A thickener for improving oil recovery and preparation method thereof

The problem is solved by using a thickening agent copolymerized with cage octamer (3-ammonium chloride propyl) silsesquioxane, acrylamide and 2-acrylamido-2-methylpropanesulfonic acid, combined with a clay stabilizer, etc. Existing thickeners are prone to degradation and formation adsorption in high-temperature and high-salt environments, so efficient and environmentally friendly oil recovery has been achieved.

CN118516100BActive Publication Date: 2024-10-25PANJIN LIAOYOU HUALIAN IND GROUP CO LTD

Patent Information

Application Number
CN202410986690.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-25
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing thickeners are prone to degradation in high-temperature and high-salt environments, resulting in formation adsorption losses, high costs, and environmental pollution, making it difficult to meet the demand for increased oil recovery.

Method used

It is a polymer obtained by copolymerizing cage octamer (3-ammonium chloride propyl) silsesquioxane, acrylamide and 2-acrylamido-2-methylpropanesulfonic acid, combined with clay stabilizer, emulsifier, Buffering agent and preservative, forming thickener with high viscosity and stability.

Benefits of technology

It maintains good thickening performance and stability under high-temperature and high-salt conditions, reduces formation adsorption losses, improves oil recovery, and is environmentally friendly and cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516100B_ABST
    Figure CN118516100B_ABST
Patent Text Reader

Abstract

The invention relates to the field of oil production, and specifically to a thickener for improving oil recovery and a preparation method thereof, wherein the thickener for improving oil recovery is composed of the following raw materials in parts by weight: 40-70 parts of OCAPS / AMPS / AM polymer, 2-6 parts of clay stabilizer, 8-12 parts of emulsifier, 1-3 parts of buffer and 1-2 parts of preservative, the OCAPS / AMPS / AM polymer is prepared from the following raw materials in parts by weight: 2.5-25 parts of OCAPS, 10-100 parts of AMPS, 1000 parts of AM and 0.5-1.9 parts of AIBA, and OCAPS is prepared from the following raw materials in parts by weight: 0.94-1.88 parts of KH550 and 1.18-1.77 parts of concentrated hydrochloric acid. The thickener for improving oil recovery prepared by the invention has good thickening and viscosity-enhancing effects and improves oil recovery, is stable under early high temperature and high salt conditions, and has good oil displacement performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of petroleum exploitation, in particular to a thickener for improving oil recovery and a preparation method thereof. Background Art

[0002] As one of the world's major energy sources, the exploration and development of oil is of great significance to the national economy and social development. However, the non-renewable and consumable nature of oil resources makes how to efficiently recover underground oil one of the key issues in the oil industry. Oil recovery rate is directly related to the economic benefits and sustainable development of oil fields. In order to improve the recovery rate, traditional mining methods have gradually become unable to meet modern needs. As a result, various technologies to improve oil recovery have emerged, among which the application of thickeners has become an important means. Thickeners are a class of chemical substances that can significantly change the rheological properties of liquids and increase their viscosity. In the process of oil extraction, thickeners are mainly used in two fields: chemical flooding and physical flooding. Chemical flooding changes the oil-water interfacial tension and fluid rheological properties by injecting chemical solutions, such as surfactants and polymer solutions, into the bottom layer, thereby improving oil recovery efficiency; physical flooding changes the formation conditions by injecting gases, thermal fluids and other substances to increase the fluidity of crude oil.

[0003] At present, polymer flooding is one of the most widely used thickener technologies. Acrylamide (AM) and its derivatives have become the main thickener components for polymer flooding due to their excellent thickening effect and chemical stability. However, polymer flooding still faces challenges in practical applications, such as degradation in high temperature and high salt environments, and formation adsorption loss. Although the existing thickener technology has improved oil recovery to a certain extent, it still has the following problems: (1) The formation temperature of many oil fields is high and the mineralization is large, which requires high chemical stability of the thickener. Acrylamide polymers are prone to degradation and lose their thickening effect in such environments; (2) After the thickener is injected into the formation, part of it will be adsorbed or retained by the formation rock, resulting in a decrease in effective utilization, increased costs and reduced oil recovery effects; (3) High cost: The preparation cost of high-efficiency thickeners is high. The synthesis process of some new functional polymers is complicated, and it is difficult to reduce production costs, which limits their application; (4) Traditional chemically synthesized polymers are difficult to degrade, causing environmental pollution. Therefore, there is still room for the development and research of thickeners, such as improving the resistance to high temperature and high salt by introducing nanomaterials and functionalized monomers, or using natural polymer materials to develop thickeners that are biocompatible and environmentally friendly, improving processes and reducing costs, etc.

[0004] Thickeners for enhanced oil recovery have important application value and broad development prospects in the petroleum industry. With the introduction and optimization of new materials and new processes, their performance and application effects will be significantly improved, providing strong support for efficient and environmentally friendly oil development. Summary of the invention

[0005] The invention provides a thickener for improving oil recovery and a preparation method thereof. The thickener components include a cage-type octa-(3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer (OCAPS / AMPS / AM polymer) obtained by copolymerization of cage-type octa-(3-ammonium chloride propyl) silsesquioxane, acrylamide and 2-acrylamido-2-methylpropanesulfonic acid, a clay stabilizer, an emulsifier, a buffer and a preservative. The prepared thickener has good viscosity-increasing effect in an aqueous phase and good stability in use.

[0006] A thickener for improving oil recovery, comprising the following raw materials in parts by weight: 40-70 parts of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, 2-6 parts of clay stabilizer, 8-12 parts of emulsifier, 1-3 parts of buffer and 1-2 parts of preservative;

[0007] The caged octa (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 2.5-25 parts of caged octa (3-ammonium chloride propyl) silsesquioxane (OCAPS), 10-100 parts of 2-acrylamido-2-methylpropane sulfonic acid (AMPS), 1000 parts of acrylamide (AM) and 0.5-1.9 parts of azobisisobutyramidine hydrochloride (AIBA), wherein 2-acrylamido-2-methylpropane sulfonic acid, acrylamide and azobisisobutyramidine hydrochloride are all commercially available analytical reagents;

[0008] The cage-type octa(3-ammonium chloride propyl)silsesquioxane is prepared from the following raw materials in parts by weight: 0.94-1.88 parts of 3-aminopropyltriethoxysilane (KH550) and 1.18-1.77 parts of concentrated hydrochloric acid, wherein both 3-aminopropyltriethoxysilane and concentrated hydrochloric acid are analytical grade reagents.

[0009] Further, the preparation of the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer comprises the following steps:

[0010] Q1, add 3-aminopropyltriethoxysilane and concentrated hydrochloric acid to anhydrous methanol in sequence, and stir magnetically at 400-800 rpm for 30-90 min until homogeneous to obtain a mixture;

[0011] Q2, stirring the mixture at room temperature at 300-500 rpm for 10-14 days to generate a white microcrystalline precipitate, which was filtered, recrystallized, washed, and dried to obtain cage-type octameric (3-ammonium chloride propyl) silsesquioxane;

[0012] Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring at 300-500 rpm until completely dissolved to obtain monomer solution A;

[0013] Q4, add cage-type octameric (3-ammonium chloride propyl) silsesquioxane to the monomer solution A obtained in Q3, stir mechanically at 400-700 rpm for 30-60 min to fully disperse it, transfer it to a three-necked flask, and introduce nitrogen for 30 min to remove dissolved oxygen, thereby obtaining monomer solution B;

[0014] Q5, dissolve azobisisobutylamidine hydrochloride in deionized water, ultrasonicate for 10-15 minutes until dissolved, to obtain azobisisobutylamidine hydrochloride solution, place the monomer solution B in Q4 in a constant temperature water bath at 50-70°C, and maintain mechanical stirring at 200-300 rpm, inject the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerize under a nitrogen atmosphere. After the reaction is completed, cool to room temperature, filter to obtain a colloidal product, transfer to anhydrous ethanol, soak and dehydrate for 20-24 hours, and dry at 80°C in a vacuum drying oven for 20-30 hours to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer.

[0015] Preferably, the volume ratio of 3-aminopropyltriethoxysilane, concentrated hydrochloric acid and anhydrous methanol in step Q1 is 1~2:1~1.5:1000.

[0016] Preferably, the total monomer concentration in the monomer solution B in step Q4 is 20-30 wt %, wherein the mass ratio of cage-type octa(3-ammonium chloride propyl)silsesquioxane:2-acrylamido-2-methylpropanesulfonic acid:acrylamide is 0.25-2.5:1-10:100.

[0017] Preferably, the concentration of the azobisisobutylamidine hydrochloride solution in step Q5 is 0.01-0.05 wt %, and the copolymerization reaction is carried out at 50-70° C. for 2-6 h.

[0018] Furthermore, the present invention also proposes a method for preparing a thickener for enhancing oil recovery, comprising the following steps:

[0019] S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder;

[0020] S2, dissolving 4-7 g / L cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder, 0.2-0.6 g / L clay stabilizer, 0.8-1.2 g / L emulsifier, 0.1-0.3 g / L buffer and 0.1-0.2 g / L preservative in water, stirring at 300-600 rpm until the mixture is uniformly mixed, thereby obtaining the thickener for enhancing oil recovery.

[0021] Preferably, the clay stabilizer is one of epichlorohydrin / diethylenetriamine clay stabilizer, 2-chloroethyltrimethylammonium chloride clay stabilizer or potassium chloride clay stabilizer.

[0022] Preferably, the emulsifier is one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate or lecithin.

[0023] Preferably, the preservative is glutaraldehyde.

[0024] Preferably, the buffer is disodium hydrogen phosphate-sodium dihydrogen phosphate or disodium hydrogen phosphate-potassium dihydrogen phosphate;

[0025] Further, the preparation method of epichlorohydrin / diethylenetriamine clay stabilizer is as follows:

[0026] Add diethylenetriamine and distilled water into a four-necked flask, stir at 200 rpm until completely dissolved, then cool, slowly drop epichlorohydrin in a water bath at 25-30°C, and start stirring at the same time, with a stirring speed of 300-500 rpm. After the addition is completed, heat to 60-80°C, react for 2-3 hours, collect the product, wash, and dry to obtain epichlorohydrin / diethylenetriamine clay stabilizer.

[0027] Preferably, the molar ratio of diethylenetriamine to epichlorohydrin is 1 to 3:1.

[0028] The beneficial effects achieved by the present invention are as follows:

[0029] The invention provides a thickener for improving oil recovery, which consists of a cage-type octa-(3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, a clay stabilizer, an emulsifier, a buffer and a preservative. The cage-type octa-(3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is a high molecular polymer obtained by copolymerizing cage-type octa-(3-ammonium chloride propyl) silsesquioxane, 2-acrylamido-2-methylpropane sulfonic acid and acrylamide.

[0030] The reaction system generates free radicals under the action of the initiator, and the free radicals initiate the double bonds in acrylamide and 2-acrylamido-2-methylpropane sulfonic acid to form active centers and copolymerize with other monomers. Cage-type octa-(3-ammonium chloride propyl) silsesquioxane, 2-acrylamido-2-methylpropane sulfonic acid and acrylamide participate in the copolymerization reaction. Cage-type octa-(3-ammonium chloride propyl) silsesquioxane contains ammonium chloride groups and siloxy groups. The ammonium chloride groups are deprotonated to generate amino groups, and then copolymerize with other monomers to form a three-dimensional cross-linked network structure, thereby obtaining a cage-type octa-(3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer. The polymer is the main component of the thickener. Different units in its structure are not only covalently bonded, but also hydrogen-bonded and electrostatically interact with each other. The long-chain polymer molecules are intertwined and extended with each other, which has an excellent thickening effect. It can significantly increase the viscosity and flow resistance of the water phase at a lower concentration and improve the oil displacement effect. The sulfonic acid group provided by the 2-acrylamido-2-methylpropanesulfonic acid monomer is hydrophilic and negatively charged, which can effectively resist ion interference in a high-salinity environment and can still maintain good thickening performance and stability under high temperature and high-salinity conditions. At the same time, 2-acrylamido-2-methylpropanesulfonic acid monomer has a hydrophilic and negatively charged sulfonic acid group, which can effectively resist ion interference in a high-salinity environment and can still maintain good thickening performance and stability under high temperature and high-salinity conditions. The synergistic effect of methylpropane sulfonic acid and acrylamide monomers has a reinforcing effect on its performance; the cage-type octa(3-ammonium chloride propyl) silsesquioxane structure provides cage-type steric hindrance, preventing the polymer molecular chains from transitioning close and folding, maintaining the unfolded state of the high molecular weight polymer, and further improving and maintaining the viscosity. The cage-type octa(3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is easily soluble in water to form a uniform and stable solution. The polymer has low adsorption on the rock surface and less loss during injection and flow, which improves its utilization efficiency.

[0031] The thickener obtained by compounding cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer with clay stabilizer, emulsifier, buffer and preservative not only has the effect of increasing viscosity and improving recovery rate, but also can maintain good stability under high temperature and high salt conditions, has good oil displacement effect and strong usability. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions therein, the following briefly introduces the drawings required for use in the descriptions of the embodiments and comparative examples. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0033] Figure 1 Apparent viscosity-viscosity release rate bar graph of thickeners used for enhanced oil recovery;

[0034] Figure 2 A bar graph of shear stability of thickeners used for enhanced oil recovery;

[0035] Figure 3 Viscosity bar graph of degelling hydrated liquid with thickener for enhanced oil recovery;

[0036] Figure 4 Bar graph of suspended sand fraction for thickeners used to enhance oil recovery. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The described embodiments are part of the embodiments of the present invention, but not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1: A thickener for enhancing oil recovery, comprising the following raw materials in parts by weight: 55 parts of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer, 4 parts of clay stabilizer, 10 parts of emulsifier, 2 parts of buffer and 1.5 parts of preservative;

[0039] The caged octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 12.5 parts of caged octapoly (3-ammonium chloride propyl) silsesquioxane, 50 parts of 2-acrylamido-2-methylpropane sulfonic acid, 1000 parts of acrylamide and 1.2 parts of azobisisobutyramidine hydrochloride;

[0040] The cage-type octa(3-ammonium chloride propyl)silsesquioxane was prepared from the following raw materials in parts by weight: 0.94 parts of 3-aminopropyltriethoxysilane and 1.18 parts of concentrated hydrochloric acid.

[0041] The preparation of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer comprises the following steps:

[0042] Q1, 1 mL of 3-aminopropyltriethoxysilane and 1 mL of concentrated hydrochloric acid were added to 1000 mL of anhydrous methanol in sequence, and magnetically stirred at 400 rpm for 90 min until homogeneous to obtain a mixture;

[0043] Q2, the mixture was stirred at room temperature at 300 rpm for 14 days to generate white microcrystalline precipitate, which was filtered, recrystallized, washed and dried to obtain cage-type octameric (3-ammonium chloride propyl) silsesquioxane;

[0044] Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring at 300 rpm until completely dissolved, to obtain a monomer solution A;

[0045] Q4, add cage-type octa(3-ammonium chloride propyl)silsesquioxane to the monomer solution A obtained in Q3, stir mechanically at 400 rpm for 60 min to make it completely dispersed, transfer to a three-necked flask, and introduce nitrogen for 30 min to remove dissolved oxygen, to obtain a 20 wt% monomer solution B;

[0046] Q5, dissolve azobisisobutylamidine hydrochloride in deionized water, ultrasonicate for 10 minutes until dissolved, obtain a 0.01wt% azobisisobutylamidine hydrochloride solution, place the monomer solution B in Q4 in a constant temperature water bath at 50°C, and maintain mechanical stirring at 200rpm, inject the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerize at 50°C under a nitrogen atmosphere. After the reaction is completed for 6 hours, cool to room temperature, filter to obtain a colloidal product, transfer to anhydrous ethanol, soak and dehydrate for 20 hours, and dry at 80°C in a vacuum drying oven for 20 hours to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer.

[0047] The present invention also proposes a method for preparing a thickener for improving oil recovery, comprising the following steps:

[0048] S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh powder sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder;

[0049] S2, 5.5 g / L of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder, 0.4 g / L of epichlorohydrin / diethylenetriamine clay stabilizer, 1 g / L of sodium dodecyl sulfate, 0.2 g / L of disodium hydrogen phosphate-sodium dihydrogen phosphate and 0.15 g / L of glutaraldehyde are dissolved in water, and stirred at 300 rpm until the mixture is uniformly mixed, thereby obtaining the thickener for enhancing oil recovery.

[0050] Wherein, the preparation method of epichlorohydrin / diethylenetriamine clay stabilizer is as follows:

[0051] Add diethylenetriamine and distilled water into a four-necked flask, stir at 200 rpm until completely dissolved and then cool, slowly add epichlorohydrin dropwise in a water bath at 25°C and start stirring at 300 rpm. After the addition is complete, heat to 60°C and react for 3 hours. Collect the product, wash and dry to obtain epichlorohydrin / diethylenetriamine clay stabilizer, the molar ratio of diethylenetriamine to epichlorohydrin is 1:1.

[0052] Example 2: A thickener for enhancing oil recovery, comprising the following raw materials in parts by weight: 55 parts of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer, 4 parts of clay stabilizer, 10 parts of emulsifier, 2 parts of buffer and 1.5 parts of preservative;

[0053] The caged octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 12.5 parts of caged octapoly (3-ammonium chloride propyl) silsesquioxane, 50 parts of 2-acrylamido-2-methylpropane sulfonic acid, 1000 parts of acrylamide and 1.2 parts of azobisisobutyramidine hydrochloride;

[0054] The cage-type octa(3-ammonium chloride propyl)silsesquioxane was prepared from the following raw materials in parts by weight: 1.41 parts of 3-aminopropyltriethoxysilane and 1.475 parts of concentrated hydrochloric acid.

[0055] The preparation of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer comprises the following steps:

[0056] Q1, 1.5 mL of 3-aminopropyltriethoxysilane and 1.25 mL of concentrated hydrochloric acid were added to 1000 mL of anhydrous methanol in sequence, and magnetically stirred at 600 rpm for 60 min until homogeneous to obtain a mixture;

[0057] Q2, the mixture was stirred at room temperature at 400 rpm for 12 days to generate white microcrystalline precipitate, which was filtered, recrystallized, washed and dried to obtain cage-type octameric (3-ammonium chloride propyl) silsesquioxane;

[0058] Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring at 400 rpm until completely dissolved, to obtain a monomer solution A;

[0059] Q4, add cage-type octameric (3-ammonium chloride propyl) silsesquioxane to the monomer solution A obtained in Q3, stir mechanically at 550 rpm for 45 minutes to make it completely dispersed, transfer it to a three-necked flask, and pass nitrogen for 30 minutes to remove dissolved oxygen to obtain a 25 wt% monomer solution B;

[0060] Q5, dissolve azobisisobutylamidine hydrochloride in deionized water, ultrasonicate for 15 minutes until dissolved, obtain a 0.025wt% azobisisobutylamidine hydrochloride solution, place the monomer solution B in Q4 in a constant temperature water bath at 60°C, and maintain mechanical stirring at 250rpm, inject the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerize at 60°C under a nitrogen atmosphere. After the reaction is completed for 4 hours, cool to room temperature, filter to obtain a colloidal product, transfer to anhydrous ethanol, soak and dehydrate for 22 hours, and dry at 80°C in a vacuum drying oven for 25 hours to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer.

[0061] The present invention also proposes a method for preparing a thickener for improving oil recovery, comprising the following steps:

[0062] S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh powder sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder;

[0063] S2, 5.5 g / L of cage-type octa (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder, 0.4 g / L of epichlorohydrin / diethylenetriamine clay stabilizer, 1 g / L of sodium dodecylbenzene sulfonate, 0.2 g / L of disodium hydrogen phosphate-potassium dihydrogen phosphate and 0.15 g / L of glutaraldehyde are dissolved in water, and stirred at 450 rpm until the mixture is uniformly mixed, thereby obtaining the thickener for enhancing oil recovery.

[0064] Wherein, the preparation method of epichlorohydrin / diethylenetriamine clay stabilizer is as follows:

[0065] Add diethylenetriamine and distilled water into a four-necked flask, stir at 200 rpm until completely dissolved, then cool, slowly drop epichlorohydrin in a water bath at 30°C, and start stirring at the same time, the stirring speed is 500 rpm. After the addition is completed, heat to 80°C, react for 2 hours, collect the product, wash, and dry to obtain epichlorohydrin / diethylenetriamine clay stabilizer, the molar ratio of diethylenetriamine to epichlorohydrin is 3:1.

[0066] Example 3: A thickener for enhancing oil recovery, comprising the following raw materials in parts by weight: 55 parts of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, 4 parts of clay stabilizer, 10 parts of emulsifier, 2 parts of buffer and 1.5 parts of preservative;

[0067] The caged octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 12.5 parts of caged octapoly (3-ammonium chloride propyl) silsesquioxane, 50 parts of 2-acrylamido-2-methylpropane sulfonic acid, 1000 parts of acrylamide and 1.2 parts of azobisisobutyramidine hydrochloride;

[0068] The cage-type octa(3-ammonium chloride propyl)silsesquioxane was prepared from the following raw materials in parts by weight: 1.88 parts of 3-aminopropyltriethoxysilane and 1.77 parts of concentrated hydrochloric acid.

[0069] The preparation of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer comprises the following steps:

[0070] Q1, 2 mL of 3-aminopropyltriethoxysilane and 1.5 mL of concentrated hydrochloric acid were added to 1000 mL of anhydrous methanol in sequence, and magnetically stirred at 800 rpm for 30 min until homogeneous to obtain a mixture;

[0071] Q2, the mixture was stirred at room temperature at 500 rpm for 10 days to generate white microcrystalline precipitate, which was filtered, recrystallized, washed and dried to obtain cage-type octameric (3-ammonium chloride propyl) silsesquioxane;

[0072] Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring at 500 rpm until completely dissolved, to obtain a monomer solution A;

[0073] Q4, add cage-type octa(3-ammonium chloride propyl)silsesquioxane to the monomer solution A obtained in Q3, stir mechanically at 700 rpm for 30 min to make it completely dispersed, transfer to a three-necked flask, and introduce nitrogen for 30 min to remove dissolved oxygen, to obtain a 30 wt% monomer solution B;

[0074] Q5, dissolve azobisisobutylamidine hydrochloride in deionized water, ultrasonicate for 15 minutes until dissolved, obtain a 0.05wt% azobisisobutylamidine hydrochloride solution, place the monomer solution B in Q4 in a constant temperature water bath at 70°C, and maintain mechanical stirring at 300rpm, inject the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerize at 70°C under a nitrogen atmosphere. After the reaction is completed for 2 hours, cool to room temperature, filter to obtain a colloidal product, transfer to anhydrous ethanol, soak and dehydrate for 24 hours, and dry at 80°C in a vacuum drying oven for 30 hours to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer.

[0075] The present invention also proposes a method for preparing a thickener for improving oil recovery, comprising the following steps:

[0076] S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh powder sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder;

[0077] S2, 5.5 g / L of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide powder, 0.4 g / L of potassium chloride clay stabilizer, 1 g / L of lecithin, 0.2 g / L of disodium hydrogen phosphate-potassium dihydrogen phosphate and 0.15 g / L of glutaraldehyde are dissolved in water, and stirred at 450 rpm until the mixture is uniformly mixed, thereby obtaining the thickener for enhancing oil recovery.

[0078] Example 4: A thickener for enhancing oil recovery, comprising the following raw materials in parts by weight: 55 parts of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, 4 parts of clay stabilizer, 10 parts of emulsifier, 2 parts of buffer and 1.5 parts of preservative;

[0079] The caged octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 2.5 parts of caged octapoly (3-ammonium chloride propyl) silsesquioxane, 10 parts of 2-acrylamido-2-methylpropane sulfonic acid, 1000 parts of acrylamide and 0.5 parts of azobisisobutyramidine hydrochloride;

[0080] The cage-type octa(3-ammonium chloride propyl)silsesquioxane was prepared from the following raw materials in parts by weight: 1.41 parts of 3-aminopropyltriethoxysilane and 1.475 parts of concentrated hydrochloric acid.

[0081] The preparation of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer comprises the following steps:

[0082] Q1, 1.5 mL of 3-aminopropyltriethoxysilane and 1.25 mL of concentrated hydrochloric acid were added to 1000 mL of anhydrous methanol in sequence, and magnetically stirred at 800 rpm for 30 min until homogeneous to obtain a mixture;

[0083] Q2, the mixture was stirred at room temperature at 500 rpm for 10 days to generate white microcrystalline precipitate, which was filtered, recrystallized, washed and dried to obtain cage-type octameric (3-ammonium chloride propyl) silsesquioxane;

[0084] Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring at 500 rpm until completely dissolved, to obtain a monomer solution A;

[0085] Q4, add cage-type octa(3-ammonium chloride propyl)silsesquioxane to the monomer solution A obtained in Q3, stir mechanically at 700 rpm for 30 min to make it completely dispersed, transfer to a three-necked flask, and introduce nitrogen for 30 min to remove dissolved oxygen, to obtain a 25 wt% monomer solution B;

[0086] Q5, dissolve azobisisobutylamidine hydrochloride in deionized water, ultrasonicate for 15 minutes until dissolved, obtain a 0.05wt% azobisisobutylamidine hydrochloride solution, place the monomer solution B in Q4 in a constant temperature water bath at 70°C, and maintain mechanical stirring at 300rpm, inject the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerize at 70°C under a nitrogen atmosphere. After the reaction is completed for 2 hours, cool to room temperature, filter to obtain a colloidal product, transfer to anhydrous ethanol, soak and dehydrate for 24 hours, and dry at 80°C in a vacuum drying oven for 30 hours to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer.

[0087] The present invention also proposes a method for preparing a thickener for improving oil recovery, comprising the following steps:

[0088] S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh powder sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder;

[0089] S2, 5.5 g / L of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder, 0.4 g / L of epichlorohydrin / diethylenetriamine clay stabilizer, 1 g / L of lecithin, 0.2 g / L of disodium hydrogen phosphate-potassium dihydrogen phosphate and 0.15 g / L of glutaraldehyde are dissolved in water, and stirred at 450 rpm until the mixture is uniformly mixed, thereby obtaining the thickener for enhancing oil recovery.

[0090] Example 5: A thickener for enhancing oil recovery, comprising the following raw materials in parts by weight: 55 parts of cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, 4 parts of clay stabilizer, 10 parts of emulsifier, 2 parts of buffer and 1.5 parts of preservative;

[0091] The caged octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 25 parts of caged octapoly (3-ammonium chloride propyl) silsesquioxane, 100 parts of 2-acrylamido-2-methylpropane sulfonic acid, 1000 parts of acrylamide and 1.9 parts of azobisisobutyramidine hydrochloride;

[0092] The cage-type octa(3-ammonium chloride propyl)silsesquioxane was prepared from the following raw materials in parts by weight: 1.41 parts of 3-aminopropyltriethoxysilane and 1.475 parts of concentrated hydrochloric acid.

[0093] The preparation of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer comprises the following steps:

[0094] Q1, 1.5 mL of 3-aminopropyltriethoxysilane and 1.25 mL of concentrated hydrochloric acid were added to 1000 mL of anhydrous methanol in sequence, and magnetically stirred at 800 rpm for 30 min until homogeneous to obtain a mixture;

[0095] Q2, the mixture was stirred at room temperature at 500 rpm for 10 days to generate white microcrystalline precipitate, which was filtered, recrystallized, washed and dried to obtain cage-type octameric (3-ammonium chloride propyl) silsesquioxane;

[0096] Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring at 500 rpm until completely dissolved, to obtain a monomer solution A;

[0097] Q4, add cage-type octa(3-ammonium chloride propyl)silsesquioxane to the monomer solution A obtained in Q3, stir mechanically at 700 rpm for 30 min to make it completely dispersed, transfer to a three-necked flask, and introduce nitrogen for 30 min to remove dissolved oxygen, to obtain a 25 wt% monomer solution B;

[0098] Q5, dissolve azobisisobutylamidine hydrochloride in deionized water, ultrasonicate for 15 minutes until dissolved, obtain a 0.05wt% azobisisobutylamidine hydrochloride solution, place the monomer solution B in Q4 in a constant temperature water bath at 70°C, and maintain mechanical stirring at 300rpm, inject the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerize at 70°C under a nitrogen atmosphere. After the reaction is completed for 2 hours, cool to room temperature, filter to obtain a colloidal product, transfer to anhydrous ethanol, soak and dehydrate for 24 hours, and dry at 80°C in a vacuum drying oven for 30 hours to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer.

[0099] The present invention also proposes a method for preparing a thickener for improving oil recovery, comprising the following steps:

[0100] S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh powder sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder;

[0101] S2, 5.5 g / L of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder, 0.4 g / L of epichlorohydrin / diethylenetriamine clay stabilizer, 1 g / L of lecithin, 0.2 g / L of disodium hydrogen phosphate-potassium dihydrogen phosphate and 0.15 g / L of glutaraldehyde are dissolved in water, and stirred at 450 rpm until the mixture is uniformly mixed, thereby obtaining the thickener for enhancing oil recovery.

[0102] Example 6: A thickener for enhancing oil recovery, comprising the following raw materials in parts by weight: 40 parts of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, 2 parts of clay stabilizer, 8 parts of emulsifier, 1 part of buffer and 1 part of preservative;

[0103] The caged octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 25 parts of caged octapoly (3-ammonium chloride propyl) silsesquioxane, 100 parts of 2-acrylamido-2-methylpropane sulfonic acid, 1000 parts of acrylamide and 1.9 parts of azobisisobutyramidine hydrochloride;

[0104] The cage-type octa(3-ammonium chloride propyl)silsesquioxane was prepared from the following raw materials in parts by weight: 1.41 parts of 3-aminopropyltriethoxysilane and 1.475 parts of concentrated hydrochloric acid.

[0105] The preparation of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer comprises the following steps:

[0106] Q1, 1.5 mL of 3-aminopropyltriethoxysilane and 1.25 mL of concentrated hydrochloric acid were added to 1000 mL of anhydrous methanol in sequence, and magnetically stirred at 800 rpm for 30 min until homogeneous to obtain a mixture;

[0107] Q2, the mixture was stirred at room temperature at 500 rpm for 10 days to generate white microcrystalline precipitate, which was filtered, recrystallized, washed and dried to obtain cage-type octameric (3-ammonium chloride propyl) silsesquioxane;

[0108] Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring at 500 rpm until completely dissolved, to obtain a monomer solution A;

[0109] Q4, add cage-type octa(3-ammonium chloride propyl)silsesquioxane to the monomer solution A obtained in Q3, stir mechanically at 700 rpm for 30 min to make it completely dispersed, transfer to a three-necked flask, and introduce nitrogen for 30 min to remove dissolved oxygen, to obtain a 25 wt% monomer solution B;

[0110] Q5, dissolve azobisisobutylamidine hydrochloride in deionized water, ultrasonicate for 15 minutes until dissolved, obtain a 0.05wt% azobisisobutylamidine hydrochloride solution, place the monomer solution B in Q4 in a constant temperature water bath at 70°C, and maintain mechanical stirring at 300rpm, inject the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerize at 70°C under a nitrogen atmosphere. After the reaction is completed for 2 hours, cool to room temperature, filter to obtain a colloidal product, transfer to anhydrous ethanol, soak and dehydrate for 24 hours, and dry at 80°C in a vacuum drying oven for 30 hours to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer.

[0111] The present invention also proposes a method for preparing a thickener for improving oil recovery, comprising the following steps:

[0112] S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh powder sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder;

[0113] S2, 4 g / L cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide powder, 0.2 g / L epichlorohydrin / diethylenetriamine clay stabilizer, 0.8 g / L lecithin, 0.1 g / L disodium hydrogen phosphate-potassium dihydrogen phosphate and 0.1 g / L glutaraldehyde are dissolved in water, and stirred at 450 rpm until the mixture is uniformly mixed, thereby obtaining the thickener for enhancing oil recovery.

[0114] Example 7: A thickener for enhancing oil recovery, comprising the following raw materials in parts by weight: 70 parts of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, 6 parts of clay stabilizer, 12 parts of emulsifier, 3 parts of buffer and 2 parts of preservative;

[0115] The caged octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 25 parts of caged octapoly (3-ammonium chloride propyl) silsesquioxane, 100 parts of 2-acrylamido-2-methylpropane sulfonic acid, 1000 parts of acrylamide and 1.9 parts of azobisisobutyramidine hydrochloride;

[0116] The cage-type octa(3-ammonium chloride propyl)silsesquioxane was prepared from the following raw materials in parts by weight: 1.41 parts of 3-aminopropyltriethoxysilane (3-aminopropyltriethoxysilane) and 1.475 parts of concentrated hydrochloric acid.

[0117] The preparation of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer comprises the following steps:

[0118] Q1, 1.5 mL of 3-aminopropyltriethoxysilane and 1.25 mL of concentrated hydrochloric acid were added to 1000 mL of anhydrous methanol, and magnetic stirring was performed at 800 rpm for 30 min until homogeneous to obtain a mixture;

[0119] Q2, the mixture was stirred at room temperature at 500 rpm for 10 days to generate white microcrystalline precipitate, which was filtered, recrystallized, washed and dried to obtain cage-type octameric (3-ammonium chloride propyl) silsesquioxane;

[0120] Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring at 500 rpm until completely dissolved, to obtain a monomer solution A;

[0121] Q4, add cage-type octa(3-ammonium chloride propyl)silsesquioxane to the monomer solution A obtained in Q3, stir mechanically at 700 rpm for 30 min to make it completely dispersed, transfer to a three-necked flask, and introduce nitrogen for 30 min to remove dissolved oxygen, to obtain a 25 wt% monomer solution B;

[0122] Q5, dissolve azobisisobutylamidine hydrochloride in deionized water, ultrasonicate for 15 minutes until dissolved, obtain a 0.05wt% azobisisobutylamidine hydrochloride solution, place the monomer solution B in Q4 in a constant temperature water bath at 70°C, and maintain mechanical stirring at 300rpm, inject the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerize at 70°C under a nitrogen atmosphere. After the reaction is completed for 2 hours, cool to room temperature, filter to obtain a colloidal product, transfer to anhydrous ethanol, soak and dehydrate for 24 hours, and dry at 80°C in a vacuum drying oven for 30 hours to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer.

[0123] The present invention also proposes a method for preparing a thickener for improving oil recovery, comprising the following steps:

[0124] S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh powder sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder;

[0125] S2, 7 g / L of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder, 0.6 g / L of epichlorohydrin / diethylenetriamine clay stabilizer, 1.2 g / L of lecithin, 0.3 g / L of disodium hydrogen phosphate-potassium dihydrogen phosphate and 0.2 g / L of glutaraldehyde are dissolved in water, and stirred at 450 rpm until the mixture is uniformly mixed, thereby obtaining the thickener for enhancing oil recovery.

[0126] Comparative Example 1: Based on Example 7, the difference is that 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer is used instead of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer, and the remaining steps are consistent with Example 7.

[0127] Comparative Example 2: Based on Example 8, the difference is that acrylamide is used instead of cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, and the remaining steps are consistent with Example 7.

[0128] Experimental example:

[0129] 1. Appearance:

[0130] 10 mL of sample was measured and placed in a 20 mL colorimetric tube, and observed under natural light to see whether the thickener for enhanced oil recovery was stratified and precipitated. The test results are shown in Table 1.

[0131] 2. Apparent viscosity:

[0132] Use a measuring cylinder to measure 500mL of tap water and pour it into a 1000mL beaker. Place the beaker under the blade of an electric stirrer and adjust the speed to 1000r / min. Use a pipette or syringe to transfer 3mL of thickener for enhanced oil recovery and slowly add it to the beaker. After stirring for 5 minutes, use a six-speed rotary viscometer (fixed speed of 100r / min) to measure the solution viscosity η at this time. 2 .

[0133] The test results are shown in Table 2 and Figure 1 shown.

[0134] 3. Viscosity release rate:

[0135] Use a measuring cylinder to measure 500mL of tap water and pour it into a 1000mL beaker. Place the beaker under the blade of an electric stirrer and adjust the speed to 1000r / min. Use a pipette or syringe to transfer 3mL of thickener for enhanced oil recovery and slowly add it to the beaker. After stirring for 2 minutes, use a six-speed rotary viscometer (fixed speed of 100r / min) to measure the solution viscosity η at this time. 1 , viscosity release rate C 1 Calculate according to the following formula:

[0136] C 1 =η 1 / η 2 ×100%;

[0137] C 1 ——Viscosity release rate, %;

[0138] η 1 ——Viscosity after stirring for 2 minutes, mPa·s;

[0139] η 2 ——Viscosity after stirring for 5 minutes, mPa·s.

[0140] The test results are shown in Table 2 and Figure 1 shown.

[0141] 4. Shear stability:

[0142] (1) Preparation of 0.6% solution: Use a measuring cylinder to measure 500 mL of tap water and pour it into a 1000 mL beaker. Place the beaker under the blade of an electric stirrer and adjust the speed to 1000 r / min. Use a pipette or syringe to transfer 3 mL of thickener for enhanced oil recovery and slowly add it into the beaker. Stir for 5 min.

[0143] (2) Take an appropriate amount of 0.6% solution and pour it into the sample cup of RS300 or RS6000, and heat the sample; control the heating rate to 3℃ / min±0.2℃ / min, start the test at 30℃, and rotate the rotor at 170s -1 The shear rate is set to 90°C, and the shear rate and temperature are kept constant. The shear time is 60 min, and the shear viscosity value is read in mPa·s.

[0144] The test results are shown in Table 2 and Figure 2 shown.

[0145] 5. Gel breaking performance:

[0146] Take the 0.6% solution prepared in 4 (1) and put it into a beaker. Weigh 0.05% potassium persulfate and put it into a sample cup. Stir the potassium persulfate evenly with a glass rod. Seal the sample cup and place it in a constant temperature drying oven for constant heating at 90°C. After 6 hours, use a capillary viscometer to measure the viscosity of the degumming liquid at room temperature in mPa·s.

[0147] The test results are shown in Table 2 and Figure 3 shown.

[0148] 6. Static suspended sand performance

[0149] Take 435 mL of the 0.6% solution prepared in 4 (1) and put it into a 1000 mL beaker. Measure 100 mL of 20-40 mesh quartz sand and slowly add it to the beaker. Stir the solution quickly to evenly disperse the quartz sand in the solution. Pour the sample into a 500 mL graduated cylinder and observe the height of the quartz sand in the cylinder. Read the height H of the quartz sand in the cylinder after 20 minutes. 1 , calculate the suspended sand rate W according to the following formula.

[0150] W = H 1 / 500×100%;

[0151] W——suspended sand rate, %;

[0152] H 1 ——The height of quartz sand in the measuring cylinder after 20 minutes, mL.

[0153] The test results are shown in Table 2 and Figure 4 shown.

[0154] 7. Low temperature fluidity:

[0155] 300mL~500mL of thickener for enhanced oil recovery was put into a plastic bottle and placed in a -30℃ environment for 4h to observe whether the thickener for enhanced oil recovery has good fluidity and whether it is frozen. The test results are shown in Table 1.

[0156] Table 1 Appearance test and low temperature fluidity test of thickener samples for enhanced oil recovery

[0157]

[0158] Table 2 Other performance tests of thickener samples for enhanced oil recovery

[0159]

[0160] The performance of the thickener samples for enhanced oil recovery prepared in the embodiments and comparative examples was tested by experimental examples, as shown in Tables 1-2 and Figures 1 to 4As shown. The appearance test shows that the sample is translucent as a whole and has a certain viscosity. The apparent viscosity, viscosity release rate, shear stability and suspended sand rate of Examples 1 to 3 are all increased. This is because the change in the components of the preparation of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane forms more active sites on the surface of the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane, which is more conducive to the occurrence of polymerization reaction. The cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is easier to copolymerize to obtain a three-dimensional crosslinked The network structure shows that the viscosity attenuation under shearing is weakened, indicating that the viscosity of the thickener has good stability under shearing, and the viscosity of the degelling hydration liquid is significantly reduced, indicating that it has good degelling performance and can quickly and completely reduce the viscosity, which is conducive to reflux; Examples 4, 3, and 5 mainly reflect the influence of the proportion of each component of the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer on its structure and performance, and the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane, 2-acrylamido-2-methylpropanesulfonic acid The changes in the dosage of methylpropanesulfonic acid, acrylamide and initiator determine the chain length of the polymer, the entanglement of the molecular chain and the molecular weight of the polymer. With the change of the components, the apparent viscosity, viscosity release rate, shear stability and suspended sand rate of the thickener sample tend to increase, the viscosity of the degelling hydrated liquid decreases, and the degelling performance is enhanced; Examples 6, 5 and 7 mainly reflect the influence of the dosage ratio of each component of the thickener on the performance of the prepared thickener. With the change of the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer With the increase of dosage, the high molecular weight polymer in the thickener system increases, and the three-dimensional network structure and the entanglement and intermolecular interaction between the molecular chains lead to an increasing trend in the apparent viscosity, viscosity release rate, shear stability and suspended sand rate of the thickener samples, a decrease in the viscosity of the degelling hydration liquid, and an enhancement in the degelling performance; Comparative Examples 1 and 2 compare the thickeners prepared by the ternary copolymerization of cage-type octa(3-ammonium chloride propyl) silsesquioxane with 2-acrylamido-2-methylpropane sulfonic acid and acrylamide, binary copolymerization and only adding monomers, which have a significant effect on improving the performance of the thickener.

[0161] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A thickener for enhancing oil recovery, characterized in that: The method is composed of the following raw materials in parts by weight: 40-70 parts of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer, 2-6 parts of clay stabilizer, 8-12 parts of emulsifier, 1-3 parts of buffer and 1-2 parts of preservative; The cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer is prepared from the following raw materials in parts by weight: 2.5-25 parts of cage-type octapoly (3-ammonium chloride propyl) silsesquioxane, 10-100 parts of 2-acrylamido-2-methylpropane sulfonic acid, 1000 parts of acrylamide and 0.5-1.9 parts of azobisisobutyramidine hydrochloride; The cage-type octa(3-ammonium chloride propyl)silsesquioxane is prepared from the following raw materials in parts by weight: 0.94-1.88 parts of 3-aminopropyltriethoxysilane and 1.18-1.77 parts of concentrated hydrochloric acid; The preparation of the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer comprises the following steps: Q1, 3-aminopropyltriethoxysilane and concentrated hydrochloric acid are added to anhydrous methanol in sequence, and magnetic stirring is performed until homogeneous to obtain a mixture; Q2, stirring the mixture at a constant speed at room temperature for 10 to 14 days to generate a white microcrystalline precipitate, which is filtered, recrystallized, washed, and dried to obtain a cage-type octameric (3-ammonium chloride propyl) silsesquioxane; Q3, dissolving 2-acrylamido-2-methylpropanesulfonic acid and acrylamide in deionized water, and mechanically stirring until completely dissolved to obtain a monomer solution A; Q4, adding cage-type octa(3-ammonium chloride propyl)silsesquioxane to the monomer solution A obtained in Q3, mechanically stirring to completely disperse it, transferring it to a three-necked flask, passing nitrogen gas to remove dissolved oxygen, and obtaining monomer solution B; Q5, dissolving azobisisobutylamidine hydrochloride in deionized water, ultrasonicating until dissolved, obtaining azobisisobutylamidine hydrochloride solution, placing the monomer solution B in Q4 in a constant temperature water bath, and maintaining mechanical stirring, injecting the azobisisobutylamidine hydrochloride solution into the monomer solution B with a syringe, and copolymerizing under a nitrogen atmosphere, cooling to room temperature after the reaction, filtering to obtain a colloidal product, transferring to anhydrous ethanol to soak and dehydrate for 20 to 24 hours, and vacuum drying to obtain the cage-type octameric (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropanesulfonic acid / acrylamide polymer; The emulsifier is one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate or lecithin, the preservative is glutaraldehyde, and the buffer is disodium hydrogen phosphate-sodium dihydrogen phosphate or disodium hydrogen phosphate-potassium dihydrogen phosphate; The clay stabilizer is one of epichlorohydrin / diethylenetriamine clay stabilizer, 2-chloroethyltrimethylammonium chloride clay stabilizer or potassium chloride clay stabilizer.

2. The thickener for enhancing oil recovery according to claim 1, characterized in that: The volume ratio of 3-aminopropyltriethoxysilane, concentrated hydrochloric acid and anhydrous methanol in step Q1 is 1-2:1-1.5:1000.

3. The thickener for enhancing oil recovery according to claim 2, characterized in that: The total monomer concentration in the monomer solution B in step Q4 is 20-30 wt %, and the mass ratio of cage-type octa(3-ammonium chloride propyl)silsesquioxane:2-acrylamido-2-methylpropanesulfonic acid:acrylamide in the total monomer is 0.25-2.5:1-10:

100.

4. The thickener for enhancing oil recovery according to claim 3, characterized in that: The concentration of the azobisisobutylamidine hydrochloride solution in step Q5 is 0.01-0.05 wt %, and the copolymerization reaction is carried out at 50-70° C. for 2-6 h.

5. The thickener for enhancing oil recovery according to claim 4, characterized in that: The preparation method of the epichlorohydrin / diethylenetriamine clay stabilizer is as follows: Add diethylenetriamine and distilled water into a four-necked flask, stir until completely dissolved and then cool, slowly drop epichlorohydrin in a water bath at a temperature of 25-30°C, and start stirring at the same time. After the dropwise addition is completed, heat to 60-80°C for reaction. After the reaction is completed, collect the product, wash and dry to obtain epichlorohydrin / diethylenetriamine clay stabilizer.

6. The thickener for enhancing oil recovery according to claim 5, characterized in that: The molar ratio of diethylenetriamine to epichlorohydrin is 1 to 3:

1.

7. The method for preparing a thickener for enhancing oil recovery according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, the cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide polymer obtained in Q5 is crushed by a crusher and passed through a 40-mesh powder sieve to obtain cage-type octapoly (3-ammonium chloride propyl) silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder; S2, dissolving 4-7 g / L cage-type octa(3-ammonium chloride propyl)silsesquioxane / 2-acrylamido-2-methylpropane sulfonic acid / acrylamide powder, 0.2-0.6 g / L clay stabilizer, 0.8-1.2 g / L emulsifier, 0.1-0.3 g / L buffer and 0.1-0.2 g / L preservative in water, stirring until the mixture is uniform, thereby obtaining the thickener for enhancing oil recovery.

Citation Information

Patent Citations

  • POSS / PNIPAM nanocomposite with reversible sol-gel transition as well as preparation method and application thereof

    CN108373579A

  • Injectable organosilicone / chitosan nanocomposite hydrogel as well as preparation method and application thereof

    CN108404221A

  • Preparation method of high-strength stretchable conductive self-healing supramolecular hydrogel

    CN109880123A

  • Composite hydrogel as well as preparation method and application thereof in adsorption treatment

    CN112755980A

  • Liquid thickening agent and preparation method thereof

    CN116285937A

Cited By

  • Thickening agent for improving recovery efficiency and preparation method thereof

    CN119331179A