A kind of preparation process of nylon fiber
By preparing hyperbranched polyamide flame retardant and modified carbon nanotubes in nylon fiber to form a cross-linked network, the problem of insufficient flame retardant performance and breaking strength of nylon fiber is solved, and its flame retardant performance and breaking strength are significantly improved. .
Patent Information
- Application Number
- CN202410945972.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-21
AI Technical Summary
Nylon fiber lacks flame retardant properties and has poor breaking strength, which limits its application in high-performance fire-resistant fiber materials.
Hyperbranched polyamide flame retardant was prepared by polymerization reaction of pentaerythritol bisphosphate diphosphoryl (imidazole-4,5-dioic acid chloride), 2,5-diaminopyrazine and triethylamine, and acidified carbon nanotubes were Organic modification, through melt blending spinning technology, modified carbon nanotubes and hyperbranched polyamide flame retardants are added during the spinning process to form a cross-linked network to improve breaking strength and flame retardant properties.
The breaking strength and flame retardant properties of nylon fiber are significantly improved, the modified carbon nanotubes are evenly dispersed, and the hyperbranched polyamide flame retardant effectively captures combustion free radicals, inhibits combustion reactions, and improves the flame retardant properties and char-forming properties of the fiber.
Smart Images

Figure CN118516778B_ABST
Abstract
Description
[0001] This application is a divisional application with application number 2024106290800, application date May 21, 2024, and invention name “A high breaking strength flame-retardant nylon fiber and its preparation process”. Technical Field
[0002] The invention relates to the technical field of nylon fibers, and in particular to a preparation process of nylon fibers. Background Art
[0003] Nylon fiber has good wear resistance and high heat resistance, and is widely used in textiles and other fields. However, nylon fiber has low breaking strength and no flame retardant properties, which is not conducive to the practical application of nylon fiber in high-performance fireproof fiber materials. Hyperbranched polymers have many branching points, molecular chains are not easy to entangle, and have unique physical and chemical properties. They can be used as new functional materials such as flame retardants and toughening agents.
[0004] Carbon nanotubes are a new type of carbon nanomaterial with high mechanical strength and high temperature resistance, which can improve the flame retardancy and mechanical properties of polymer materials. The patent with announcement number CN106929939B discloses the use of carbon nanotubes and melamine to improve the flame retardancy, strength and heat resistance of nylon fibers; however, carbon nanotubes are prone to agglomeration, have poor compatibility with nylon, and have poor reinforcing effects on materials such as nylon fibers. Therefore, the organic modification of the surface of carbon nanotubes is a research difficulty. At the same time, compared with single melamine nitrogen-containing flame retardants, nitrogen-phosphorus flame retardants have better carbonization-promoting properties and flame retardant properties. Summary of the invention
[0005] The technical problem solved by the invention is to solve the problem that nylon fiber has no flame retardant property and poor breaking strength.
[0006] Technical solution:
[0007] A preparation process of nylon fiber with high breaking strength and flame retardancy:
[0008] Step (1) in an ice water bath, add pentaerythritol diphosphate diphosphoryl (imidazole-4,5-diacid chloride), 2,5-diaminopyrazine and triethylamine to N,N-dimethylformamide solvent, react for 20-30 minutes, and then react at a temperature of 20-35° C. for 6-18 hours. After the reaction, add water to the solution for precipitation, filter and wash with water and ethanol in sequence to obtain a hyperbranched polyamide flame retardant.
[0009] Step (2) In an ice-water bath, add acidified carbon nanotubes, pentaerythritol diphosphate diphosphoyl (imidazole-4,5-diacid chloride), and triethylamine to a dichloromethane solvent, react at a temperature of 20-40° C. for 24-48 hours, add water after the reaction, stir, filter, and wash with ethanol to obtain modified carbon nanotubes.
[0010] Step (3) melt-blending and spinning polyamide 6, modified carbon nanotubes and hyperbranched polyamide flame retardant in a spinning machine, controlling the melt-blending temperature to be 235-245° C. and the spinning temperature to be 250-260° C., and then stretching and heat-setting the fiber through a hot roller stretching machine, the stretching multiple is 3-4 times, and the heat-setting temperature is 90-100° C., to obtain nylon fiber with high breaking strength and flame retardancy.
[0011] The masses of 2,5-diaminopyrazine and triethylamine in step (1) are 36-45% and 32-42% of the mass of pentaerythritol bisphosphate diphosphoyl (imidazole-4,5-diacid chloride), respectively.
[0012] Wherein, in step (2), the masses of pentaerythritol diphosphate diphosphoyl (imidazole-4,5-diacyl chloride) and triethylamine are 180-350% and 25-50% of the mass of the acidified carbon nanotubes, respectively.
[0013] The mass of the modified carbon nanotubes and the hyperbranched polyamide flame retardant in step (3) are 0.2-1% and 0.5-5% of the mass of polyamide 6, respectively.
[0014] The preparation process of pentaerythritol diphosphate diphosphoryl (imidazole-4,5-diacyl chloride) comprises the following steps:
[0015] In an ice-water bath, add pentaerythritol bisphosphate diphosphoryl chloride, imidazole-4,5-dicarboxylic acid and triethylamine to a toluene solvent, stir for 10-30 min, react at 30-40°C for 6-12 h, rotary evaporate, wash the product with petroleum ether, add to toluene solvent, add thionyl chloride and catalyst N,N-dimethylformamide, condense and reflux at 75-80°C for 12-18 h, rotary evaporate, wash the product with petroleum ether to obtain pentaerythritol bisphosphate diphosphoryl chloride (imidazole-4,5-diacyl chloride).
[0016] The masses of imidazole-4,5-dicarboxylic acid and triethylamine are 110-125% and 65-72% of the mass of pentaerythritol bisphosphate diphosphoryl chloride, respectively.
[0017] Technical effect: The present invention uses pentaerythritol bisphosphate diphosphoryl chloride, imidazole-4,5-dicarboxylic acid, thionyl chloride, etc. as reactants to prepare pentaerythritol bisphosphate diphosphoryl chloride (imidazole-4,5-diacid chloride). The acyl chloride group thereof reacts with the hydroxyl group on the surface of the acidified carbon nanotube, and then the unreacted acyl chloride group is hydrolyzed in water to generate carboxyl groups to obtain modified carbon nanotubes.
[0018] The invention conducts polymerization reaction on pentaerythritol bisphosphate diphosphoyl (imidazole-4,5-diacid chloride) and 2,5-diaminopyrazine to obtain a novel hyperbranched polyamide flame retardant, which contains amide structural units and has good compatibility with polyamide 6. Meanwhile, after carbon nanotubes are modified with organic functional groups, they also have good compatibility with polyamide 6, improve the agglomeration problem of carbon nanotubes, and have better dispersibility in a polyamide 6 matrix. The three can be well melt-blended and spun. The hyperbranched polyamide has a three-dimensional branched molecular chain, which forms a physical chain entanglement with a polyamide 6 molecular chain to form a cross-linked network, and can improve the fracture performance of nylon fibers. The modified carbon nanotubes are uniformly dispersed in the nylon fibers, play a better reinforcing role, and significantly improve the fracture strength of the nylon fibers.
[0019] Hyperbranched polyamide flame retardant contains the phosphorus-containing flame retardant structure of spirocyclic phosphamide, as well as the nitrogen-containing structure of imidazole and pyrazine. As a nitrogen-phosphorus flame retardant, it can test phosphorus-containing free radicals during combustion, capture combustion chain free radicals, hinder the combustion reaction, and produce nitrogen-containing non-combustible gases such as nitrogen. It improves the carbonization and residual carbon content of nylon fibers and their textiles, promotes the formation of an expanded carbon layer, has the function of isolating oxygen and suppressing smoke, and has a synergistic flame retardant effect with carbon nanotubes, showing excellent flame retardant properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a reaction route for preparing pentaerythritol diphosphate diphosphoryl (imidazole-4,5-diacyl chloride).
[0021] Figure 2 It is a reaction route for preparing hyperbranched polyamide flame retardants. DETAILED DESCRIPTION
[0022] In order to further understand the present invention, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The CAS number of pentaerythritol bisphosphate diphosphoryl chloride in the embodiment of the present invention is 714-87-4. The CAS number of imidazole-4,5-dicarboxylic acid is 570-22-9. The CAS number of thionyl chloride is 7719-09-7. The CAS number of 2,5-diaminopyrazine is 768386-37-4.
[0024] Add carbon nanotubes to a solution of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3, condense and reflux at 140° C. for 1 h, filter, and wash with water to obtain acidified carbon nanotubes.
[0025] Example 1
[0026] (1) In an ice-water bath, add 1 g of pentaerythritol bisphosphate diphosphoryl chloride, 1.25 g of imidazole-4,5-dicarboxylic acid, and 0.65 g of triethylamine to a toluene solvent, stir for 10 min, react at 35°C for 6 h, rotary evaporate, wash the product with petroleum ether, add to toluene solvent, add 10 g of thionyl chloride and 0.52 g of catalyst N,N-dimethylformamide, react under condensation reflux at 75°C for 18 h, rotary evaporate, wash the product with petroleum ether to obtain pentaerythritol bisphosphate diphosphoryl chloride (imidazole-4,5-diacyl chloride).
[0027] (2) In an ice-water bath, 2 g of pentaerythritol diphosphate diphosphoyl (imidazole-4,5-diacid chloride), 0.72 g of 2,5-diaminopyrazine, and 0.8 g of triethylamine were added to 20 mL of N,N-dimethylformamide solvent, and the mixture was reacted for 30 min and then at 30 °C for 6 h. After the reaction, water was added to the solution for precipitation. After filtering, the mixture was washed with water and ethanol in turn to obtain a hyperbranched polyamide flame retardant.
[0028] (3) In an ice-water bath, add 0.2 g of acidified carbon nanotubes, 0.36 g of pentaerythritol diphosphite diphosphoyl (imidazole-4,5-diacid chloride), and 0.1 g of triethylamine to 8 mL of dichloromethane solvent, and react at 40 °C for 24 h. After the reaction, add water, stir, filter, and wash with ethanol to obtain modified carbon nanotubes.
[0029] (4) 100 g of polyamide 6, 0.2 g of modified carbon nanotubes, and 0.5 g of hyperbranched polyamide flame retardant were melt-blended and spun in a spinning machine, the melt-blending temperature was controlled to be 235°C, the spinning temperature was controlled to be 250°C, and then the fiber was stretched and heat-set by a hot roller stretching machine, the stretching multiple was 4 times, and the heat-setting temperature was 90°C, to obtain a nylon fiber with high breaking strength and flame retardancy.
[0030] Example 2
[0031] (1) In an ice-water bath, add 1 g of pentaerythritol bisphosphate diphosphoryl chloride, 1.25 g of imidazole-4,5-dicarboxylic acid, and 0.68 g of triethylamine to a toluene solvent, stir for 30 min, react at 30°C for 10 h, rotary evaporate, wash the product with petroleum ether, add to toluene solvent, add 12 g of thionyl chloride and 0.45 g of catalyst N,N-dimethylformamide, react under condensation reflux at 75°C for 18 h, rotary evaporate, wash the product with petroleum ether to obtain pentaerythritol bisphosphate diphosphoryl chloride (imidazole-4,5-diacyl chloride).
[0032] (2) In an ice water bath, 2 g of pentaerythritol bisphosphate diphosphoyl (imidazole-4,5-diacid chloride), 0.72 g of 2,5-diaminopyrazine, and 0.84 g of triethylamine were added to 20 mL of N,N-dimethylformamide solvent, and the mixture was reacted for 20 min, and then reacted at 35 °C for 6 h. After the reaction, water was added to the solution for precipitation. After filtering, the mixture was washed with water and ethanol in turn to obtain a hyperbranched polyamide flame retardant.
[0033] (3) In an ice-water bath, add 0.2 g of acidified carbon nanotubes, 0.56 g of pentaerythritol diphosphate diphosphoyl (imidazole-4,5-diacid chloride), and 0.05 g of triethylamine to 8 mL of dichloromethane solvent, and react at 40 °C for 24 h. After the reaction, add water, stir, filter, and wash with ethanol to obtain modified carbon nanotubes.
[0034] (4) 100 g of polyamide 6, 0.6 g of modified carbon nanotubes, and 2.5 g of hyperbranched polyamide flame retardant were melt-blended and spun in a spinning machine, the melt-blending temperature was controlled to be 245°C, and the spinning temperature was controlled to be 260°C. The fiber was then stretched and heat-set by a hot roller stretching machine, the stretching multiple was 3 times, and the heat-setting temperature was 100°C, to obtain a nylon fiber with high breaking strength and flame retardancy.
[0035] Example 3
[0036] (1) In an ice-water bath, add 1 g of pentaerythritol bisphosphate diphosphoryl chloride, 1.1 g of imidazole-4,5-dicarboxylic acid, and 0.72 g of triethylamine to a toluene solvent, stir for 30 min, react at 40°C for 12 h, rotary evaporate, wash the product with petroleum ether, add to toluene solvent, add 12 g of thionyl chloride and 0.52 g of catalyst N,N-dimethylformamide, react under condensation reflux at 80°C for 12 h, rotary evaporate, wash the product with petroleum ether to obtain pentaerythritol bisphosphate diphosphoryl chloride (imidazole-4,5-diacyl chloride).
[0037] (2) In an ice-water bath, 2 g of pentaerythritol bisphosphate diphosphoyl (imidazole-4,5-diacid chloride), 0.9 g of 2,5-diaminopyrazine, and 0.64 g of triethylamine were added to 40 mL of N,N-dimethylformamide solvent, and the mixture was reacted for 30 min, and then reacted at 20 °C for 18 h. After the reaction, water was added to the solution for precipitation. After filtering, the mixture was washed with water and ethanol in turn to obtain a hyperbranched polyamide flame retardant.
[0038] (3) In an ice-water bath, 0.2 g of acidified carbon nanotubes, 0.36 g of pentaerythritol diphosphite diphosphoyl (imidazole-4,5-diacid chloride), and 0.1 g of triethylamine were added to 10 mL of dichloromethane solvent, and the mixture was reacted at 40 °C for 36 h. After the reaction, water was added, the mixture was stirred, filtered, and washed with ethanol to obtain modified carbon nanotubes.
[0039] (4) 100 g of polyamide 6, 1 g of modified carbon nanotubes, and 5 g of hyperbranched polyamide flame retardant were melt-blended and spun in a spinning machine, the melt-blending temperature was controlled to be 235°C, and the spinning temperature was controlled to be 255°C. The fiber was then stretched and heat-set by a hot roller stretching machine, the stretching multiple was 4 times, and the heat-setting temperature was 90°C, to obtain a nylon fiber with high breaking strength and flame retardancy.
[0040] The main difference between Comparative Example 1 and Example 1 is that no hyperbranched polyamide flame retardant and modified carbon nanotubes are added.
[0041] The polyamide 6 is melt-spun in a spinning machine at a spinning temperature of 250°C, and then the fiber is stretched and heat-set by a hot roller stretching machine at a stretching multiple of 4 times and a heat-setting temperature of 90°C to obtain nylon fiber.
[0042] The main difference between Comparative Example 2 and Example 1 is that no hyperbranched polyamide flame retardant is added.
[0043] 100g polyamide 6 and 0.2g modified carbon nanotubes are melt-blended and spun in a spinning machine, the melt-blending temperature is controlled to be 235°C, the spinning temperature is controlled to be 250°C, and then the fiber is stretched and heat-set by a hot roller stretching machine, the stretching multiple is 4 times, and the heat-setting temperature is 90°C, to obtain nylon fiber with high breaking strength and flame retardancy.
[0044] The main difference between Comparative Example 3 and Example 1 is that no modified carbon nanotubes are added.
[0045] 100g of polyamide 6 and 0.5g of hyperbranched polyamide flame retardant are melt-blended and spun in a spinning machine, the melt-blending temperature is controlled to be 235°C, the spinning temperature is controlled to be 250°C, and then the fiber is stretched and heat-set by a hot roller stretching machine, the stretching multiple is 4 times, and the heat-setting temperature is 90°C, to obtain nylon fiber with high breaking strength and flame retardancy.
[0046] Comparative Example 4 The main difference between Comparative Example 3 and Example 1 is that carbon nanotubes are used instead of modified carbon nanotubes.
[0047] 100g polyamide 6, 0.2g carbon nanotubes and 0.5g hyperbranched polyamide flame retardant are melt-blended and spun in a spinning machine, the melt-blending temperature is controlled to be 235°C, the spinning temperature is controlled to be 250°C, and then the fiber is stretched and heat-set by a hot roller stretching machine, the stretching multiple is 4 times, and the heat-setting temperature is 90°C, to obtain nylon fiber with high breaking strength and flame retardancy.
[0048] The breaking performance of nylon fiber was tested by electronic single fiber strength test, with a clamping distance of 20 mm and a tensile speed of 20 mm / min. The linear density of nylon fiber is 1.67 dtex.
[0049]
[0050] The carbon residue of nylon fiber was measured in a thermogravimetric analyzer in a nitrogen atmosphere with a heating rate of 10°C and a maximum test temperature of 800°C. The nylon fiber was woven into fabrics and the limiting oxygen index was tested according to the method of GB / T5454-1997. The larger the limiting oxygen index, the better the flame retardant performance.
[0051]
[0052] The modified carbon nanotubes and hyperbranched polyamide flame retardant added in Examples 1-3 of the present invention, the hyperbranched polyamide flame retardant contains amide structural units, and has good compatibility with polyamide 6. At the same time, after the carbon nanotubes are modified with organic functional groups, they are also very compatible with polyamide 6, which improves the agglomeration problem of the carbon nanotubes and has better dispersibility in the polyamide 6 matrix. The three can be well melt-blended and spun. The hyperbranched polyamide has a three-dimensional branched molecular chain, which forms a physical chain entanglement with the polyamide 6 molecular chain to form a cross-linked network, which can improve the breaking performance of the nylon fiber, and the modified carbon nanotubes are evenly dispersed in the nylon fiber, which plays a better reinforcing role and significantly improves the breaking strength of the nylon fiber.
[0053] Hyperbranched polyamide flame retardant contains the phosphorus-containing flame retardant structure of spirocyclic phosphamide, as well as the nitrogen-containing structure of imidazole and pyrazine. As a nitrogen-phosphorus flame retardant, it can test phosphorus-containing free radicals during combustion, capture combustion chain free radicals, hinder the combustion reaction, and produce nitrogen-containing non-combustible gases such as nitrogen. It improves the carbonization and residual carbon content of nylon fibers and their textiles, promotes the formation of an expanded carbon layer, has the function of isolating oxygen and suppressing smoke, and has a synergistic flame retardant effect with carbon nanotubes, showing excellent flame retardant properties.
[0054] Comparative Example 1 does not add hyperbranched polyamide flame retardant and modified carbon nanotubes. The breaking strength and limiting oxygen index are the lowest.
[0055] In Comparative Example 2, modified carbon nanotubes were added. Compared with Comparative Example 1, the breaking properties of nylon fibers were significantly improved. However, no hyperbranched polyamide flame retardant was added, and the breaking strength and limiting oxygen index were lower than those in Example 1.
[0056] In comparative example 3, the addition of hyperbranched polyamide flame retardant significantly improves the limiting oxygen index and improves the breaking strength to a certain extent. However, without the addition of modified carbon nanotubes, there is no reinforcing effect and no synergistic flame retardant effect, and the breaking strength and limiting oxygen index are lower than those in example 1.
[0057] Comparative Example 4 uses carbon nanotubes instead of modified carbon nanotubes. The carbon nanotubes have not been organically modified, have poor compatibility with polyamide 6, are easily agglomerated in nylon fibers, and do not exert the reinforcing effect of the carbon nanotubes well, and have a lower breaking strength than Example 1.
[0058] It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the protection scope of the claims of the present invention.
Claims
1. A process for preparing nylon fiber, characterized in that: The steps include: Step (1) adding pentaerythritol bisphosphate diphosphoyl (imidazole-4,5-diacid chloride), 2,5-diaminopyrazine and triethylamine to N,N-dimethylformamide solvent in an ice-water bath to react and obtain a hyperbranched polyamide flame retardant; Step (2) adding acidified carbon nanotubes, pentaerythritol diphosphate diphosphoyl (imidazole-4,5-diacid chloride) and triethylamine to a dichloromethane solvent in an ice-water bath to react and obtain modified carbon nanotubes; Step (3) melt-blending and spinning polyamide 6, modified carbon nanotubes and hyperbranched polyamide flame retardant in a spinning machine, controlling the melt-blending temperature to be 235-245° C. and the spinning temperature to be 250-260° C., and then stretching and heat-setting the fiber through a hot roller stretching machine, the stretching multiple is 3-4 times, and the heat-setting temperature is 90-100° C., to obtain a nylon fiber with high breaking strength and flame retardancy; In the step (1), the mass of 2,5-diaminopyrazine and triethylamine is 36-45% and 32-42% of the mass of pentaerythritol diphosphate diphosphoyl (imidazole-4,5-diacid chloride), respectively; the reaction in the step (1) is first carried out in an ice water bath for 20-30 minutes, and then at a temperature of 20-35° C. for 6-18 hours; In the step (2), the masses of pentaerythritol diphosphate diphosphoyl (imidazole-4,5-diacid chloride) and triethylamine are 180-350% and 25-50% of the mass of the acidified carbon nanotubes, respectively; and the reaction in the step (2) is carried out at a temperature of 20-40° C. for 24-48 hours.
2. The process for preparing nylon fiber according to claim 1, characterized in that: In the step (3), the mass of the modified carbon nanotubes and the hyperbranched polyamide flame retardant are 0.2-1% and 0.5-5% of the mass of polyamide 6, respectively.
3. According to the preparation process of nylon fiber according to claim 2, the preparation process of pentaerythritol bisphosphate diphosphoyl (imidazole-4,5-diacid chloride) comprises the following steps: In an ice-water bath, add pentaerythritol bisphosphate diphosphoryl chloride, imidazole-4,5-dicarboxylic acid, and triethylamine to a toluene solvent, stir for 10-30 minutes, react at a temperature of 30-40°C for 6-12 hours, and rotary evaporate. The product is washed with petroleum ether and then added to a toluene solvent. Add thionyl chloride and a catalyst N,N-dimethylformamide, and condense and reflux at a temperature of 75-80°C for 12-18 hours to obtain pentaerythritol bisphosphate diphosphoryl chloride (imidazole-4,5-diacyl chloride). The masses of the imidazole-4,5-dicarboxylic acid and triethylamine are 110-125% and 65-72% of the mass of pentaerythritol bisphosphate diphosphoryl chloride, respectively.
Citation Information
Patent Citations
A flame-retardant nylon fiber and its preparation method
CN106929939B
Synthesis and applications of hyperbranched polyamide type TPO modifier
CN107586384A
Modified polyamide PA flame-retardant material and preparation method thereof
CN116574369A
Flame retardancy treatment of polymeric material
GB9917592D0
Reactive polyurethane flame retardant, preparation method therefor and use thereof
WO2021155715A1