A preparation method of P-MoC co-catalyst, a preparation method of photocatalyst and application thereof
The nano-P-MoC cocatalyst was prepared by a one-step reaction method and modified with Zn0.5Cd0.5S and g-C3N4, which solved the problems of MoC material particle aggregation and poor conductivity, improved the stability of the photocatalyst and the hydrogen evolution reaction efficiency, and achieved Efficient photocatalytic hydrogen production.
Patent Information
- Application Number
- CN202410985921.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-23
AI Technical Summary
Existing MoC materials are synthesized by direct high-temperature pyrolysis of precursors, which leads to particle aggregation, reduced specific surface area and exposed active sites, poor conductivity, high hydrogen evolution overpotential, and difficult desorption of H.
A one-step reaction method is used to use metal organic framework ZIF-8 as the template, and phosphomolybdic acid containing P element as the molybdenum source. Through high-temperature carbonization and removal of the ZIF-8 template, the nano-P-MoC cocatalyst is obtained, and combined with Zn0.5Cd0 .5S and g-C3N4 modification improves the efficiency of photogenerated carrier separation and hydrogen evolution reaction.
The specific surface area and conductivity of the P-MoC cocatalyst are increased, the hydrogen evolution overpotential is reduced, the stability and surface reaction efficiency of the photocatalyst are enhanced, and the activity of photocatalytic hydrogen production is significantly improved.
Smart Images

Figure CN118527168B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material preparation, and in particular relates to a preparation method of a P-MoC co-catalyst, a preparation method of a photocatalyst and applications thereof. Background Art
[0002] The burning of fossil pigments can lead to problems such as air pollution, water pollution and global warming. Therefore, it is imperative to develop clean and environmentally friendly renewable energy. Solar energy has the advantages of being renewable, rich in energy storage and low in price. Hydrogen is clean, non-toxic and has high energy density, making it the best choice to replace fossil energy. Therefore, solar photocatalytic hydrogen production is one of the most promising solutions to solve environmental pollution and develop sustainable clean energy.
[0003] Since 1972, Fujishima et al. have used TiO 2 Photoelectric water splitting to produce hydrogen (H 2 ) and oxygen (O 2 ) has been widely used in the production of H by photocatalytic water splitting. 2 Rapid development. Due to the fact that the photogenerated carriers of current photocatalysts are prone to recombination and the high overpotential of the surface hydrogen evolution reaction, the photocatalytic hydrogen evolution activity of current semiconductor photocatalysts is not ideal. Studies have found that the modification of high-efficiency co-catalysts can effectively improve the stability of photocatalysts, the separation efficiency of photogenerated charges and the rate of surface hydrogen evolution reaction, and is an effective method to improve the activity of semiconductor photocatalytic hydrogen evolution reaction.
[0004] The precious metal Pt is an ideal co-catalyst in the photocatalytic hydrogen production system, but its high price and small reserves severely limit its widespread application. Non-precious metals are abundant in the earth's crust, and it is of great significance to develop efficient non-precious metal co-catalysts that can replace the precious metal Pt. MoC materials have an electronic structure similar to Pt, and have excellent stability and conductivity. They are considered to be ideal materials to replace Pt co-catalysts. At present, most MoC materials are synthesized by direct high-temperature pyrolysis of precursors. The high-temperature process will cause particle aggregation, thereby reducing its specific surface area and reducing the exposed active sites. At the same time, MoC materials have poor conductivity, high hydrogen evolution overpotential, and difficult H desorption. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the fact that most MoC materials in the prior art are directly synthesized by high-temperature pyrolysis of precursors. The high-temperature process will cause particle aggregation, thereby reducing its specific surface area and reducing the defects of exposed active sites, thereby providing a method for preparing a P-MoC co-catalyst.
[0006] The invention also provides a preparation method and application of a photocatalyst.
[0007] In order to solve the above technical problems, the present invention provides a method for preparing a P-MoC co-catalyst, comprising the following steps:
[0008] S1, mixing and stirring zinc nitrate hexahydrate, phosphomolybdic acid, polyethylpyrrolidone and methanol to obtain solution A; the molar ratio of zinc element to molybdenum element is 1:(0.9-1.2);
[0009] S2, dispersing dimethylimidazole in methanol and stirring to obtain solution B; the molar ratio of the zinc element to the dimethylimidazole is 1:(10-13);
[0010] S3, mixing solution A and solution B, stirring, filtering, washing, and drying to obtain a P-MoC precursor;
[0011] S4, the P-MoC precursor is calcined in an inert gas atmosphere to obtain a P-MoC co-catalyst.
[0012] As a preferred embodiment, in step S3, the stirring time is 20-30 h, and the drying condition is vacuum drying at 50-70 °C for 8-12 h.
[0013] As a preferred solution, in step S3, methanol and ethanol are used sequentially for washing.
[0014] As a preferred solution, in step S4, during the calcination process, the heating rate is 3-8°C / min, the calcination temperature is 750-850°C, and the calcination time is 1.5-2.5 h.
[0015] The present invention also provides a P-MoC / Zn 0.5 Cd 0.5 The preparation method of S photocatalyst comprises the following steps:
[0016] Weigh Zn 0.5 Cd 0.5 The S catalyst was dispersed in deionized water, and the P-MoC cocatalyst was added, stirred, centrifuged, washed, and dried to obtain P-MoC / Zn 0.5 Cd 0.5 S;
[0017] The Zn 0.5 Cd 0.5 The mass ratio of the S catalyst to the P-MoC co-catalyst is 1:(0.05-0.2).
[0018] As a preferred solution, the stirring time is 10-14 h, the drying temperature is 60-100 °C, and the drying time is 3-5 h.
[0019] The present invention also provides a P-MoC / Zn prepared by the above preparation method.0.5 Cd 0.5 Application of S photocatalyst in photocatalytic hydrogen production.
[0020] The present invention also provides a P-MoC / gC 3 N 4 The method for preparing a photocatalyst comprises the following steps:
[0021] Weigh gC 3 N 4 The catalyst was dispersed in deionized water, and the above-mentioned P-MoC co-catalyst was added, stirred, centrifuged, washed, and dried to obtain P-MoC / gC 3 N 4 ;
[0022] The gC 3 N 4 The mass ratio of the catalyst to the P-MoC co-catalyst is 1:(0.05-0.2).
[0023] As a preferred solution, the stirring time is 10-14 h, the drying temperature is 60-100 °C, and the drying time is 3-5 h.
[0024] The present invention also provides a P-MoC / gC prepared by the above preparation method. 3 N 4 Application of photocatalysts in photocatalytic hydrogen production.
[0025] The technical solution of the present invention has the following advantages:
[0026] 1. The preparation method of the P-MoC co-catalyst provided by the present invention uses the metal organic framework ZIF-8 as a template material and phosphomolybdic acid containing the P element as a molybdenum source. The ZIF-8 organic metal framework containing phosphomolybdic acid is first prepared by a one-step reaction method, and further by high-temperature carbonization, while removing the ZIF-8 template, the P-containing functional group obtained after the decomposition of the phosphomolybdic acid reacts with the molybdenum-containing functional group, thereby obtaining a nano P-MoC co-catalyst.
[0027] 2. The preparation method of the photocatalyst provided by the present invention is to use P-MoC for Zn 0.5 Cd 0.5 S and gC 3 N 4 The modification of the photocatalyst achieves efficient separation of photogenerated charge carriers and improves the efficiency of surface hydrogen evolution reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 is the XRD pattern of P-MoC prepared in Example 1, Example 2 and Example 3 of the present invention;
[0030] Figure 2 is an X-ray photoelectron spectrum of the P-MoC prepared in Example 1 of the present invention; (a) is an overall X-ray photoelectron spectrum of the P-MoC prepared in Example 1 of the present invention, (b) is an X-ray photoelectron spectrum of the P element in the P-MoC prepared in Example 1 of the present invention;
[0031] Figure 3 is the SEM spectrum of P-MoC prepared in Example 1 of the present invention;
[0032] Figure 4 is the TEM spectrum of P-MoC prepared in Example 1 of the present invention;
[0033] Figure 5 1 is a linear sweep voltammogram of the P-MoC co-catalyst prepared in Example 1 of the present invention and the MoC co-catalyst prepared in Comparative Example 1;
[0034] Figure 6 1 is an AC impedance spectrum of the P-MoC co-catalyst prepared in Example 1 of the present invention and the MoC co-catalyst prepared in Comparative Example 1;
[0035] Figure 7 The photocatalytic hydrogen evolution diagrams of Experimental Examples 1 and 2;
[0036] Figure 8 This is the photocatalytic hydrogen evolution diagram of Experimental Example 3. DETAILED DESCRIPTION
[0037] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0038] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially. Example 1
[0039] Weigh 2.97 g of zinc nitrate hexahydrate (Zn(NO 3 ) 2 6H 2 O) and 1.52 g phosphomolybdic acid (H 5 PMo 12 O 41 ) was dispersed in 180 ml of methanol, ultrasonicated for 30 min, 1.0 g of polyethylpyrrolidone PVP (Mw=58000) was weighed and added to the above solution, stirred for 30 min to obtain solution A; 9.85 g of dimethylimidazole (C 4 H 6 N 2 ) was dispersed in 180 ml of methanol and stirred for 30 min to obtain solution B;
[0040] Solution A was quickly dropped into solution B, stirred at room temperature (25 °C) for 24 h, filtered, washed with methanol and ethanol respectively, and dried under vacuum at 60 °C for 10 h to obtain a P-MoC precursor;
[0041] The prepared P-MoC precursor was placed in a tubular furnace, and under an argon protective atmosphere, the heating rate was 5 ℃ / min, the calcination temperature was 850 ℃, and the calcination time was 2 h to obtain a P-MoC co-catalyst. Example 2
[0042] Weigh 2.97g zinc nitrate hexahydrate and 1.38g phosphomolybdic acid and disperse them in 180ml methanol. Ultrasonicate for 30min. Weigh 1.0g polyethylpyrrolidone PVP (Mw=58000) and add it to the above solution. Stir for 30min to obtain solution A. Weigh 8.21g dimethylimidazole (C 4 H 6 N 2 ) was dispersed in 180 ml methanol and stirred for 30 min to obtain solution B; solution A was quickly dropped into solution B, stirred at room temperature (25°C) for 20 h, filtered, washed with methanol and ethanol respectively, and vacuum dried at 50°C for 12 h to obtain P-MoC precursor;
[0043] The prepared P-MoC precursor was placed in a tubular furnace, and under an argon atmosphere, the heating rate was 3 °C / min, the calcination temperature was 800 °C, and the calcination time was 1.5 h to obtain a P-MoC co-catalyst. Example 3
[0044] Weigh 2.97g zinc nitrate hexahydrate and 1.84g phosphomolybdic acid and disperse them in 180ml methanol. Ultrasonicate for 30min. Weigh 1.0g polyethylpyrrolidone PVP (Mw=58000) and add it to the above solution. Stir for 30min to obtain solution A. Weigh 10.67g dimethylimidazole (C 4 H 6 N 2 ) was dispersed in 180 ml methanol and stirred for 30 min to obtain solution B; solution A was quickly dropped into solution B, stirred at room temperature (25°C) for 30 h, filtered, washed with methanol and ethanol respectively, and vacuum dried at 70°C for 8 h to obtain P-MoC precursor;
[0045] The prepared P-MoC precursor was placed in a tubular furnace, and under an argon atmosphere, the heating rate was 8 °C / min, the calcination temperature was 750 °C, and the calcination time was 2.5 h to obtain a P-MoC co-catalyst.
[0046] Comparative Example 1
[0047] Weigh 2.97 g zinc nitrate hexahydrate (Zn(NO 3 ) 2 6H 2 O) and 1.77 g ammonium molybdate tetrahydrate (H 32 Mo 7 N 6 O 28 ) was dispersed in 180 ml methanol, ultrasonicated for 30 min, 1.0 g polyethylpyrrolidone PVP (Mw=58000) was weighed and added to the above solution, stirred for 30 min to obtain solution A; 9.85 g dimethylimidazole (C 4 H 6 N 2 ) was dispersed in 180 ml of methanol and stirred for 30 min to obtain solution B.
[0048] Solution A was quickly dropped into solution B, stirred at room temperature (25 °C) for 24 h, filtered, washed with methanol and ethanol respectively, and dried under vacuum at 60 °C for 10 h to obtain a MoC precursor;
[0049] The prepared MoC precursor was placed in a tube furnace, and under an Ar protective atmosphere, the temperature was raised to 850 °C at 5 °C / min for 2 h to obtain a MoC co-catalyst.
[0050] Figure 1 is the XRD pattern of P-MoC prepared in Example 1, Example 2 and Example 3, as shown Figure 1As shown, the XRD diffraction peaks correspond to the MoC standard card (JCPDS No.89-2868), which indicates that P-MoC can be synthesized in the range of 750 ℃-850 ℃, and the incorporation of P does not change the crystal structure of MoC.
[0051] Figure 2 (a) is the overall X-ray photoelectron spectrum of P-MoC prepared in Example 1 of the present invention, Figure 2 (b) is an X-ray photoelectron spectrum of the P element in the P-MoC prepared in Example 1 of the present invention; Figure 2 (a) It can be seen that the P-MoC sample contains P element. The valence state of P element is analyzed by high-resolution XPS spectrum, such as Figure 2 As shown in (b), the characteristic peak at 129.5 ev corresponds to the C-Mo-P bond, and the characteristic peak at 133.7 ev corresponds to the PO bond, which proves the successful preparation of P-doped MoC.
[0052] Figure 3 , Figure 4 The SEM and TEM images of the P-MoC sample prepared in Example 1 respectively show that the prepared P-MoC is nanoparticles with a diameter of 30-50 nm.
[0053] Figure 5 The linear scanning voltammograms of the P-MoC co-catalyst prepared in Example 1 and the MoC co-catalyst prepared in Comparative Example 1 are shown. The electrocatalytic hydrogen evolution performance of P-MoC and MoC is compared by electrochemical analysis. It can be seen from the figure that at the same current density, P-MoC has a smaller hydrogen evolution overpotential. The introduction of P can effectively reduce the hydrogen evolution overpotential of MoC, thereby facilitating the hydrogen evolution reaction.
[0054] Figure 6 The AC impedance spectra of the P-MoC co-catalyst prepared in Example 1 and the MoC co-catalyst prepared in Comparative Example 1 are shown. The impedance of P-MoC was tested under the same conditions. It can be seen from the figure that the introduction of P reduces the impedance of MoC, so that electrons can be transferred to the MoC surface more quickly for hydrogen evolution reaction. Example 4
[0055] Weigh 0.1999 g of cadmium acetate dihydrate (C 4 H 10 CdO 6 ) and 0.1647 g zinc acetate dihydrate (C 4 H 10 ZnO 6) was dispersed in 12.5 ml of water, and the pH was adjusted to 7.3 with 0.2 mol / L sodium hydroxide solution. Under stirring, 0.3 mol / L sodium sulfide nonahydrate (Na 2 S.9H 2 O) 7.5 ml solution, continue stirring for 20 min to completely dissolve it, transfer the above solution to a polytetrafluoroethylene hydrothermal reactor, react in an oven at 160 ° C for 4 h, and wash with distilled water to obtain a yellow precipitate Zn 0.5 Cd 0.5 S is denoted as ZCS.
[0056] Weigh 0.181 g Zn 0.5 Cd 0.5 S was dispersed in 30 ml of deionized water, 0.00905 g of the P-MoC nanoparticles prepared in Example 1 were weighed, stirred for 12 h at room temperature (25 °C), washed three times with deionized water, and dried at 80 °C for 4 h to obtain 5% P-MoC / ZCS. Example 5
[0057] Weigh 0.1999 g of cadmium acetate dihydrate (C 4 H 10 CdO 6 ) and 0.1647 g zinc acetate dihydrate (C 4 H 10 ZnO 6 ) was dispersed in 12.5 ml of water, and the pH was adjusted to 7.3 with 0.2 mol / L sodium hydroxide solution. Under stirring, 0.3 mol / L sodium sulfide nonahydrate (Na 2 S.9H 2 O) 7.5 ml solution, continue stirring for 20 min to completely dissolve it, transfer the above solution to a polytetrafluoroethylene hydrothermal reactor, react in an oven at 160 ° C for 4 h, and wash with distilled water to obtain a yellow precipitate Zn 0.5 Cd 0.5 S is denoted as ZCS.
[0058] Weigh 0.181g Zn 0.5 Cd 0.5 S was dispersed in 30 ml of deionized water, 0.0181 g of the P-MoC nanoparticles prepared in Example 1 were weighed, stirred for 10 h at room temperature (25 °C), washed three times with deionized water, and dried at 60 °C for 5 h to obtain 10% P-MoC / ZCS. Example 6
[0059] Weigh 0.1999 g of cadmium acetate dihydrate (C 4 H 10CdO 6 ) and 0.1647 g zinc acetate dihydrate (C 4 H 10 ZnO 6 ) was dispersed in 12.5 ml of water, and the pH was adjusted to 7.3 with 0.2 mol / L sodium hydroxide solution. Under stirring, 0.3 mol / L sodium sulfide nonahydrate (Na 2 S.9H 2 O) 7.5 ml solution, continue stirring for 20 min to completely dissolve it, transfer the above solution to a polytetrafluoroethylene hydrothermal reactor, react in an oven at 160 ° C for 4 h, and wash with distilled water to obtain a yellow precipitate Zn 0.5 Cd 0.5 S is denoted as ZCS.
[0060] Weigh 0.181g Zn 0.5 Cd 0.5 S was dispersed in 30 ml of deionized water, 0.0272 g of the P-MoC nanoparticles prepared in Example 1 were weighed, stirred at room temperature (25 °C) for 14 h, washed three times with deionized water, and dried at 100 °C for 3 h to obtain 15% P-MoC / ZCS. Example 7
[0061] Weigh 0.1999 g of cadmium acetate dihydrate (C 4 H 10 CdO 6 ) and 0.1647 g zinc acetate dihydrate (C 4 H 10 ZnO 6 ) was dispersed in 12.5 ml of water, and the pH was adjusted to 7.3 with 0.2 mol / L sodium hydroxide solution. Under stirring, 0.3 mol / L sodium sulfide nonahydrate (Na 2 S.9H 2 O) 7.5 ml solution, continue stirring for 20 min to completely dissolve it, transfer the above solution to a polytetrafluoroethylene hydrothermal reactor, react in an oven at 160 ° C for 4 h, and wash with distilled water to obtain a yellow precipitate Zn 0.5 Cd 0.5 S is denoted as ZCS.
[0062] Weigh 0.181g Zn 0.5 Cd 0.5 S was dispersed in 30 ml of deionized water, 0.0363 g of the P-MoC nanoparticles prepared in Example 1 were weighed, stirred for 12 h at room temperature (25 °C), washed three times with deionized water, and dried at 80 °C for 4 h to obtain 20% P-MoC / ZCS. Example 8
[0063] Weigh 40 g urea (CH 4 N 2 O) was placed in a crucible and heated to 550 °C in a muffle furnace at 20 °C / min for 3 h to obtain gC 3 N 4 C 3 N 4 .
[0064] Weigh 0.181 g of C 3 N 4 Dispersed in 30 ml of deionized water, 0.00905 g of the P-MoC nanoparticles prepared in Example 1 were weighed, stirred at room temperature (25 °C) for 12 h, washed three times with deionized water, and dried at 80 °C for 4 h to obtain 5% P-MoC / C 3 N 4 . Example 9
[0065] Weigh 40 g urea (CH 4 N 2 O) was placed in a crucible and heated to 550 °C in a muffle furnace at 20 °C / min for 3 h to obtain gC 3 N 4 C 3 N 4 .
[0066] Weigh 0.181 g of C 3 N 4 Dispersed in 30 ml of deionized water, 0.0181 g of the P-MoC nanoparticles prepared in Example 1 were weighed, stirred at room temperature (25 °C) for 10 h, washed three times with deionized water, and dried at 60 °C for 5 h to obtain 10% P-MoC / C 3 N 4 . Example 10
[0067] Weigh 40 g urea (CH 4 N 2 O) was placed in a crucible and heated to 550 °C in a muffle furnace at 20 °C / min for 3 h to obtain gC 3 N 4 C 3 N 4 .
[0068] Weigh 0.181 g of C 3 N 4Dispersed in 30 ml of deionized water, 0.0272 g of the P-MoC nanoparticles prepared in Example 1 were weighed, stirred at room temperature (25 °C) for 14 h, washed three times with deionized water, and dried at 100 °C for 3 h to obtain 15% P-MoC / C 3 N 4 . Embodiment 11
[0069] Weigh 40 g urea (CH 4 N 2 O) was placed in a crucible and heated to 550 °C in a muffle furnace at 20 °C / min for 3 h to obtain gC 3 N 4 C 3 N 4 .
[0070] Weigh 0.181 g of C 3 N 4 Dispersed in 30 ml of deionized water, 0.0363 g of the P-MoC nanoparticles prepared in Example 1 were weighed, stirred at room temperature (25 °C) for 12 h, washed three times with deionized water, and dried at 80 °C for 4 h to obtain 20% P-MoC / C 3 N 4 .
[0071] Experimental Example 1
[0072] 15 mg of the P-MoC nanoparticles prepared in Example 1, the ZCS prepared in Example 4, the 5% P-MoC / ZCS prepared in Example 4, the 10% P-MoC / ZCS prepared in Example 5, the 15% P-MoC / ZCS prepared in Example 6, and the 20% P-MoC / ZCS prepared in Example 7 were respectively dispersed in 30 ml of lactic acid aqueous solution and placed in a quartz reactor. The reaction temperature was kept constant at 15° C. A xenon lamp was used as the light source for single-side irradiation (300 W, Perfect Light, with a 400 nm cutoff filter). Ar was used as the carrier gas, and the hydrogen production performance was analyzed every 1 h by a gas chromatograph.
[0073] Experimental Example 2
[0074] 15 mg of the ZCS photocatalyst prepared in Example 4, 0.75 ml of chloroplatinic acid and 29.25 ml of lactic acid aqueous solution were placed in a quartz reactor and continuously stirred. At the same time, the temperature in the reactor was stabilized at 15°C. A xenon lamp was used as a light source (300 W, Perfect Light, with a 400 nm cutoff filter) to pre-illuminate the quartz reactor for 30 minutes, and precious metal Pt was deposited on the surface of the ZCS photocatalyst. After exhausting, a xenon lamp was used as a light source (300 W, Perfect Light, with a 400 nm cutoff filter) to illuminate the quartz reactor, and Ar was used as a carrier gas. The hydrogen production performance was analyzed every 1 h using a gas chromatograph (Techcomp GC7900, thermal conductivity detector).
[0075] Figure 7 The photocatalytic hydrogen evolution diagram of Experimental Example 1 and Experimental Example 2. The photocatalytic hydrogen evolution activity of 10% P-MoC / ZCS is 1.44 times that of ZCS loaded with precious metal Pt, which shows that the introduction of P-MoC greatly improves the hydrogen evolution efficiency of ZCS. The hydrogen evolution efficiency of 10% P-MoC / ZCS is also significantly improved compared with ZCS-Pt.
[0076] Experimental Example 3
[0077] The P-MoC nanoparticles prepared in Example 1 and the C prepared in Example 8 were respectively 3 N 4 , 5% P-MoC / C prepared in Example 8 3 N 4 , 10% P-MoC / C prepared in Example 9 3 N 4 , 15% P-MoC / C prepared in Example 10 3 N 4 , 20% P-MoC / C prepared in Example 11 3 N 4 15 mg of sample was dispersed in 30 ml of lactic acid aqueous solution and placed in a quartz reactor. The reaction temperature was kept constant at 15 °C. A xenon lamp was used as the light source for single-side irradiation (300 W, Perfect Light, with a 400 nm cutoff filter). Ar was used as the carrier gas, and the hydrogen production performance was analyzed every 1 h by gas chromatograph.
[0078] Figure 8 This is the photocatalytic hydrogen evolution diagram of Experimental Example 3. 10% P-MoC / C 3 N 4 The photocatalytic hydrogen evolution activity is C 3 N 4 This indicates that the introduction of P-MoC greatly improves the3 N 4 of hydrogen evolution efficiency.
[0079] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a P-MoC co-catalyst for photocatalytic hydrogen production, characterized in that: The following steps are involved: S1, mixing and stirring zinc nitrate hexahydrate, phosphomolybdic acid, polyethylpyrrolidone and methanol to obtain solution A; the molar ratio of zinc element to molybdenum element is 1:(0.9-1.2); S2, dispersing dimethylimidazole in methanol and stirring to obtain solution B; the molar ratio of the zinc element to the dimethylimidazole is 1:(10-13); S3, mixing solution A and solution B, stirring, filtering, washing, and drying to obtain a P-MoC precursor; the stirring time is 20-30 hours, and the drying condition is vacuum drying at 50-70 °C for 8-12 hours; S4, the P-MoC precursor is calcined in an inert gas atmosphere to obtain a P-MoC co-catalyst; during the calcination process, the heating rate is 3-8 °C / min, the calcination temperature is 750-850 °C, and the calcination time is 1.5-2.5 h.
2. The method for preparing the P-MoC co-catalyst for photocatalytic hydrogen production according to claim 1, characterized in that: In step S3, methanol and ethanol are used in sequence for washing.
3. A P-MoC / Zn 0.5 Cd 0.5 The method for preparing S photocatalyst is characterized in that: The following steps are involved: Zn 0.5 Cd 0.5 The S catalyst is dispersed in deionized water, and the P-MoC co-catalyst prepared in the preparation method of the P-MoC co-catalyst for photocatalytic hydrogen production according to any one of claims 1 to 2 is added, stirred, centrifuged, washed, and dried to obtain P-MoC / Zn 0.5 Cd 0.5 S; stirring time is 10-14 h, drying temperature is 60-100 ℃, and drying time is 3-5 h; The Zn 0.5 Cd 0.5 The mass ratio of the S catalyst to the P-MoC co-catalyst is 1:(0.05-0.2).
4. A P-MoC / Zn as claimed in claim 3 0.5 Cd 0.5 P-MoC / Zn S photocatalyst prepared in the preparation method 0.5 Cd 0.5 Application of S photocatalyst in photocatalytic hydrogen production.
5. A method for preparing a P-MoC / g-C3N4 photocatalyst, characterized in that: The following steps are involved: Dispersing the g-C3N4 catalyst in deionized water, adding the P-MoC co-catalyst prepared in the preparation method of the P-MoC co-catalyst for photocatalytic hydrogen production according to any one of claims 1 to 2, stirring, centrifuging, washing, and drying to obtain P-MoC / g-C3N4; the stirring time is 10-14 h, the drying temperature is 60-100 ° C, and the drying time is 3-5 h; The mass ratio of the g-C3N4 catalyst to the P-MoC co-catalyst is 1:(0.05-0.2).
6. Use of the P-MoC / g-C3N4 photocatalyst prepared by the method for preparing the P-MoC / g-C3N4 photocatalyst as claimed in claim 5 in photocatalytic hydrogen production.