

[0118]

[0119] According to Table 1, the coating material prepared in the embodiment of the present application has basically the same physical phase before and after coating, which proves that the coating material has stable performance and is not easy to deform at high temperature.

[0120] In Comparative Example 1, the mass of the titanium dioxide powder used was too small, and the mass of the titanium powder and calcium oxide powder was even smaller, resulting in the CaTi 0.75 O 1.97 The molar amounts of oxygen atoms and titanium atoms are reduced. According to the test results, the performance of the prepared coating material is very unstable, and the phase changes significantly after coating, which will affect the hardness and refractive index of the film.

[0121] In Comparative Example 2, more titanium dioxide powder and less titanium powder and calcium oxide powder are used, which will result in the obtained CaTi 1.89 O 4.36 The number of oxygen atoms is excessive. According to the test results, the performance of the prepared coating material is also unstable. This is because the quality of each component is too different, resulting in incomplete reaction, and the uniformity and density of the obtained coating material are not high. When the coating is applied at high temperature, its phase structure is unstable and easy to change.

[0122] Therefore, a reasonable distribution of the mass of titanium dioxide powder, titanium powder and calcium oxide will help improve the performance of the coating material itself and the refractive effect after coating.

[0123] Example 5

[0124] The only difference between Example 5 and Example 1 is that the high temperature treatment during preparation and the temperature during melting are different.

[0125] Preparation of a new type of high refractive index coating material:

[0126] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0127] 2. Under vacuum conditions, the temperature is raised to 1200°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0128] 3. Raise the temperature to 1850℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 The coating material is composed.

[0129] Example 6

[0130] The only difference between Example 6 and Example 1 is that the high temperature treatment during preparation and the temperature during melting are different.

[0131] Preparation of a new type of high refractive index coating material:

[0132] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0133] 2. Under vacuum conditions, the temperature was raised to 1100°C at a rate of 6°C / min and kept at that temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body was obtained;

[0134] 3. Raise the temperature to 1900℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 The coating material is composed.

[0135] Example 7

[0136] The only difference between Example 7 and Example 1 is that the high temperature treatment during preparation and the temperature during melting are different.

[0137] Preparation of a new type of high refractive index coating material:

[0138] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0139] 2. Under vacuum conditions, the temperature is raised to 1000°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0140] 3. Raise the temperature to 1750℃ at a rate of 7℃ / min to completely melt the blank. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 The coating material is composed.

[0141] Example 8

[0142] The only difference between Example 8 and Example 1 is that the high temperature treatment during preparation and the temperature during melting are different.

[0143] Preparation of a new type of high refractive index coating material:

[0144] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0145] 2. Under vacuum conditions, the temperature is raised to 1400°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0146] 3. Raise the temperature to 1700℃ at a rate of 7℃ / min to completely melt the blank. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 The coating material is composed.

[0147] Example 9

[0148] The only difference between Example 9 and Example 1 is that the high temperature treatment during preparation and the temperature during melting are different.

[0149] Preparation of a new type of high refractive index coating material:

[0150] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0151] 2. Under vacuum conditions, the temperature is raised to 1500°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high-temperature sintering treatment, a sintered body is obtained;

[0152] 3. Raise the temperature to 1800℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 The coating material is composed.

[0153] Comparative Examples 3-5 were set based on Examples 5-9.

[0154] Comparative Example 3

[0155] The difference between Comparative Example 3 and Example 1 is that the high temperature treatment during preparation and the temperature during melting are different.

[0156] Preparation of a new type of high refractive index coating material:

[0157] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0158] 2. Under vacuum conditions, the temperature is raised to 900°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0159] 3. Raise the temperature to 1650℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 The coating material is composed.

[0160] Comparative Example 4

[0161] The difference between Comparative Example 4 and Example 1 is that the high temperature treatment during preparation and the temperature during melting are different.

[0162] Preparation of a new type of high refractive index coating material:

[0163] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0164] 2. Under vacuum conditions, the temperature is raised to 800°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0165] 3. Raise the temperature to 1950℃ at a rate of 7℃ / min to completely melt the green body. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 The coating material is composed.

[0166] Comparative Example 5

[0167] The difference between Comparative Example 5 and Example 1 is that the high temperature treatment during preparation and the temperature during melting are different.

[0168] Preparation of a new type of high refractive index coating material:

[0169] 1. Mix 52g of titanium dioxide powder, 8g of titanium powder and 37g of calcium oxide powder evenly, and press them into a green body by cold isostatic pressing;

[0170] 2. Under vacuum conditions, the temperature is raised to 1600°C at a rate of 6°C / min and kept at this temperature for 4 hours to allow the green body to undergo a solid phase synthesis reaction. After high temperature sintering treatment, a sintered body is obtained;

[0171] 3. Raise the temperature to 2000℃ at a rate of 7℃ / min to completely melt the blank. The resulting melt is crushed and screened to obtain CaTi 1.24 O 2.97 , CaTi 1.24 O 2.97 The coating material is composed.

[0172] In Example 1, Examples 5 to 9 and Comparative Examples 3 to 5, the prepared CaTi x O y The melting effect of , the inspection results refer to Table 2.

[0173] According to Table 2, the coating materials prepared at different sintering temperatures or melting treatment temperatures have different corresponding treatment effects. The melting effect will affect the density and uniformity of the obtained coating material.

[0174] According to Table 2, compared with Example 1 and Comparative Example 3, the sintering temperature and the melting treatment temperature are too low, which will cause part of the material to not melt, resulting in poor uniformity and low density of the prepared coating material.

[0175] According to Table 2, by comparing Example 1 with Comparative Example 4, if the sintering temperature is too low, only increasing the melting temperature will cause many pores to form in the melt, resulting in poor melt quality.

[0176] According to Table 2, by comparing Example 1 with Comparative Example 5, if the sintering and melting temperatures are greatly increased, overburning will occur, i.e., energy will continue to be consumed, but the performance of the obtained material will not be further improved, which will easily lead to a waste of resources.

[0177] Therefore, reasonable control of sintering temperature and melting temperature can not only optimize the performance of the obtained material, but also achieve reasonable allocation of resources and avoid waste of resources.

[0178] Table 2. Preparation temperature (℃)

[0179]

[0180] Performance Testing

[0181] 1. Detection of CaTi 1.24 O 2.97 Transmittance curve of the film prepared under the same conditions as LaTiO3, where the coating conditions are: 100℃ substrate, 1×10 -2Charge with oxygen and coat at a rate of 0.3 nm / s. See the test results in Figure 3 .

[0182] Figure 3 The "1" in 1.24 refers to CaTi 1.24 O 2.97 The transmittance curve of the thin film prepared from the coating material composed of 1.24 and 2.97 , and the "2" refers to the transmittance curve of the thin film prepared from LaTiO3.

[0183] According to Figure 3 It can be obtained that the thin film of the coating material composed of CaTi 1.24 O 2.97 has better transmittance.

[0184] Second, test the refractive indices of CaTi 1.24 O 2.97 and LaTiO3 thin films at different wavelengths. The comparison results are shown in Tables 3(a) and (b).

[0185] Table 3(a). Comparison of refractive indices of CaTi 1.24 O 2.97 and LaTiO3 at different wavelengths

[0186]

[0187] According to Table 3(a), it can be first obtained that under the same wavelength condition, the refractive index of CaTi 1.24 O 2.97 is higher than that of LaTiO3. And through testing, the refractive indices of CaTi x O y with atomic numbers in the range of (0.8 < x < 2, 2 < y < 4) are also higher than that of LaTiO x .

[0188] Secondly, according to Table 3(b), it can be obtained that when the wavelength is in the range of 400 - 540, as the wavelength increases, the refractive index of the material gradually increases. When the wavelength exceeds 540, the refractive index slightly decreases. Therefore, for the CaTi x O y prepared in the embodiments of the present application, the refractive index of the film layer formed in the wavelength range of 500 - 540 is the best.

[0189] Table 3(b). Comparison of refractive indices of CaTi 1.24 O 2.97 and LaTiO3 at different wavelengths

[0190]

[0191] In summary, for the CaTi x O yNot only is the performance more stable, but also the CaTi x O y The coating material composed of the above-mentioned components has a higher refractive index after coating and the coating conditions are simpler, which can avoid damaging the coating matrix material.

[0192] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0193] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present application.

[0194] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.

[0195] The above is a detailed introduction to a new type of high-refractive index coating material, preparation method and application provided by the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for general technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. Application of a high refractive index coating material, characterized in that: The coating material consists of CaTi x O y where (0.8 < x < 2, 2 < y < 4); The preparation method of the coating material comprises: A certain proportion of titanium dioxide powder, titanium powder and calcium oxide are mixed evenly and pressed into a green body; Under vacuum conditions, the green body is subjected to high-temperature sintering treatment to obtain a sintered body; the high-temperature sintering treatment comprises: heating to 1000-1500° C. at a rate of 2-25° C. / min, and then keeping the temperature for 1-10 h to obtain the sintered body; The sintered body is heated to melt, and the melt is cooled, crushed and sieved to obtain the CaTi x O y , the CaTi x O y The coating material is formed; when the sintered body is heated to melt, the temperature is raised to 1700-1900°C at a rate of 1.5-15°C / min, and then kept at this temperature for 1-10 hours to obtain the melt; Wherein, by weight, in the green body, the mass fraction of the titanium dioxide powder is 40-60%, the mass fraction of the titanium powder is 5-10%, and the mass fraction of the calcium oxide is 30-45%; The CaTi x O y Depositing on the cleaned camera resin substrate to form a film layer; Among them, the voltage during deposition is 6~8KV, the current is 65~75mA, and the electron beam power is 450~520W.

2. The use of the high refractive index coating material according to claim 1, characterized in that: The CaTi x O y In which, the value range of the number of titanium atoms x includes: 0.85 < x < 1.5, and the value range of the number of oxygen atoms y includes: 2.5 < y < 3.

5.

3. The use of the high refractive index coating material according to claim 1, characterized in that: By weight, in the green body, the mass fraction of the titanium dioxide powder is 48-53%, the mass fraction of the titanium powder is 6-8%, and the mass fraction of the calcium oxide is 35-40%.

4. The use of the high refractive index coating material according to claim 1, characterized in that: The high temperature sintering treatment comprises: heating to 1200-1400° C. at a rate of 4-8° C. / min, and then keeping the temperature for 3-5 hours to obtain the sintered body.

5. The use of the high refractive index coating material according to claim 1, characterized in that: The step of heating the sintered body to melt comprises: heating the temperature to 1750-1850° C. at a rate of 2-11° C. / min, and then keeping the temperature for 3-5 hours to obtain the melt.