A porous silicon-carbon negative electrode and its preparation method and application
By adopting the preparation method of porous silicon carbon negative electrode in lithium ion batteries, using the reduction and carbonization treatment of trapezoidal phenyl polysilsesquioxane, a porous structure with high conductivity and stability is formed, which solves the problem of Si volume in lithium ion batteries. The problem of capacity loss and poor cycle performance caused by changes has been achieved, and high cycle stability and specific capacity improvement have been achieved.
Patent Information
- Application Number
- CN202410719197.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-05
AI Technical Summary
The theoretical capacity of graphite anodes in lithium-ion batteries is low, resulting in huge volume changes of Si during charging and discharging of lithium-ion batteries, leading to particle fragmentation and repeated formation of solid electrolyte interface layers, resulting in capacity loss and poor cycle performance.
Using the preparation method of porous silicon-carbon negative electrode, through the reduction and carbonization treatment of trapezoidal phenyl polysilsesquioxane, a porous structure with high conductivity and stability is formed, which adsorbs the catalyst and forms carbon nanotubes in the pores to enhance Si Particle protection and conductivity.
The cycle stability, conductivity and specific capacity of lithium-ion batteries are improved. By controlling the volume change and ion transport path of Si, a dense carbon layer and carbon nanotube structure are formed, which enhances the electrochemical performance.
Smart Images

Figure CN118515282B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrode materials, and in particular relates to a porous silicon-carbon negative electrode and a preparation method and application thereof. Background Art
[0002] With the continuous development of technology, the demand for lithium-ion battery (LIB) performance in applications such as electric vehicles and mobile devices continues to increase. The development of high-capacity and long-cycle-life positive and negative electrode battery materials is essential to achieve high-performance lithium-ion batteries. Among them, the low theoretical capacity of graphite negative electrodes has greatly hindered the further development of high-capacity lithium-ion batteries. Therefore, the development of negative electrode materials with high theoretical capacity is of great significance to the development of lithium-ion batteries.
[0003] Unlike graphite’s intercalation lithium storage mechanism, silicon (Si) anodes store Li by alloying + , making the silicon negative electrode have a higher theoretical specific capacity. In addition, silicon is abundant on the earth, environmentally friendly, and has a voltage platform of 0.3-0.5V, which eliminates the risk of lithium dendrites during charging, thereby significantly improving the safety performance of lithium-ion batteries. However, during the charging and discharging process, the huge volume change of Si caused by the lithium alloying and dealloying cycle leads to particle crushing and repeated formation of solid electrolyte interface (SEI) layer on its surface, which ultimately leads to capacity loss and poor cycle performance of silicon-based negative electrode materials. Therefore, there is an urgent need for a silicon-carbon negative electrode with good cycle stability, conductivity and specific capacity. Summary of the invention
[0004] The object of the present invention is to provide a porous silicon-carbon negative electrode and a preparation method and application thereof, so as to improve cycle stability, conductivity and specific capacity.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for preparing a porous silicon-carbon negative electrode, comprising the following steps:
[0007] Step (1) in an argon atmosphere, trapezoidal phenyl polysilsesquioxane, magnesium aluminum alloy powder, and anhydrous AlCl3 are mixed, heated, reacted, and cooled to obtain reduced porous trapezoidal phenyl polysilsesquioxane;
[0008] In the above process, magnesium-aluminum alloy powder is used to reduce trapezoidal phenyl polysilsesquioxane to partial zero-valent silicon.
[0009] Step (2) adding the reduced porous trapezoidal phenyl polysilsesquioxane into a tris(hydroxymethyl)aminomethane buffer solution, ultrasonically dispersing, adding dopamine hydrochloride, and reacting by magnetic stirring to obtain a coating polysilsesquioxane;
[0010] In the above process, dopamine hydrochloride is evenly coated on the surface of the porous trapezoidal phenyl polysilsesquioxane through self-polymerization.
[0011] Step (3) dispersing the coated polysilsesquioxane and the catalyst in ethanol, ultrasonically treating, stirring, and then stirring and drying to obtain a coated polysilsesquioxane with a catalyst loaded on its surface;
[0012] In the above process, the open pores of the porous trapezoidal phenyl polysilsesquioxane are used to adsorb the catalyst, so that the metal salt catalyst is deposited in the pores, and the cobalt nitrate etches the excess magnesium and aluminum and forms catalytic sites on the surface of the porous trapezoidal phenyl polysilsesquioxane.
[0013] Step (4) introducing a mixed gas of Ar, H2 and C2H4 into the coated polysilsesquioxane with the catalyst loaded on the surface, treating it with a dilute nitric acid solution after the reaction, removing impurities, and vacuum drying to obtain carbide deposited silicon;
[0014] In the above process, the phenyl groups of the polydopamine layer and the outer layer of the polysilsesquioxane are simultaneously carbonized at high temperature to be converted into a double carbon layer coating; and the carbon source gas C2H4 is cracked at high temperature, so that part of the carbon atoms are deposited on the surface of the porous silicon to form a carbon coating layer, and part of them are deposited on the catalyst to form carbon nanotubes interspersed in the pores; and the unreacted metal catalyst particles are removed by treatment with dilute nitric acid.
[0015] Step (5) putting carbonized deposited silicon, asphalt and graphite into a high-speed mixer, stirring and collecting the materials to obtain a porous silicon-carbon negative electrode.
[0016] Preferably, in step (1), the method for preparing ladder-shaped phenyl polysilsesquioxane comprises the following steps:
[0017] 200-400 g of cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane is placed in an autoclave, cooled to -50°C, ammonia is pumped in, and then the temperature is raised to 140-160°C for reaction for 3-5 hours, and then the ammonia is removed under reduced pressure to obtain a mixture; at room temperature, the mixture is added to a mixed solution of 1.2-2.4 kg of pyridine, 0.64-1.2 kg of trimethylsilyl chloride and 150-300 mL of tetrahydrofuran for treatment for 20-28 hours, and then added to a tetrahydrofuran ethanol solution with a volume ratio of 3:7, filtered, and a ladder-shaped phenyl polysilsesquioxane is obtained.
[0018] Preferably, the preparation method of cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane comprises the following steps:
[0019] 400-600 g of phenyltrichlorosilane is added to 1.2-1.8 L of acetone, and 20-30 kg of an ice-water mixture with a volume ratio of 1:1 is added under stirring at 2-4° C., and the precipitate precipitated after 9-11 days is collected at 3-5° C.; then the precipitate is dissolved in ether, and the ether mixture is washed with water until the washing water is neutral, and then dried with Na2SO4 for 20-28 hours, and then the ether is evaporated at 40-45° C., and the precipitate is washed with benzene for 3-5 times to obtain cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane.
[0020] The structural formula of cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane is as follows:
[0021] Among them, cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane was subjected to mass spectrometry analysis, HRMS (ESI) m / z: 552.05 (100.0%), 553.06 (26.5%), 553.05 (20.3%), 554.05 (14.9%), 554.06 (10.4%), 555.06 (5.7%), 555.05 (2.1%), 556.05 (1.3%).
[0022] Preferably, in step (1), the mass ratio of magnesium to aluminum alloy is 1:0.5-0.75; the oxygen and water contents of the argon gas are both lower than 1 ppm; the mass ratio of trapezoidal phenyl polysilsesquioxane, magnesium to aluminum alloy powder, and anhydrous AlCl3 is (0.05-0.1):(0.15-0.3):(0.5-1); and the heating rate is 4-6°C·min -1 ; Heating temperature is 530-550℃; Reaction time is 10-14h; Cooling method is natural cooling to room temperature.
[0023] Preferably, in step (2), the amount ratio of the reduced porous trapezoidal phenyl polysilsesquioxane, tris(hydroxymethyl)aminomethane buffer solution, and dopamine hydrochloride is (20-40) g:(20-40) L:(40-80) g; the concentration of the tris(hydroxymethyl)aminomethane buffer solution is 0.1 mol / L, and the pH is 8.5; the ultrasonic dispersion time is 20-30 min; and the magnetic stirring reaction conditions are: the magnetic stirring reaction temperature is room temperature, and the magnetic stirring reaction time is 20-28 h.
[0024] Preferably, in step (3), the ratio of the amount of coating polysilsesquioxane, catalyst and ethanol is (20-40) g: (8-16) g: (100-200) mL; the ultrasonic treatment time is 2-3 h; the stirring treatment time is 4-6 h; the stirring and drying temperature is 90-110° C.; and the catalyst includes at least one of cobalt nitrate and nickel nitrate.
[0025] Preferably, in step (4), the ratio of Ar, H2 and C2H4 mixed gas is (30-40):(1-1.5):(3-4); reaction conditions: reaction temperature is 700-900°C, reaction time is 2-4h; concentration of dilute nitric acid solution is 6-7wt%; treatment time of dilute nitric acid solution is 0.4-0.6h, and impurity removal method is washing with water 3-5 times; vacuum drying conditions: vacuum drying temperature is 55-65°C, vacuum drying time is 10-14h.
[0026] Preferably, in step (5), the mass ratio of carbonized deposited silicon, asphalt and graphite is (800-1200):(30-50):(10-20); the stirring conditions are: stirring temperature is 100-120°C, stirring speed is 600-1200r / min, and stirring time is 10-30min; the average particle size of asphalt D50 is 4-6μm.
[0027] The porous silicon-carbon negative electrode is prepared by the method for preparing the porous silicon-carbon negative electrode.
[0028] Preferably, the present invention also provides application of the porous silicon-carbon negative electrode in lithium-ion batteries.
[0029] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0030] 1. The present invention adopts ladder-shaped polyphenyl silsesquioxane with improved physical and chemical properties, which has high thermal stability and thermal oxidation stability; by controlling the ratio of aluminum and magnesium metals, the inner part of the Si-O-Si skeleton of the ladder-shaped phenyl polysilsesquioxane is partially reduced to Si, and silicon is segregated at the same time, and pores are formed inside the ladder-shaped phenyl polysilsesquioxane; the open pores are used to adsorb catalysts, and the closed pores provide space for volume expansion. The developed pore structure fully adapts to the volume change of silicon, shortens the diffusion path of ions, is beneficial to ion transmission, and accelerates the transmission rate.
[0031] 2. In the present invention, the phenyl groups directly connected to the Si atoms in the polysilsesquioxane act as the carbon source of the internal dense coating, and are simultaneously carbonized at high temperature with the polydopamine layer to be converted into a double carbon layer coating to obtain an inorganic-organic hybrid material. Due to the bonding interaction between the phenyl groups and the Si atoms, the carbon layer wrapped by the phenyl groups is abnormally dense, providing effective protection for the internal Si particles and forming a stable solid electrolyte interface layer. The carbonization of the external polydopamine layer enhances the electrical conductivity of the internal Si particles and synergistically buffers the volume expansion with the porous structure. At the same time, the carbon source gas is cracked at high temperature and in-situ deposited on the catalyst to form carbon nanotubes interspersed in the pores. The carbon nanotubes have high conductivity and flexibility, and form a highly elastic and highly conductive layer on the surface of the double carbon deposited Si, achieving a highly stable buffering effect.
[0032] 3. In the present invention, the in-situ growth of carbon nanotubes will greatly increase the specific surface area of the material. Excessive active sites exposed to the electrolyte will cause uncontrollable electrolyte decomposition, resulting in low first efficiency. Asphalt and graphite are used to reduce the specific surface area to improve the electrochemical performance of the porous silicon-carbon negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 It is a process flow chart of the preparation of the porous silicon-carbon negative electrode of the present invention;
[0035] Figure 2 is a bar graph of the reversible specific capacity of the porous silicon-carbon negative electrode of the present invention;
[0036] Figure 3 It is a line graph of the charge and discharge efficiency and cycle capacity retention rate of the porous silicon-carbon negative electrode of the present invention. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Example 1
[0039] This embodiment discloses a method for preparing cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane, comprising the following steps:
[0040] 500 g of phenyltrichlorosilane was added to 1.5 L of acetone, and 25 kg of an ice-water mixture with a volume ratio of 1:1 was added under stirring at 3° C. The precipitate precipitated after 10 days was collected at 4° C. The precipitate was then dissolved in ether, and the ether mixture was washed with water until the washing water was neutral, and then dried with Na2SO4 for 24 h, and then the ether was evaporated at 42° C. The obtained precipitate was washed with benzene 4 times to obtain cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane.
[0041] Example 2
[0042] This embodiment discloses a method for preparing a ladder-shaped phenyl polysilsesquioxane, comprising the following steps:
[0043] 300 g of cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane prepared in Example 1 was placed in an autoclave, cooled to -50°C, ammonia was pumped in, and then the temperature was raised to 150°C for reaction for 3-5 h, and then the ammonia was removed under reduced pressure to obtain a mixture; at room temperature, the mixture was added to a mixed solution of 1.8 kg of pyridine, 0.96 kg of trimethylsilyl chloride and 225 mL of tetrahydrofuran and treated for 24 h, and then added to a tetrahydrofuran ethanol solution with a volume ratio of 3:7, filtered, and a ladder-shaped phenyl polysilsesquioxane was obtained.
[0044] Example 3
[0045] See also Figure 1 As shown, this embodiment discloses a method for preparing a porous silicon-carbon negative electrode, comprising the following steps:
[0046] Step (1) In an argon atmosphere with oxygen and water contents both lower than 1 ppm, 75 g of the trapezoidal phenyl polysilsesquioxane prepared in Example 2, 0.22 kg of magnesium-aluminum alloy powder, and 0.75 kg of anhydrous AlCl3 were mixed and heated at 5 °C / min. -1 The temperature was raised to 540° C. at a heating rate of 1:1, and the reaction was continued for 12 hours, and then the temperature was naturally cooled to room temperature to obtain reduced porous trapezoidal phenyl polysilsesquioxane, wherein the mass ratio of the magnesium-aluminum alloy was 1:0.6;
[0047] Step (2) adding 30 g of reduced porous trapezoidal phenyl polysilsesquioxane to 30 L of 0.1 mol / L tris(hydroxymethylaminomethane) buffer solution with a pH of 8.5, and ultrasonically dispersing for 25 min, adding 60 g of dopamine hydrochloride, and reacting under magnetic stirring at room temperature for 24 h to obtain a coating polysilsesquioxane;
[0048] Step (3) dispersing 30 g of the coated polysilsesquioxane and 12 g of cobalt nitrate in 150 mL of ethanol, ultrasonically treating for 2.5 h, stirring for 5 h to make them uniformly dispersed, and then stirring and drying at 100° C. to obtain a coated polysilsesquioxane with a surface-loaded catalyst;
[0049] Step (4) introducing a mixed gas of Ar, H2 and C2H4 into the coated polysilsesquioxane with the catalyst loaded on the surface, reacting at 800° C. for 3 h, treating with a 6.5 wt % dilute nitric acid solution for 0.5 h, washing with water 4 times, and vacuum drying at 60° C. for 12 h to obtain carbide deposited silicon, wherein the ratio of the mixed gas of Ar, H2 and C2H4 is 35:1.3:3.5;
[0050] Step (5) putting carbonized deposited silicon, asphalt and graphite into a high-speed mixer, stirring at 100-120° C. and a speed of 600-1200 r / min for 10-30 min, collecting the materials to obtain a porous silicon-carbon negative electrode, wherein the mass ratio of carbonized deposited silicon, asphalt and graphite is 1000:40:15.
[0051] Example 4
[0052] See also Figure 1 As shown, this embodiment discloses a method for preparing a porous silicon-carbon negative electrode, comprising the following steps:
[0053] Step (1) In an argon atmosphere with oxygen and water contents both lower than 1 ppm, 50 g of the trapezoidal phenyl polysilsesquioxane prepared in Example 2, 0.3 kg of magnesium aluminum alloy powder, and 0.5 kg of anhydrous AlCl3 were mixed and heated at 6 °C·min -1 The temperature was raised to 530° C. at a heating rate of 1:1, and the reaction was continued for 14 hours, and then the temperature was naturally cooled to room temperature to obtain reduced porous trapezoidal phenyl polysilsesquioxane, wherein the mass ratio of the magnesium-aluminum alloy was 1:0.5;
[0054] Step (2) adding 40 g of reduced porous trapezoidal phenyl polysilsesquioxane to 20 L of 0.1 mol / L tris(hydroxymethylaminomethane) buffer solution with a pH of 8.5, and ultrasonically dispersing for 30 min, adding 40 g of dopamine hydrochloride, and reacting under magnetic stirring at room temperature for 20 h to obtain a coating polysilsesquioxane;
[0055] Step (3) dispersing 40 g of the coated polysilsesquioxane and 8 g of nickel nitrate in 200 mL of ethanol, ultrasonically treating for 2 h, stirring for 6 h to make them uniformly dispersed, and then stirring and drying at 90° C. to obtain a coated polysilsesquioxane with a surface-loaded catalyst;
[0056] Step (4) introducing a mixed gas of Ar, H2 and C2H4 into the coated polysilsesquioxane with the catalyst loaded on the surface, reacting it at 900° C. for 2 h, treating it with a 7 wt % dilute nitric acid solution for 0.4 h, washing it with water for 5 times, and vacuum drying it at 55° C. for 14 h to obtain carbide deposited silicon, wherein the ratio of the mixed gas of Ar, H2 and C2H4 is 30:1.5:3;
[0057] Step (5) Put the carbonized deposited silicon, asphalt and graphite into a high-speed mixer, stir at 120° C. and 600 r / min for 30 min, collect the materials, and obtain a porous silicon-carbon negative electrode, wherein the mass ratio of the carbonized deposited silicon, asphalt and graphite is 800:50:10.
[0058] Example 5
[0059] See also Figure 1 As shown, this embodiment discloses a method for preparing a porous silicon-carbon negative electrode, comprising the following steps:
[0060] Step (1) In an argon atmosphere with oxygen and water contents both lower than 1 ppm, 100 g of the trapezoidal phenyl polysilsesquioxane prepared in Example 2, 0.15 kg of magnesium-aluminum alloy powder, and 1 kg of anhydrous AlCl3 were mixed and heated at 4 °C·min-1 The temperature was raised to 550° C. at a heating rate of 1:1, and the reaction was continued for 10 hours, and then the mixture was naturally cooled to room temperature to obtain reduced porous trapezoidal phenyl polysilsesquioxane, wherein the mass ratio of the magnesium-aluminum alloy was 1:0.75;
[0061] Step (2) adding 20 g of reduced porous trapezoidal phenyl polysilsesquioxane to 40 L of 0.1 mol / L tris(hydroxymethylaminomethane) buffer solution with a pH of 8.5, and ultrasonically dispersing for 20 min, adding 80 g of dopamine hydrochloride, and reacting under magnetic stirring at room temperature for 28 h to obtain a coating polysilsesquioxane;
[0062] Step (3) dispersing 20 g of the coated polysilsesquioxane and 16 g of cobalt nitrate in 100 mL of ethanol, ultrasonically treating for 3 h, stirring for 4 h to make them uniformly dispersed, and then stirring and drying at 110° C. to obtain a coated polysilsesquioxane with a surface-loaded catalyst;
[0063] Step (4) introducing a mixed gas of Ar, H2 and C2H4 into the coated polysilsesquioxane with the catalyst loaded on the surface, reacting it at 700° C. for 4 hours, treating it with a 6 wt % dilute nitric acid solution for 0.6 hours, washing it with water for 3 times, and vacuum drying it at 65° C. for 10 hours to obtain carbide deposited silicon, wherein the ratio of the mixed gas of Ar, H2 and C2H4 is 40:1:4;
[0064] Step (5) Put the carbonized deposited silicon, asphalt and graphite into a high-speed mixer, stir at 100°C and 1200 r / min for 10 min, collect the materials, and obtain a porous silicon-carbon negative electrode, wherein the mass ratio of the carbonized deposited silicon, asphalt and graphite is 1200:30:20.
[0065] Example 6
[0066] See also Figure 1 As shown, this embodiment discloses a method for preparing a porous silicon-carbon negative electrode, comprising the following steps:
[0067] Step (1) In an argon atmosphere with oxygen and water contents both lower than 1 ppm, 60 g of the trapezoidal phenyl polysilsesquioxane prepared in Example 2, 0.27 kg of magnesium aluminum alloy powder, and 0.6 kg of anhydrous AlCl3 were mixed and heated at 6 °C·min -1 The temperature was raised to 535°C at a heating rate of 1:1, and the reaction was continued for 13 hours. The temperature was then naturally cooled to room temperature to obtain reduced porous trapezoidal phenyl polysilsesquioxane. The mass ratio of the magnesium-aluminum alloy was 1:0.6.
[0068] Step (2) adding 35 g of reduced porous trapezoidal phenyl polysilsesquioxane to 25 L of 0.1 mol / L tris(hydroxymethylaminomethane) buffer solution with a pH of 8.5, and ultrasonically dispersing for 28 min, adding 50 g of dopamine hydrochloride, and reacting under magnetic stirring at room temperature for 26 h to obtain a coating polysilsesquioxane;
[0069] Step (3) dispersing 25 g of the coated polysilsesquioxane and 14 g of nickel nitrate in 130 mL of ethanol, ultrasonically treating for 3 h, stirring for 4 h to make them uniformly dispersed, and then stirring and drying at 95° C. to obtain a coated polysilsesquioxane with a surface-loaded catalyst;
[0070] Step (4) introducing a mixed gas of Ar, H2 and C2H4 into the coated polysilsesquioxane with the catalyst loaded on the surface, reacting at 850° C. for 3 h, treating with a 6 wt % dilute nitric acid solution for 0.5 h, washing with water for 5 times, and vacuum drying at 60° C. for 11 h to obtain carbide deposited silicon, wherein the ratio of the mixed gas of Ar, H2 and C2H4 is 35:1.1:3.6;
[0071] Step (5) Put the carbonized deposited silicon, asphalt and graphite into a high-speed mixer, stir at 105°C and 1100 r / min for 15 min, collect the materials, and obtain a porous silicon-carbon negative electrode. The mass ratio of the carbonized deposited silicon, asphalt and graphite is 900:45:15.
[0072] Example 7
[0073] See also Figure 1 As shown, this embodiment discloses a method for preparing a porous silicon-carbon negative electrode, comprising the following steps:
[0074] Step (1) In an argon atmosphere with oxygen and water contents both lower than 1 ppm, 90 g of the trapezoidal phenyl polysilsesquioxane prepared in Example 2, 0.18 kg of magnesium-aluminum alloy powder, and 0.9 kg of anhydrous AlCl3 were mixed and heated at 4 °C·min -1 The temperature was raised to 545°C at a heating rate of 1:1, and the reaction was continued for 13 hours. The temperature was then naturally cooled to room temperature to obtain reduced porous trapezoidal phenyl polysilsesquioxane. The mass ratio of the magnesium-aluminum alloy was 1:0.7.
[0075] Step (2) adding 25 g of reduced porous trapezoidal phenyl polysilsesquioxane to 35 L of 0.1 mol / L tris(hydroxymethylaminomethane) buffer solution with a pH of 8.5, and ultrasonically dispersing for 25 min, adding 70 g of dopamine hydrochloride, and reacting under magnetic stirring at room temperature for 22 h to obtain a coating polysilsesquioxane;
[0076] Step (3) dispersing 35 g of the coated polysilsesquioxane and 10 g of cobalt nitrate in 180 mL of ethanol, ultrasonically treating for 2 h, stirring for 6 h to make them uniformly dispersed, and then stirring and drying at 105° C. to obtain a coated polysilsesquioxane with a surface-loaded catalyst;
[0077] Step (4) introducing a mixed gas of Ar, H2 and C2H4 into the coated polysilsesquioxane with the catalyst loaded on the surface, reacting at 750° C. for 3 h, treating with a 7 wt % dilute nitric acid solution for 0.6 h, washing with water for 3 times, and vacuum drying at 55° C. for 13 h to obtain carbide deposited silicon, wherein the ratio of the mixed gas of Ar, H2 and C2H4 is 40:1.3:3.2;
[0078] Step (5) Put the carbonized deposited silicon, asphalt and graphite into a high-speed mixer, stir at 115°C and 700 r / min for 25 min, collect the materials, and obtain a porous silicon-carbon negative electrode. The mass ratio of the carbonized deposited silicon, asphalt and graphite is 1100:35:20.
[0079] Comparative Example 1
[0080] Comparative Example 1 Compared with Example 3, in the process of preparing the porous silicon-carbon negative electrode in Comparative Example 1, silicon powder is used to replace trapezoidal phenyl polysilsesquioxane, and other conditions remain unchanged.
[0081] Comparative Example 2
[0082] Compared with Example 3, in the process of preparing the porous silicon-carbon negative electrode in Comparative Example 2, step (2) is omitted, that is, dopamine hydrochloride is not added to form a coating, and other conditions remain unchanged.
[0083] Comparative Example 3
[0084] Comparative Example 3 Compared with Example 3, in the process of preparing the porous silicon-carbon negative electrode in Comparative Example 3, no carbon nanotubes were generated in situ, and other conditions remained unchanged.
[0085] Comparative Example 4
[0086] Compared with Example 3, in the process of preparing the porous silicon-carbon negative electrode, Comparative Example 4 does not include step (5), and other conditions remain unchanged.
[0087] Experimental example
[0088] The performance of the porous silicon-carbon negative electrodes prepared in Examples 3-7 and Comparative Examples 1-4 was tested:
[0089] Electrochemical performance test
[0090] The porous silicon-carbon negative electrode prepared in Examples 3-7 and Comparative Examples 1-4 and the counter electrode lithium sheet were used to make half-cells, and their related electrochemical properties were tested. The test results are shown in Table 1. Among them, the conductive agent is conductive carbon Super "p", the separator is celgard2400, and the electrolyte is 1 mol / L LiPF6 conductive salt and DMC:DEC:EC (wt%) = 1:1:1 solvent. The test conditions are: the charge and discharge cut-off voltage is 0.05-2V, the first reversible specific capacity is tested at 0.1C, and the cycle efficiency is tested 20 times at 0.2C. The test results are shown in Table 1.
[0091] Table 1
[0092]
[0093] It can be seen from Table 1 that the electrochemical performance of the porous silicon-carbon negative electrode prepared in Examples 3-7 is much better than that of the porous silicon-carbon negative electrode prepared in Comparative Examples 1-4. The preparation method of the present invention can be used to prepare a porous silicon-carbon negative electrode with good cycle stability, good conductivity and high specific capacity. From the comparison between Comparative Example 1 and Example 3, it can be seen that in the process of preparing the porous silicon-carbon negative electrode, the present invention uses trapezoidal phenyl polysilsesquioxane to improve the electrochemical performance of the porous silicon-carbon negative electrode; from the comparison between Comparative Example 2 and Example 3, it can be seen that in the process of preparing the porous silicon-carbon negative electrode, the present invention adds dopamine hydrochloride to improve the electrochemical performance of the porous silicon-carbon negative electrode; from the comparison between Comparative Example 3 and Example 3, it can be seen that in the process of preparing the porous silicon-carbon negative electrode, the present invention generates carbon nanotubes in situ to improve the electrochemical performance of the porous silicon-carbon negative electrode; from the comparison between Comparative Example 4 and Example 3, it can be seen that in the process of preparing the porous silicon-carbon negative electrode, the present invention adds asphalt and graphite to improve the electrochemical performance of the porous silicon-carbon negative electrode.
[0094] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0095] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a porous silicon-carbon negative electrode, characterized in that: The following steps are involved: Step (1) in an argon atmosphere, trapezoidal phenyl polysilsesquioxane, magnesium aluminum alloy powder, and anhydrous AlCl3 are mixed, heated, reacted, and cooled to obtain reduced porous trapezoidal phenyl polysilsesquioxane; Step (2) adding the reduced porous trapezoidal phenyl polysilsesquioxane into a tris(hydroxymethyl)aminomethane buffer solution, ultrasonically dispersing, adding dopamine hydrochloride, and reacting by magnetic stirring to obtain a coating polysilsesquioxane; Step (3) dispersing the coated polysilsesquioxane and the catalyst in ethanol, ultrasonically treating, stirring, and then stirring and drying to obtain a coated polysilsesquioxane with a surface-loaded catalyst; Step (4) introducing a mixed gas of Ar, H2 and C2H4 into the coated polysilsesquioxane with the catalyst loaded on the surface, treating with a dilute nitric acid solution after the reaction, removing impurities, and vacuum drying to obtain carbide deposited silicon; Step (5) putting carbonized deposited silicon, asphalt and graphite into a high-speed mixer, stirring and collecting the materials to obtain a porous silicon-carbon negative electrode.
2. The method for preparing a porous silicon-carbon negative electrode according to claim 1, characterized in that: In the step (1), the preparation method of ladder-shaped phenyl polysilsesquioxane comprises the following steps: 200-400 g of cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane is placed in an autoclave, cooled to -50°C, ammonia is pumped in, and then the temperature is raised to 140-160°C for reaction for 3-5 hours, and then the ammonia is removed under reduced pressure to obtain a mixture; at room temperature, the mixture is added to a mixed solution of 1.2-2.4 kg of pyridine, 0.64-1.2 kg of trimethylsilyl chloride and 150-300 mL of tetrahydrofuran for treatment for 20-28 hours, and then added to a tetrahydrofuran ethanol solution with a volume ratio of 3:7, filtered, and a ladder-shaped phenyl polysilsesquioxane is obtained.
3. The method for preparing a porous silicon-carbon negative electrode according to claim 2, characterized in that: The preparation method of the cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane comprises the following steps: 400-600 g of phenyltrichlorosilane is added to 1.2-1.8 L of acetone, and 20-30 kg of an ice-water mixture with a volume ratio of 1:1 is added under stirring at 2-4° C., and the precipitate precipitated after 9-11 days is collected at 3-5° C.; then the precipitate is dissolved in ether, and the ether mixture is washed with water until the washing water is neutral, and then dried with Na2SO4 for 20-28 hours, and then the ether is evaporated at 40-45° C., and the precipitate is washed with benzene for 3-5 times to obtain cis-tetrahydroxy-(tetraphenyl)cyclotetrasiloxane.
4. The method for preparing a porous silicon-carbon negative electrode according to claim 1, characterized in that: In the step (1), the mass ratio of magnesium-aluminum alloy is 1:0.5-0.75; the oxygen and water contents of the argon gas are both lower than 1 ppm; the mass ratio of trapezoidal phenyl polysilsesquioxane, magnesium-aluminum alloy powder, and anhydrous AlCl3 is (0.05-0.1):(0.15-0.3):(0.5-1); the heating rate is 4-6°C·min -1 ; Heating temperature is 530-550℃; Reaction time is 10-14h; Cooling method is natural cooling to room temperature.
5. The method for preparing a porous silicon-carbon negative electrode according to claim 1, characterized in that: In the step (2), the amount ratio of the reduced porous trapezoidal phenyl polysilsesquioxane, tris(hydroxymethyl)aminomethane buffer solution, and dopamine hydrochloride is (20-40) g:(20-40) L:(40-80) g; the concentration of the tris(hydroxymethyl)aminomethane buffer solution is 0.1 mol / L, and the pH is 8.5; the ultrasonic dispersion time is 20-30 min; and the magnetic stirring reaction conditions are: the magnetic stirring reaction temperature is room temperature, and the magnetic stirring reaction time is 20-28 h.
6. The method for preparing a porous silicon-carbon negative electrode according to claim 1, characterized in that: In the step (3), the amount ratio of the coating polysilsesquioxane, the catalyst, and the ethanol is (20-40) g: (8-16) g: (100-200) mL; the ultrasonic treatment time is 2-3 h; the stirring treatment time is 4-6 h; the stirring and drying temperature is 90-110° C.; and the catalyst includes at least one of cobalt nitrate and nickel nitrate.
7. The method for preparing a porous silicon-carbon negative electrode according to claim 1, characterized in that: In the step (4), the ratio of Ar, H2 and C2H4 mixed gas is (30-40):(1-1.5):(3-4); reaction conditions: reaction temperature is 700-900°C, reaction time is 2-4h; concentration of dilute nitric acid solution is 6-7wt%; treatment time of dilute nitric acid solution is 0.4-0.6h, and impurity removal method is washing with water 3-5 times; vacuum drying conditions: vacuum drying temperature is 55-65°C, vacuum drying time is 10-14h.
8. The method for preparing a porous silicon-carbon negative electrode according to claim 1, characterized in that: In the step (5), the mass ratio of carbonized deposited silicon, asphalt and graphite is (800-1200):(30-50):(10-20); the stirring conditions are: stirring temperature is 100-120°C, stirring speed is 600-1200r / min, and stirring time is 10-30min; the average particle size of asphalt D50 is 4-6μm.
Citation Information
Patent Citations
Preparation method of silicon-carbon cathode material, silicon-carbon cathode material and lithium ion battery
CN107507972A
Porous silicon-carbon composite cathode material as well as preparation method thereof and lithium ion battery
CN107994225A
Porous silicon carbon negative electrode material, preparation method and application
CN115911341A
Methods for the production of spherical silicon-carbon nanocomposites
DE102014210613A1
Silicon-Containing Carbonaceous Composite Material
US20140023929A1