Flocculent nano silver powder and preparation method thereof

By controlling the preparation method of nano-silver powder, including the configuration of silver solution and dispersion and the redox reaction conditions, the problems of low particle size, sintering activity and high porosity of nano-silver powder in the existing technology are solved, and a nano-silver powder with high conductivity and high porosity is prepared. Sintered active flocculent nano-silver powder meets the needs of high-temperature conductive and thermally conductive materials.

CN118513562BActive Publication Date: 2024-10-18CHANGCHUN GOLD RES INST
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410994798.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-18
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The existing nano-silver powder preparation technology has problems such as unstable seed crystals, high environmental protection processing costs, low particle size sintering activity and high porosity, making it difficult to meet the needs of high-temperature conductive and thermal conductive materials.

Method used

A method for preparing flocculent nanometer silver powder is adopted. By configuring silver solution, dispersion liquid and reducing liquid, the redox reaction conditions and pH value are controlled, and organic reagents such as polyethylene glycol are used to modify the surface of silver powder particles to reduce the amount of powder. The contact points between particles and organic systems improve sintering activity and conductivity.

Benefits of technology

Flocculent nano-silver powder with a monomer particle size of 50 to 150 nm is prepared. The particle size distribution is uniform and the morphology is multi-particle bridge-like. It significantly improves the affinity with low-temperature slurry and reduces the porosity and resistance value after curing. Improved electrical conductivity and sintering activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118513562B_ABST
    Figure CN118513562B_ABST
Patent Text Reader

Abstract

The present invention provides a flocculent nano silver powder and a preparation method thereof, belonging to the technical field of nano silver powder preparation. The method controls the addition mode of the dispersion liquid and the reducing liquid, so that the organic reagent cooperates with the dispersant and the reducing agent, and the pH value of the reaction system is synergistically controlled to prepare the flocculent nano silver powder. At the same time, the use of the organic reagent in the reaction process has the effect of surface modification of the silver powder particles, significantly improving the compatibility of the silver powder with the organic carrier, so that the silver powder does not need to be separately subjected to wet or dry surface coating treatment, thereby optimizing the process flow. Compared with the monodispersed micro-nano silver powder, the surface morphology of the prepared flocculent nano silver powder significantly improves the affinity with the slurry system under the same weight conditions, avoids the pore phenomenon caused by the excessively fast heating rate during solidification, thereby reducing the porosity of the slurry and the resistance value after solidification, improving the conductivity, reducing the solidification temperature, and improving the sintering activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano silver powder preparation, and in particular to flocculent nano silver powder and a preparation method thereof. Background Art

[0002] At present, micro-nano silver powder has been widely used in photovoltaic cells, electronic paste, semiconductors, biomedicine and many other fields due to its excellent electrical and thermal conductivity. With the continuous upgrading and iteration of solar cells and electronic information technology, HJT and other batteries require silver powder particle size to gradually transition to nanometer level to meet the low-temperature curing requirements of the paste.

[0003] In addition, in the field of semiconductor packaging, third-generation medium and high frequency semiconductors such as SiC and GaN require a new generation of packaging materials that can withstand an operating temperature of 300-600°C and have high thermal conductivity, electrical conductivity, and stability for long-term use at high temperatures. Common brazing packaging materials such as PbSn and AuSn can no longer meet the needs of actual applications. Ag can be used for a new generation of packaging materials with an operating temperature of more than 500°C and a thermal conductivity of 80-300W / mK, and has the characteristics of "low temperature process and high temperature service". At present, the mainstream pressureless and pressure sintering silver technologies both require rapid sintering on the substrate at a temperature below 200°C and low porosity.

[0004] At present, the preparation of nano silver powder by liquid phase chemical reduction method is usually to reduce the particle size of silver powder by increasing the amount of seed precursor in an acidic system. However, this method has problems such as unstable seed and high environmental treatment cost, while the alkaline system usually uses formaldehyde and other strong reducing agents to prepare small-particle silver powder, which is seriously harmful to the environment and human body. In addition, the sintering activity of silver powder with a particle size of about 300nm still needs to be improved. On the other hand, due to its large specific surface area, the solid content of silver powder is low and the porosity is high when it is slurried, which seriously affects the conductivity of silver paste.

[0005] Therefore, based on the above problems, it is necessary to develop a flocculent nano silver powder and a preparation method thereof to further improve the density and sintering activity of the slurry during low-temperature curing. Summary of the invention

[0006] In view of the above-mentioned defects of the prior art, the present invention provides a method for preparing flocculent nano silver powder, comprising the following steps:

[0007] S1, prepare silver solution

[0008] Fully dissolve silver nitrate in deionized water, then add an organic reagent to the solution, and after fully mixing, add ammonia water dropwise until the pH value of the solution is 5-10 to obtain a silver solution; wherein the mass ratio of silver nitrate, organic reagent, and deionized water is 2: (0.01-0.4): 5; the organic reagent is one of polyethylene glycol, polyvinyl alcohol, polypropylene glycol, and triethanolamine;

[0009] S2, prepare dispersion liquid and reducing liquid

[0010] Add polyvinyl pyrrolidone into deionized water and stir until completely dissolved to obtain a dispersion; add vitamin C into deionized water and stir until completely dissolved to obtain a reduced solution;

[0011] S3, redox reaction

[0012] Under the preset temperature and stirring conditions, the dispersion liquid and the reducing liquid are added to the silver solution respectively, and the silver powder material is obtained after the reaction is complete; wherein the dispersion liquid and the reducing liquid are added by first pouring the dispersion liquid and then immediately pouring the reducing liquid to react, or pouring the dispersion liquid once and then adjusting the solution system pH>3 with ammonia water and adding the reducing liquid by dropwise addition;

[0013] S4, silver powder post-treatment

[0014] The silver powder material obtained in step S3 is subjected to solid-liquid separation and washed with deionized water to an end point, and then washed with ethanol and dried to obtain a flocculent nano silver powder product.

[0015] As a further improvement of the present invention, in step S2, the mass concentration of the dispersion is 20 g / L to 50 g / L, and the amount of the dispersant is 0.05% to 10% of the mass of the silver nitrate.

[0016] As a further improvement of the present invention, in step S2, the mass concentration of the reducing solution is 100 g / L to 300 g / L.

[0017] As a further improvement of the present invention, in step S2, the model of the polyvinyl pyrrolidone is K30.

[0018] As a further improvement of the present invention, in step S3, when the dispersion liquid and the reducing solution are added by pouring the dispersion liquid at one time, adjusting the solution system pH>3 with ammonia water and adding the reducing solution by dropwise addition, the dropping speed of the reducing solution is 10 mL / min to 50 mL / min.

[0019] As a further improvement of the present invention, in step S3, the reaction temperature is 20°C to 30°C, and the stirring speed is 200rpm to 500rpm.

[0020] As a further improvement of the present invention, in step S4, the end point of the washing with deionized water is that the conductivity of the silver powder supernatant is less than 20 μS / cm.

[0021] As a further improvement of the present invention, in step S4, the silver powder drying temperature is 40°C to 60°C.

[0022] The present invention also provides a flocculent nano silver powder, which is prepared by the above technical solution. The monomer particle size of the flocculent nano silver powder is 50-150nm, the particle size distribution is uniform, and the morphology is multi-particle bridge-shaped.

[0023] The beneficial effects of the present invention are:

[0024] 1. The preparation method of flocculent nano silver powder of the present invention controls the adding mode of the dispersion liquid and the reducing solution. Specifically, the present invention controls the adding mode of the dispersion liquid and the reducing solution to first pour the dispersion liquid and then immediately pour the reducing solution into the mixture for reaction or pour the dispersion liquid once and then adjust the pH value of the solution system to be greater than 3 with ammonia water and add the reducing solution by dropwise addition, so that the organic reagent cooperates with the dispersant and the reducing agent, and the pH value of the reaction system is synergistically controlled to prepare the flocculent nano silver powder; at the same time, the use of the organic reagent in the reaction process plays an effect of surface modification of the silver powder particles, significantly improves the compatibility of the silver powder with the organic carrier, eliminates the need for separate wet or dry surface coating treatment of the silver powder, and optimizes the process flow.

[0025] 2. The monomer particle size of the flocculent nano silver powder prepared by the present invention is 50-150nm, the particle size distribution is uniform, and the morphology is multi-particle bridge-shaped; compared with the monodispersed micro-nano silver powder, under the same weight conditions, the flocculent nano silver powder can reduce the contact points between the powder particles and the organic system, and the surface morphology of the clustered silver powder can significantly improve the affinity with the low-temperature slurry system, avoiding the pore phenomenon caused by the excessively fast heating rate during curing, thereby reducing the porosity of the slurry and the resistance value after curing, and improving the conductivity. In addition, the bridge-shaped nano silver powder can further reduce the curing temperature and improve the sintering activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the SEM image of the flocculent nano-silver powder prepared in Example 1.

[0027] Figure 2 This is the SEM image of the flocculent nano-silver powder prepared in Example 2.

[0028] Figure 3 This is the SEM image of the flocculent nano-silver powder prepared in Example 3.

[0029] Figure 4 This is the SEM image of the flocculent nano-silver powder prepared in Example 7.

[0030] Figure 5 This is the SEM image of the flocculent nano-silver powder prepared in Comparative Example 1.

[0031] Figure 6 This is the SEM image of the flocculent nano-silver powder prepared in Comparative Example 2.

[0032] Figure 7 This is the SEM image of the flocculent nano-silver powder prepared in Comparative Example 3.

[0033] Figure 8 This is the SEM image of the flocculent nano-silver powder prepared in Comparative Example 4. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0036] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0037] The present invention provides a method for preparing flocculent nano silver powder, comprising the following steps:

[0038] S1. Prepare silver solution

[0039] Fully dissolve silver nitrate in deionized water, then add a certain amount of organic reagent to the solution, and after fully mixing, add ammonia water until the pH value of the solution is 5-10 to obtain a silver solution; wherein the mass ratio of silver nitrate, organic reagent and deionized water is 2: (0.01-0.4): 5; the organic reagent is one or more of polyethylene glycol, polyvinyl alcohol, polypropylene glycol and triethanolamine;

[0040] S2. Prepare dispersion liquid and reducing liquid

[0041] A certain amount of polyvinyl pyrrolidone and vitamin C are added into deionized water respectively, and stirred until completely dissolved to obtain a dispersion liquid and a reduced solution respectively; the mass concentrations of the dispersion liquid and the reduced solution are 20g / L-50g / L and 100g / L-300g / L respectively, and the amount of the dispersant is 0.05%-10% of the mass of silver nitrate; the model of polyvinyl pyrrolidone is K30;

[0042] S3. Redox reaction

[0043] Under certain temperature and stirring conditions, the dispersion liquid and the reducing liquid are added to the silver solution respectively, and the silver powder material is obtained after the reaction is complete; wherein the dispersion liquid and the reducing liquid are added in a manner of first pouring the dispersion liquid and then immediately pouring the reducing liquid to react, or pouring the dispersion liquid once and then adjusting the pH of the solution system to greater than 3 with ammonia water and adding the reducing liquid by dropwise addition; the reaction temperature and the stirring speed are 20° C. to 30° C. and 200 rpm to 500 rpm respectively;

[0044] When the dispersion liquid and the reducing solution are added by pouring the dispersion liquid at once, adjusting the solution system pH>3 with ammonia water, and adding the reducing solution by dropwise addition, the dropping speed of the reducing solution is 10 mL / min to 50 mL / min;

[0045] S4, silver powder post-processing

[0046] The silver powder material obtained in step S3 is subjected to solid-liquid separation and washed with deionized water until the conductivity of the silver powder supernatant is less than 20 μS / cm, and then washed with ethanol and dried to obtain a flocculent nano silver powder product. The silver powder is dried at a temperature of 40° C. to 60° C. for 4 to 8 hours.

[0047] The monomer particle size of the flocculent nano silver powder obtained by the above-mentioned preparation method is 50-150nm, the particle size distribution is uniform, and the morphology is a multi-particle bridge shape.

[0048] Compared with monodisperse micro-nano silver powder, the flocculent nano silver powder prepared by the present invention can reduce the contact points between powder particles and organic systems under the same weight conditions, and the surface morphology of clustered silver powder can significantly improve the affinity with the slurry system, avoiding the pore phenomenon caused by too fast heating rate during curing, thereby reducing the porosity of the slurry and the resistance value after curing, and improving the conductivity. In addition, the bridge-shaped nano silver powder can further reduce the curing temperature and improve the sintering activity.

[0049] The preparation method of the flocculent nano silver powder provided by the present invention is described below with reference to specific examples.

[0050] Example 1

[0051] This embodiment provides a method for preparing flocculent nano silver powder, which specifically comprises the following steps:

[0052] S1. Prepare silver solution

[0053] 20 g of silver nitrate was fully dissolved in 50 mL of deionized water, and then 0.1 g of triethanolamine was added to the solution. After the mixture was fully mixed, ammonia water was added dropwise to obtain a silver solution with a pH value of 5; that is, the mass ratio of silver nitrate, organic reagent, and deionized water was 2:0.01:5;

[0054] S2. Prepare dispersion liquid and reducing liquid

[0055] 2 g of polyvinyl pyrrolidone K30 and 12.5 g of vitamin C were added to 50 mL of deionized water, respectively, and stirred until completely dissolved to obtain a dispersion and a reduced solution, respectively; that is, the mass concentration of the dispersion was 40 g / L, and the mass concentration of the reduced solution was 250 g / L;

[0056] S3. Redox reaction

[0057] Under the conditions of a temperature of 25° C. and a stirring speed of 300 rpm, the dispersion liquid is first poured into the silver solution at once, the pH value of the solution system is adjusted to about 4 with ammonia water, and the reducing liquid is added to the reaction system at a drop rate of 20 mL / min to react;

[0058] S4, silver powder post-processing

[0059] The silver powder material obtained in step S3 is subjected to solid-liquid separation and washed with deionized water until the conductivity of the silver powder supernatant is 15 μS / cm. After washing with ethanol, it is dried at 50° C. for 6 hours to obtain a flocculent nano silver powder product.

[0060] Example 2

[0061] A method for preparing flocculent nano silver powder is disclosed. Compared with Example 1, the difference is that in step S3, the dispersion liquid and the reducing solution are added by pouring the dispersion liquid at one time and then immediately pouring the reducing solution into the dispersion liquid for reaction. The rest is substantially the same as Example 1 and will not be described herein.

[0062] Embodiment 3-5

[0063] A method for preparing flocculent nano silver powder, compared with Example 1, is different in that the organic reagent used in step S1 is changed, as shown in Table 1; the rest is substantially the same as Example 1 and will not be described again.

[0064] Table 1

[0065]

[0066] The microscopic morphologies of the flocculent nano silver powders prepared in Examples 1, 2 and 3 are as follows: Figure 1 , Figure 2 , Figure 3It can be seen that the monomer particle size of the flocculent nano silver powder prepared by the present invention is 50-150 nm, the particle size distribution is uniform, and the morphology is a multi-particle bridge shape.

[0067] As can be seen from the figure, adding equal amounts of polyethylene glycol, polyvinyl alcohol, polypropylene glycol, and triethanolamine can prepare flocculent nano-silver powder with a monomer particle size of about 100nm and uniform particle size distribution, and the slurry-forming performance is excellent. The viscosity of the prepared low-temperature silver paste under the test condition of 100rpm is about 75Pa·s, and it can achieve rapid curing at a temperature of 160°C.

[0068] Examples 6-7 and Comparative Examples 1-2

[0069] A method for preparing flocculent nano silver powder, compared with Example 1, is different in that the mass ratio of silver nitrate, organic reagent and deionized water in step S1 is changed, as shown in Table 2; the rest is substantially the same as Example 1 and will not be repeated here.

[0070] Table 2

[0071]

[0072] Figure 4 , Figure 5 , Figure 6 They are SEM images of flocculent nano silver powder prepared in Example 7, Comparative Example 1 and Comparative Example 2, respectively.

[0073] As can be seen from the figure, when the mass ratio of silver nitrate, organic reagent and deionized water is 2: (0.01-0.4): 5, the monomer particle size of the prepared flocculent nano-silver powder is about 100 nm, the particle size distribution is uniform, and the powder sintering activity is high.

[0074] When the mass ratio of silver nitrate, organic reagent and deionized water is 2:0.005:5, the obtained silver powder has thick flakes of about 2 μm, a wide particle size distribution, poor dispersibility, and the viscosity of the prepared low-temperature slurry at 100 rpm is greater than 100 Pa·s. This is because the small amount of organic reagent used cannot achieve complete coating of the nanosilver particles and some of their crystal faces, which leads to growth differences of the silver powder particles. On the other hand, it also reduces the compatibility of the silver powder particle surface with the slurry system, resulting in poor slurry performance.

[0075] When the mass ratio of silver nitrate, organic reagent and deionized water is 2:0.5:5, the silver grains generated during the reduction process are fully coated by the excess organic reagent, which prevents some silver grains from continuing to grow. As a result, the sphericity of the prepared nano-silver powder is acceptable, but the particle size is uneven.

[0076] Comparative Example 3

[0077] A method for preparing flocculent nano silver powder is different from that in Example 1, in step S3, no ammonia water is used to adjust the pH value of the reaction process. Other aspects are substantially the same as those in Example 1 and will not be described in detail herein.

[0078] The microscopic morphology of the flocculent nano silver powder prepared in Comparative Example 3 is as follows: Figure 7 As shown, since the pH value was not regulated during the reaction, the pH of the solution was less than 1 in the later stage of the reaction, the reduction rate of the silver powder slowed down, and some of the nanosilver generated in the early stage of the reaction continued to grow, which eventually led to the increase in the diameter of the generated silver powder particles, forming large and small doped silver powder.

[0079] Comparative Example 4

[0080] A method for preparing flocculent nano silver powder is disclosed. Compared with Example 1, the difference is that in step S3, ammonia water is used to adjust the pH value of the solution system to about 4, and the dispersion liquid and the reducing solution are simultaneously added to the silver solution at a dropping speed of 20 mL / min for reaction. The rest is substantially the same as Example 1 and will not be repeated here.

[0081] The microscopic morphology of the flocculent nano silver powder prepared in Comparative Example 4 is as follows: Figure 8 As shown, since the dispersion liquid and the reducing solution are added to the silver solution in a dropwise manner at the same time, part of the nano silver powder generated during the reaction cannot be effectively wrapped by the dispersant, causing the nano silver powder to continue to grow and eventually form large and small doped silver powder.

[0082] In summary, the present invention provides a method for preparing flocculent nano silver powder. By controlling the addition method of the dispersing liquid and the reducing liquid, the organic reagent is coordinated with the dispersant and the reducing agent, and the pH value of the reaction system is synergistically controlled to prepare the flocculent nano silver powder. At the same time, the use of the organic reagent in the reaction process has the effect of modifying the surface of the silver powder particles, significantly improving the compatibility of the silver powder with the organic carrier, so that the silver powder does not need to be separately subjected to wet or dry surface coating treatment, thereby optimizing the process flow.

[0083] The monomer particle size of the flocculent nano silver powder prepared by the present invention is 50-150nm, the particle size distribution is uniform, and the morphology is multi-particle bridge-shaped; compared with the monodispersed micro-nano silver powder, under the same weight condition, the flocculent nano silver powder can reduce the contact points between the powder particles and the organic system, and the surface morphology of the clustered silver powder can significantly improve the affinity with the slurry system, avoid the pore phenomenon caused by the excessively fast heating rate during curing, thereby reducing the porosity of the slurry and the resistance value after curing, and improving the conductivity. In addition, the bridge-shaped nano silver powder can further reduce the curing temperature and improve the sintering activity.

[0084] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing flocculent nano silver powder, It is characterized in that The steps include: S1, prepare silver solution Fully dissolve silver nitrate in deionized water, then add an organic reagent to the solution, and after fully mixing, drop ammonia water until the pH value of the solution is 5-10 to obtain a silver solution; wherein the mass ratio of silver nitrate, organic reagent, and deionized water is 2: (0.01-0.4): 5; The organic reagent is one of polyethylene glycol, polyvinyl alcohol, polypropylene glycol, and triethanolamine; S2, prepare dispersion liquid and reducing liquid Add polyvinyl pyrrolidone into deionized water and stir until completely dissolved to obtain a dispersion; add vitamin C into deionized water and stir until completely dissolved to obtain a reduced solution; S3, redox reaction Under the preset temperature and stirring conditions, the dispersion liquid and the reducing liquid are added to the silver solution respectively, and the silver powder material is obtained after the reaction is complete; wherein the dispersion liquid and the reducing liquid are added by first pouring the dispersion liquid and then immediately pouring the reducing liquid to react, or pouring the dispersion liquid once and then adjusting the solution system pH>3 with ammonia water and adding the reducing liquid by dropwise addition; When the dispersion liquid and the reducing solution are added by pouring the dispersion liquid at once, adjusting the solution system pH>3 with ammonia water, and adding the reducing solution by dropwise addition, the dropping speed of the reducing solution is 10 mL / min to 50 mL / min; S4, silver powder post-treatment The silver powder material obtained in step S3 is subjected to solid-liquid separation and washed with deionized water to an end point, and then washed with ethanol and dried to obtain a flocculent nano silver powder product.

2. The method for preparing flocculent nano silver powder according to claim 1, Features: In step S2, the mass concentration of the dispersion is 20 g / L to 50 g / L, and the amount of the dispersant is 0.05% to 10% of the mass of silver nitrate.

3. The method for preparing the flocculent nano silver powder according to claim 1, Features: In step S2, the mass concentration of the reducing solution is 100 g / L to 300 g / L.

4. The method for preparing flocculent nano silver powder according to claim 1, Features: In step S2, the model of polyvinyl pyrrolidone is K30.

5. The method for preparing flocculent nano silver powder according to claim 1, Features: In step S3, the preset temperature is 20°C to 30°C, and the stirring speed is 200rpm to 500rpm.

6. The method for preparing flocculent nano silver powder according to claim 1, Features: In step S4, the end point of the deionized water washing is when the conductivity of the silver powder supernatant is less than 20 μS / cm.

7. The method for preparing flocculent nano silver powder according to claim 1, Features: In step S4, the silver powder is dried at a temperature of 40°C to 60°C.

8. A flocculent nano silver powder, It is characterized in that The flocculent nano silver powder is prepared by the preparation method of any one of claims 1 to 7, wherein the monomer particle size of the flocculent nano silver powder is 50 to 150 nm, the particle size distribution is uniform, and the morphology is a multi-particle bridge shape.

Citation Information

Patent Citations

  • Nano-silver powder and, preparation of nano-silver powder and application of nano-silver powder in low-temperature curing conductive silver paste

    CN109692971A

  • High-dispersion submicron silver powder and preparation method thereof

    CN118143278A